Preparation method of thermoplastic biodegradable plastic
By introducing lactic acid into PBAT and adopting a melt polycondensation process, its elastic modulus and tensile strength are improved, which solves the problem of insufficient mechanical properties of PBAT and is suitable for applications such as high-strength packaging materials and disposable tableware.
Patent Information
- Application Number
- CN202411005210.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-25
AI Technical Summary
Existing PBAT has poor performance in mechanical indicators such as elastic modulus and tensile strength, making it difficult to meet certain application requirements.
By introducing lactic acid as a chain extender, a high molecular weight three-member block copolyester is synthesized using a melt polycondensation process to modify the amorphous region of PBAT and increase its elastic modulus and tensile strength.
The elastic modulus and tensile strength of PBAT are significantly improved, enabling the preparation of high-strength modulus thermoplastic biodegradable plastics, which are suitable for packaging materials, disposable tableware and other fields.
Smart Images

Figure CN118772386A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing degradable plastics, in particular to a method for preparing thermoplastic biodegradable plastics. Background Art
[0002] As a new type of functional plastic, degradable plastic products are characterized by the fact that after reaching a certain service life, their chemical structure will change significantly under specific environmental conditions, causing certain performance losses and changes in appearance, thereby achieving the purpose of being harmless or less harmful to the natural environment.
[0003] Polybutylene terephthalate adipate (PBAT) is a thermoplastic biodegradable material made from 1,4-butanediol (BDO), adipic acid (AA), terephthalic acid (PTA) or dimethyl terephthalate (DMT) through esterification and polycondensation reactions.
[0004] PBAT has good film properties, excellent flexibility and biodegradability, good thermal stability and excellent mechanical properties. PBAT can be processed in a variety of forms such as injection molding, extrusion molding, blow molding, etc., and is widely used in sheet materials, mulch films, packaging, foaming and other material fields. It is particularly suitable for packaging films, garbage bags, agricultural mulch films, dust-proof nets, etc. This material is biodegradable and can fight against white pollution. It is a green material and one of the most active and best-used degradable materials in the current research of degradable plastics.
[0005] However, compared with other general-purpose plastics, PBAT performs poorly in mechanical indicators such as elastic modulus and tensile strength. How to use chemical synthesis modification to improve the mechanical indicators of PBAT has become a technical problem that needs to be solved urgently. Summary of the invention
[0006] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a thermoplastic biodegradable plastic to solve the problem of how to improve the elastic modulus, tensile strength and other mechanical indicators of the existing PBAT.
[0007] Technical solution: The method for preparing a thermoplastic biodegradable plastic according to the present invention is characterized by comprising the following steps:
[0008] (1) subjecting adipic acid and 1,4-butanediol to an esterification and dehydration reaction to obtain a first product;
[0009] (2) reacting dimethyl terephthalate or terephthalic acid with 1,4-butanediol to obtain a second product;
[0010] (3) pre-condensing the lactic acid monomer to obtain a third product;
[0011] (4) The first product, the second product and the third product are subjected to a melt polycondensation reaction to obtain a final product.
[0012] The present invention uses lactic acid or multiple diol copolymers to modify PBAT, introduces lactic acid monomers or diols into the amorphous region of PBAT, and replaces a small amount of adipic acid-butanediol chain segments to prepare high-barrier, high-strength modulus PBAT-based copolyesters. The synthesis of copolyesters adopts a fractional esterification method, in which lactic acid is dehydrated and condensed to prepare a prepolymer, adipic acid and butanediol, terephthalic acid and butanediol are esterified to form prepolymers, and the three prepolymers are mixed, and then pre-polycondensed and melt-polycondensed to obtain a ternary block copolyester mixture with different high molecular weights.
[0013] The reaction formulas of each step are as follows:
[0014]
[0015] The side reactions in each step are as follows:
[0016]
[0017] The final product ternary block copolyester includes a polymer of the following structural formula:
[0018]
[0019] The present invention introduces lactic acid as a chain extender and adopts a melt polycondensation process to directly synthesize high molecular weight polybutylene adipate terephthalate (number average molecular weight is 30000 g / mol-70000 g / mol), and the molecular weight of the novel high-strength thermoplastic biodegradable plastic PBAT is 60000-200000.
[0020] Preferably, in step (1), the method of the esterification dehydration reaction is: adipic acid and 1,4-butanediol are mixed in a molar ratio of 1:1-1.5, a titanium-based catalyst is added, and the mixture is heated to 130-180°C to carry out an esterification dehydration reaction at normal pressure, and the end point of the esterification reaction is determined based on the amount of water produced by the esterification reaction and the acid value to obtain a first product.
[0021] Preferably, the endpoint of the esterification reaction is that the amount of water produced by the esterification reaction reaches 85% of the theoretical value and the acid value is <15 mg / g, and the titanium-based catalyst includes one or more of tetra-n-butyl titanate, tetraisopropyl titanate, titanium-phosphorus compounds, titanium-silicon compounds and titanium-magnesium composite catalysts.
[0022] Preferably, in step (2), the reaction comprises:
[0023] After dimethyl terephthalate and 1,4-butanediol are mixed at a molar ratio of 1:1-3, a titanium catalyst is added, the temperature is slowly raised to 200-260°C, and an ester exchange reaction is carried out at a pressure of 40 kPa to remove methanol. The reaction endpoint is determined according to the output of methanol to obtain a second product;
[0024] Or after mixing terephthalic acid and 1,4-butanediol in a molar ratio of 1:1-3, adding a titanium catalyst, slowly heating to 200-260°C, performing a secondary esterification reaction at a pressure of 40 kPa to remove water, judging the reaction endpoint based on the amount of water produced by the secondary esterification reaction, and obtaining a second product.
[0025] Preferably, the amount of titanium catalyst used in the transesterification reaction is 0.2‰-0.4‰ of the theoretical discharge weight, and the reaction time is 0.5-2.5h; the amount of titanium catalyst used in the secondary esterification reaction is 1‰-5‰ of the theoretical discharge weight, and the reaction time is 1.5-3.5h; the titanium catalyst includes one or more of tetra-n-butyl titanate, tetraisopropyl titanate, titanium-phosphorus compound, titanium-silicon compound and titanium-magnesium composite catalyst. The titanium-phosphorus compound is a compound with titanium as the central atom and phosphorus compound as ligand; the titanium-silicon compound is TiO2 / SiO2, wherein Ti / Si is 9:1; the titanium-magnesium composite catalyst is a complex of titanate and magnesium acetate.
[0026] Preferably, in step (3), the method for pre-condensation of lactic acid monomer is: adding a zinc catalyst to the lactic acid aqueous solution, heating to 130-170°C, stirring the reaction for 3-4 hours, judging the reaction endpoint based on the amount of water produced by the reaction, and obtaining an intermediate; condensing the intermediate under a vacuum degree of 150-200Pa for 5-15 minutes to obtain a third product.
[0027] Preferably, the zinc catalyst is one or more of zinc, diethyl zinc, zinc octoate, zinc acetate, zinc oxide and zinc chloride.
[0028] Preferably, in step (4), the melt polycondensation reaction comprises: mixing the first product, the second product, the titanium catalyst, the antioxidant and the stabilizer, stirring and reacting at 190°C for 20-30 minutes, adding the third product and mixing, heating to 200-210°C, reacting under vacuum conditions, judging the reaction progress according to the instrument current, and terminating the polycondensation reaction when a preset value is reached.
[0029] Preferably, the method of reacting under vacuum conditions is: reacting at a vacuum degree of 100-1000 Pa for 0.2-1.6 h; and then reacting at a vacuum degree below 100 Pa for 0.2-1.6 h.
[0030] Preferably, the stabilizer is an organic phosphite in an amount of 0.3‰-2‰ of the theoretical discharge weight, and the antioxidant is a hindered phenol.
[0031] In some embodiments, the organic phosphites are one or more of triphenyl phosphate, triethyl phosphite, pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, and dioctadecylpentaerythritol diphosphite; the hindered phenols are one or two of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine.
[0032] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0033] (1) The present invention directly adds lactic acid modification during the synthesis stage, introduces low-cost lactic acid monomers into the PBAT amorphous region, and replaces a small amount of BA segments to achieve the preparation of high molecular weight, high strength modulus polybutylene adipate terephthalate copolyester. The present invention can achieve controllable synthesis of copolyester molecular weight, uniform molecular weight, and uniform molecular chain structure;
[0034] (2) The added lactic acid or polyol is easy to obtain and the added amount is small, which can not only reduce the production cost of the product, but also improve the mechanical properties of the product such as elastic modulus and tensile strength;
[0035] (3) Through the control of the process and the optimization of the reaction aids, the reaction time is greatly shortened. The synthesized product has good color and excellent mechanical properties. It is completely biodegradable and can be widely used in consumer products such as packaging materials and disposable tableware. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The material balance diagram for the designed formula PBA30LA20T50;
[0037] Figure 2 The H-NMR spectra of the esterification products of terephthalic acid and 1,4-butanediol at different alcohol-acid ratios;
[0038] Figure 3 H NMR spectra of PBLA10T50-PBLA30T50;
[0039] Figure 4 This is the stress-strain curve of PBALA10T50-PBALA30T50 copolyester. DETAILED DESCRIPTION
[0040] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0041] Example 1: A method for preparing a thermoplastic biodegradable plastic is as follows: Diol terephthalate (DMT)
[0042] (1) Esterification reaction of terephthalic acid and 1,4-butanediol
[0043] First, 10.814 kg of 1,4-butanediol (BDO) was added to a 30L stainless steel esterification kettle, followed by 9.968 kg of terephthalic acid (PTA), an alcohol-acid ratio of 2:1, and 30.6 g of tetrabutyl titanate (TBT), a catalyst, and mixed into a slurry. The stirring speed was 600 rpm. The reaction was heated to 190 ° C at the beginning, and then to 220 ° C after about half an hour. The pressure was controlled at 40 kPa, and the overall reaction time was 3-4 hours. To prevent butanediol from solidifying in the condenser, the top temperature of the condenser was set to 150 ° C. The by-products were detected, separated and weighed, and 2376 g of esterified water and 864 g of tetrahydrofuran were produced. According to the experimental water output and reaction time, the end point of the esterification reaction was judged. The end point of the reaction was when the actual weighed value of the water output was close to the calculated theoretical value. The reaction end point can be judged by observing that the reaction water production rate is reduced to 1 drop / second. In order to reduce the amount of tetrahydrofuran (THF) produced in the esterification reaction of terephthalic acid and 1,4-butanediol and reduce the consumption of 1,4-butanediol, the esterification reaction of PBAT needs to be operated under negative pressure; the polycondensation reactor is operated in a vacuum state, and a cold trap device is installed in front of the screw vacuum pump for deep cooling to capture tetrahydrofuran as much as possible.
[0044] (2) Esterification reaction of adipic acid and 1,4-butanediol
[0045] Add 3.894 kg of BDO, 5.26 kg of adipic acid (AA), 1.2:1 alcohol-acid ratio, and 18.36 g of catalyst TBT to a 30L stainless steel esterification kettle and mix well to form a slurry. Stirring speed is 600 rpm. The reaction is heated to 170°C and the overall reaction time is 3-4 hours. The by-products are tested and weighed, and 2304 g of by-product esterification water is produced. The end point of the esterification reaction is determined based on the experimental water output and reaction time. The end point of the esterification reaction is when the water output of the esterification reaction reaches 85% of the theoretical value and the acid value is <15 mg / g.
[0046] (3) Lactic acid prepolymerization
[0047] Add 6.006 kg of 90% lactic acid aqueous solution and 16.4 g of zinc acetate to a 30L stainless steel esterification kettle. Heat the reaction to 150°C, and the overall reaction time is 3-4 hours. Stir at 600 rpm. Detect and weigh the by-products, and 1680 g of esterified water is produced. According to the experimental output water volume, the end point of the lactic acid esterification reaction is determined. Then carry out lactic acid pre-condensation, condense for 10 minutes under a vacuum degree of 150-200 Pa, and end the reaction.
[0048] (4) Polycondensation reaction
[0049] The products obtained in steps (1) and (2) are first introduced into a 100L stainless steel polycondensation reactor, and 44 grams of tetra(3,5-di-tert-butyl-4-hydroxyhydrocinnamic acid) pentaerythritol ester, 21 grams of tetrabutyl titanate, and 50 grams of triphenyl phosphate, a stabilizer, are added. The temperature is controlled at 190°C, the stirring speed is 600rpm, and the stirring is carried out for 20-30 minutes. Then, the lactic acid prepolymer obtained in step (3) is introduced, mixed and stirred for about 20 minutes, and the pre-polycondensation is started. The temperature is gradually raised to 200°C, and the temperature vacuum is controlled to be below 50Pa. The reaction time is about 5-6 hours. As the reaction progresses, the stirring speed gradually decreases, and the speed in the later stage is 300rpm. The reaction progress is judged according to the instrument current. According to the change of the reaction current, when the current increases significantly and lasts for a period of time, it will gradually decrease, which can be judged as the end of the polycondensation reaction. The polycondensation reaction is terminated when the preset value is reached. The polycondensation reaction is carried out under vacuum. When the molecular chain increases to the specified molecular weight range, the reaction process is completed, the vacuum is stopped, and the material in the polycondensation reactor is pressed out by nitrogen, passed through the casting head casting belt, and then cooled and pelletized.
[0050] At the same time, the by-products were filtered for solid-liquid separation. Considering that the melting point of lactide is 93-100°C, the pipeline temperature can be raised to 100°C. 4.758 kg of by-product BDO and 2.594 kg of lactide / lactic acid mixture were obtained.
[0051] Finally, about 21.428 kg of copolyester was obtained, and in a phenol / tetrachloroethane mixed solution (1:1 wt / wt) at 30° C., the intrinsic viscosity was >1.0 dL / g.
[0052] Example 2: A method for preparing a thermoplastic biodegradable plastic is as follows:
[0053] (1) Esterification reaction of terephthalic acid and 1,4-butanediol
[0054] In a 30L stainless steel esterification kettle, 11.896 kg of BDO was first added, followed by 10.965 kg of PTA, an alcohol-acid ratio of 2:1, and 33.66 g of tetrabutyl titanate (TBT), a catalyst, and mixed into a slurry. The stirring speed was 600 rpm. The reaction was heated to 200 ° C at the beginning, and then to 230 ° C after about half an hour. The pressure was controlled at 40 kPa, and the overall reaction time was 3-4 hours. To prevent butanediol from solidifying in the condenser, the top temperature of the condenser was set to 150 ° C. The by-products were detected, separated and weighed, and 2614 g of esterified water and 952 g of tetrahydrofuran were produced. The end point of the esterification reaction was determined based on the experimental water output and reaction time.
[0055] (2) Esterification reaction of adipic acid and 1,4-butanediol
[0056] Add 3.894 kg of BDO, 3.507 kg of AA, 1.2:1 alcohol-acid ratio, and 12.24 g of catalyst TBT to a 30L stainless steel esterification kettle and mix well to form a slurry. Stirring speed is 600 rpm. Heat the reaction to 180°C, and the overall reaction time is 3-4 hours. Detect and weigh the by-products, and 864 g of esterified water is produced. Determine the end point of the esterification reaction based on the experimental water output and reaction time.
[0057] (3) Lactic acid prepolymerization
[0058] Add 6.756 kg of 90% lactic acid aqueous solution and 20.5 g of zinc acetate to a 30L stainless steel esterification kettle. Heat the reaction to 150°C, and the overall reaction time is 3-4 hours. Stirring speed is 600rpm. Detect and weigh the by-products, and 2101 g of esterified water is produced. According to the experimental output water volume, the end point of the lactic acid esterification reaction is determined. Then carry out lactic acid pre-condensation, condense for 10 minutes under vacuum conditions of 150-200Pa, and end the reaction.
[0059] (4) Polycondensation reaction
[0060] The products obtained in step (1) and step (2) are first introduced into a 100L stainless steel polycondensation reactor, and 44 grams of tetra(3,5-di-tert-butyl-4-hydroxyhydrocinnamic acid) pentaerythritol ester, 25 grams of triphenyl phosphate, and 20 grams of tetrabutyl titanate are added. The temperature is controlled at 190°C, the stirring speed is 600rpm, and the stirring is carried out for 20-30 minutes. Then, the lactic acid prepolymer obtained in step (3) is introduced, mixed and stirred for about 20 minutes, and the pre-polycondensation is started. The temperature is gradually increased to 200-210°C, and the vacuum degree is below 50Pa. The reaction time is about 5-6 hours. As the reaction progresses, the stirring speed is gradually reduced, and the speed in the later stage is 300rpm. The reaction progress is judged according to the instrument current, and the polycondensation reaction is terminated when the preset value is reached.
[0061] At the same time, the by-products were filtered for solid-liquid separation. Considering that the melting point of lactide is 93-100°C, the pipeline temperature can be raised to 100°C. 4.953 kg of by-product BDO and 3.244 kg of lactide / lactic acid mixture were obtained.
[0062] Finally, about 21.5 kg of copolyester was obtained, and in a phenol / tetrachloroethane mixed solution (1:1 wt / wt) at 30° C., the intrinsic viscosity was >1.0 dL / g.
[0063] Embodiment 3: The rest is the same as Embodiment 1, except that:
[0064] Terephthalic acid is replaced by dimethyl terephthalate, and the molar ratio of dimethyl terephthalate to 1,4-butanediol is 1:3. The molar ratio of adipic acid to 1,4-butanediol is 1:1. The catalyst TBT in steps (1) and (2) is replaced by a titanium phosphorus compound, and the amount used is 0.2‰ of the theoretical discharge weight.
[0065] In step (3), the method for pre-condensation of lactic acid monomer is: adding diethyl zinc to the lactic acid aqueous solution, heating to 130° C., stirring the reaction for 3-4 hours, judging the reaction end point based on the amount of water produced by the reaction, and obtaining an intermediate; condensing the intermediate under a vacuum condition of 150 Pa for 10 minutes to terminate the reaction.
[0066] In step (4), the temperature is gradually raised to 225° C., and the reaction is carried out at a vacuum degree of 1000 Pa for 0.2 h; then, the reaction is carried out at a vacuum degree below 100 Pa for 1.6 h.
[0067] Pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyhydrocinnamate) was replaced by N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, and triphenyl phosphate was replaced by triethyl phosphite.
[0068] Embodiment 4: The rest is the same as Embodiment 1, except that:
[0069] Terephthalic acid is replaced by dimethyl terephthalate, and the molar ratio of dimethyl terephthalate to 1,4-butanediol is 1:1. The molar ratio of adipic acid to 1,4-butanediol is 1:1.5. The catalyst TBT in steps (1) and (2) is replaced by a titanium silicon compound, and the amount used is 0.4‰ of the theoretical discharge weight.
[0070] In step (3), the method for pre-condensation of lactic acid monomer is: adding zinc octanoate to the lactic acid aqueous solution, heating to 170° C., stirring the reaction for 3-4 hours, judging the reaction endpoint based on the amount of water produced by the reaction, and obtaining an intermediate; condensing the intermediate under a vacuum condition of 200 Pa for 15 minutes to terminate the reaction.
[0071] In step (4), the temperature is gradually raised to 225° C., and the reaction is carried out for 1.6 h at a vacuum degree of 500 Pa, and then for 0.2 h at a vacuum degree below 100 Pa. Triphenyl phosphate is replaced by pentaerythritol diphosphite.
[0072] Embodiment 5: The rest is the same as Embodiment 1, except that:
[0073] Terephthalic acid is replaced by dimethyl terephthalate, and the molar ratio of dimethyl terephthalate to 1,4-butanediol is 1:3. The catalyst TBT in steps (1) and (2) is replaced by a titanium-magnesium composite catalyst, and the amount used is 0.5‰ of the theoretical discharge weight.
[0074] In step (3), the method for pre-condensation of lactic acid monomer is: adding zinc chloride to the lactic acid aqueous solution, heating to 160° C., stirring the reaction for 3-4 hours, judging the reaction endpoint based on the amount of water produced by the reaction, and obtaining an intermediate; condensing the intermediate under a vacuum condition of 200 Pa for 5 minutes to terminate the reaction.
[0075] In step (4), the temperature is gradually raised to 225° C., and the reaction is carried out for 3 hours under a vacuum degree of 100 Pa. Triphenyl phosphate is replaced by bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite.
[0076] The product performance indicators obtained from different embodiments are as follows:
[0077] Elastic modulus (MPa) Tensile strength(MPa) Elongation at break (%) PBAT 85±1 17.6±0.2 743±5 Example 1 152±5 47±5 750±30 Example 2 124±2 32±3 753±105 Example 3 141±4 45±2 784±57 Example 4 139±6 39±4 739±79 Example 5 148±3 51±3 793±41
[0078] Compared with common PBAT, the elastic modulus of the thermoplastic biodegradable plastic prepared by the present invention is increased by 30-50%, the tensile strength is increased to above 25 MPa, and the elongation at break is maintained at 650-850%.
[0079] Embodiment 6: The rest is the same as Embodiment 1, except that:
[0080] Different copolyester final products were prepared by taking the ratio of lactic acid segments and terephthalic acid segments as variables. The ratio was precisely controlled by adjusting the raw material ratio.
[0081] The nuclear magnetic hydrogen spectra and stress-strain curves of different final products were measured respectively. The results are as follows Figure 3 and Figure 4 shown. Figure 3 PBLA10T50 represents the composition of the copolyester, in which the lactic acid (LA) segment accounts for 10% and the terephthalic acid (T) segment accounts for 50%, and the same applies to other figures. Figure 4 In the figure, PBALA10T50 represents the component composition of the copolyester, with the lactic acid (LA) segment accounting for 10% and the terephthalic acid (T) segment accounting for 50%, and the other legends are similar.
[0082] Embodiment 7: The rest is the same as Embodiment 1, except that:
[0083] In step (1), different esterification products were prepared with the molar ratio of 1,4-butanediol to terephthalic acid as a variable, and the nuclear magnetic resonance hydrogen spectrum was measured. The results are as follows: Figure 3 As shown, Figure 3The alcohol-acid input ratio refers to the molar ratio of 1,4-butanediol and terephthalic acid weighed by theoretical calculation when the raw materials are added. The actual alcohol-acid ratio is the actual ratio of 1,4-butanediol and terephthalic acid in the product detected by nuclear magnetic hydrogen spectrum after the polycondensation reaction is completed. It is judged based on the characteristic peak position of H in the nuclear magnetic hydrogen spectrum. The addition of BDO is to add the polycondensation catalyst and a part of BDO to the polycondensation kettle through the auxiliary agent feeding tank after the esterification reaction is completed and before the polycondensation reaction begins. In order to ensure the vacuum degree of the polycondensation kettle, the feeding pipeline should be operated in a closed manner with double valve control.
Claims
1. A method for preparing a thermoplastic biodegradable plastic, It is characterized in that The steps include: (1) subjecting adipic acid and 1,4-butanediol to an esterification and dehydration reaction to obtain a first product; (2) reacting dimethyl terephthalate or terephthalic acid with 1,4-butanediol to obtain a second product; (3) pre-condensing the lactic acid monomer to obtain a third product; (4) The first product, the second product and the third product are subjected to a melt polycondensation reaction to obtain a final product.
2. The method for preparing the thermoplastic biodegradable plastic according to claim 1, It is characterized in that In step (1), the method for the esterification dehydration reaction is: adipic acid and 1,4-butanediol are mixed in a molar ratio of 1:1-1.5, a titanium catalyst is added, and the mixture is heated to 130-180°C to carry out an esterification dehydration reaction at normal pressure. The end point of the esterification reaction is determined based on the amount of water produced by the esterification reaction and the acid value to obtain a first product.
3. The method for preparing the thermoplastic biodegradable plastic according to claim 2, It is characterized in that The endpoint of the esterification reaction is that the water output of the esterification reaction reaches 85% of the theoretical value and the acid value is <15 mg / g. The titanium-based catalyst includes one or more of tetra-n-butyl titanate, tetraisopropyl titanate, titanium-phosphorus compounds, titanium-silicon compounds and titanium-magnesium composite catalysts.
4. The method for preparing the thermoplastic biodegradable plastic according to claim 1, It is characterized in that In step (2), the reaction comprises: After dimethyl terephthalate and 1,4-butanediol are mixed at a molar ratio of 1:1-3, a titanium catalyst is added, the temperature is slowly raised to 200-260°C, and an ester exchange reaction is carried out at a pressure of 40 kPa to remove methanol. The reaction endpoint is determined according to the output of methanol to obtain a second product; Or after mixing terephthalic acid and 1,4-butanediol in a molar ratio of 1:1-3, adding a titanium catalyst, slowly heating to 200-260°C, performing a secondary esterification reaction at a pressure of 40 kPa to remove water, judging the reaction endpoint based on the amount of water produced by the secondary esterification reaction, and obtaining a second product.
5. The method for preparing the thermoplastic biodegradable plastic according to claim 4, It is characterized in that The amount of titanium catalyst used in the ester exchange reaction is 0.2‰-0.4‰ of the theoretical output weight, and the reaction time is 0.5-2.5h; the amount of titanium catalyst used in the secondary esterification reaction is 1‰-5‰ of the theoretical output weight, and the reaction time is 1.5-3.5h; the titanium catalyst includes one or more of tetra-n-butyl titanate, tetraisopropyl titanate, titanium-phosphorus compounds, titanium-silicon compounds and titanium-magnesium composite catalysts.
6. The method for preparing the thermoplastic biodegradable plastic according to claim 1, It is characterized in that In step (3), the method for pre-condensation of lactic acid monomer is: adding a zinc catalyst to the lactic acid aqueous solution, heating to 130-170°C, stirring the reaction for 3-4 hours, judging the reaction endpoint based on the amount of water produced by the reaction, and obtaining an intermediate; condensing the intermediate under vacuum conditions of 150-200Pa for 5-15 minutes to obtain a third product.
7. The method for preparing the thermoplastic biodegradable plastic according to claim 6, It is characterized in that The zinc catalyst is one or more of zinc, diethyl zinc, zinc octoate, zinc acetate, zinc oxide and zinc chloride.
8. The method for preparing the thermoplastic biodegradable plastic according to claim 1, It is characterized in that In step (4), the melt polycondensation reaction includes: mixing the first product, the second product, the titanium catalyst, the antioxidant, and the stabilizer, stirring and reacting at 190°C for 20-30 minutes, adding the third product and mixing, heating to 200-210°C, reacting under vacuum conditions, judging the reaction progress based on the instrument current, and terminating the polycondensation reaction when a preset value is reached.
9. The method for preparing the thermoplastic biodegradable plastic according to claim 8, It is characterized in that The method of reacting under vacuum conditions is: reacting at a vacuum degree of 100-1000 Pa for 0.2-1.6 h; and then reacting at a vacuum degree below 100 Pa for 0.2-1.6 h.
10. The method for preparing the thermoplastic biodegradable plastic according to claim 8, It is characterized in that The stabilizer is 0.3‰-2‰ of the theoretical discharge weight of organic phosphites, and the antioxidant is hindered phenols.
Citation Information
Patent Citations
Method for continuously preparing biodegradable aliphatic / aromatic polyester copolymer
CN104583271A
Preparation methods for poly(polybutylene glycol-adipate-terephthalate) and polylactic-acid block copolymer of poly(polybutylene glycol-adipate-terephthalate)
CN105524262A
Copolymerization method of PBAT-PLA copolyester
CN107141458A
Cited By
Light-aging-resistant PBAT functional resin as well as preparation method and application thereof