Polyester resin for powder coating and preparation method thereof

By designing high-functionality polyester resin segments and curing them with low-functionality diglycidyl terephthalate, the problems of insufficient storage stability, gloss uniformity and impact resistance of powder coatings are solved, and high performance is achieved. The preparation of powder coatings has good market application prospects.

CN118772391APending Publication Date: 2024-10-15HUANGSHAN YUANRUN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411109181.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

HAA and TGIC curing agents in existing powder coatings have poor resistance to thick coating pinholes, high temperature yellowing, and TGIC sensitization. PT910 composite curing agent has low melting range, uneven mixing, poor storage stability, and gloss uniformity. And due to the problem of insufficient impact resistance, it is difficult to find a matching high-functionality polyester resin for the low-functionality diglycidyl terephthalate curing agent.

Method used

Using 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolinone, dimethylmalonic acid, 3-dimethylamino-1,2-propanediol, terephthalic acid, Ethylene glycol, 1,4-succinic acid, nitrogen triacetic acid and other raw materials Polymerize the materials, design high-functionality polyester resin chain segments, increase the number of ester groups and inactive nitrogen atoms, improve the adhesion to the substrate and the functionality of the polyester resin, and combine it with low-functionality diterephthalate Glycidyl ester is cured.

Benefits of technology

The prepared powder coating has good storage stability, the gloss of the coating film reaches more than 93%, excellent hardness and adhesion, and good boiling resistance. It solves the problem of insufficient compatibility with the low-functionality diglycidyl terephthalate curing agent. Improves the overall performance of powder coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991671600000021
    Figure BDA0004991671600000021
  • Figure BDA0004991671600000041
    Figure BDA0004991671600000041
  • Figure BDA0004991671600000052
    Figure BDA0004991671600000052
Patent Text Reader

Abstract

The invention relates to polyester resin for a powder coating, which is obtained by taking 4, 5-dihydroxy-1, 3-bis (hydroxymethyl)-2-imidazolinone, dimethyl malonic acid, 3-dimethylamino-1, 2-propylene glycol, terephthalic acid, ethylene glycol, 1, 4-succinic acid, nitrilotriacetic acid and the like as main raw materials and polymerizing. When the powder coating is applied to a terephthalic acid diglycidyl ester curing system, the prepared powder coating is good in storage stability, the coating film gloss reaches 93% or above, the hardness and the adhesive force are excellent, the coating film surface does not have obvious change after the powder coating is boiled in boiling water for 5 h, and the coating film has good adhesion. Therefore, the problem that the low-functionality terephthalic acid diglycidyl ester curing agent is difficult to find the matched polyester resin is well solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder coatings, and specifically relates to a polyester resin for powder coatings and a preparation method thereof, as well as application of the polyester resin in a diglycidyl terephthalate curing system. Background Art

[0002] Compared with solvent-based coatings, powder coatings have the advantages of no solvent volatilization, 100% film formation, and easy use. They have been used more and more widely in recent years. Outdoor weather-resistant powder coatings are mainly HAA system powder coatings and TGIC system powder coatings. The full name of HAA is N, N, N', N'-tetrakis (2-hydroxyethyl) adipamide. Its main defects are poor resistance to thick coating pinholes and high-temperature yellowing. The full name of TGIC is triglycidyl isocyanurate. It mainly uses epoxy groups for curing. The overall performance is relatively balanced, but it is banned by the EU due to its allergenicity. In order to overcome the defects of TGIC and HAA curing agents, foreign countries have developed PT910 composite curing agent products. This product is a compound of triglycidyl trimellitate and diglycidyl terephthalate in a mass ratio of 1:3. It also uses epoxy groups for curing, overcoming the sensitization of TGIC and the thick coating pinholes and high-temperature yellowing phenomena of HAA. However, since the composite component of PT910, triglycidyl trimellitate, is liquid at room temperature, the addition of triglycidyl trimellitate is mainly to improve the functionality of the composite curing agent. Its addition causes the following problems in PT910 curing agent: Defects: (1) Not only is the melting range low, but it is also easy to mix unevenly with diglycidyl terephthalate, resulting in high manufacturing costs, and the powder coating prepared therefrom has poor storage stability; (2) Due to the uneven dispersion of the two components of the composite curing agent PT190 and the difference in the curing activity of the functional groups of the two components, the coating curing uniformity is poor, resulting in relatively low gloss on the board surface, and defects in the uniformity of the gloss and impact resistance of the board surface are prone to occur. For example, the hardness and gloss of the coating at different positions on the same sample are significantly different. Generally, it is necessary to extend the grinding time to increase its uniformity, resulting in high energy consumption. Diglycidyl terephthalate itself is a solid powder with a melting range of about 100°C. If used alone as a curing agent, it can not only overcome the defects of TGIC curing agent and HAA curing agent, but also, as a single solid component, it will not have the defects of PT910 curing agent such as uneven mixing, easy escape of liquid leading to storage stability of powder coatings, low gloss and poor uniformity. However, since the functionality of diglycidyl terephthalate is 2, the functionality is relatively low, and the functionality of ordinary functional polyester resins currently on the market is 2-2.5, which is matched with trifunctional curing agents. If it is directly cured with diglycidyl terephthalate with a functionality of 2, the coating film strength is insufficient. Not only is the coating film low in hardness, but the adhesion is also poor, and the boiling resistance and impact performance are difficult to meet the requirements. How to develop a high-functionality polyester resin that matches it is the key to whether the diglycidyl terephthalate curing agent can be successfully promoted in the market. Summary of the invention

[0003] In view of the above problems, the present invention starts from the polyester segment structure, functionality and process control, and develops a polyester resin with excellent adhesion and hardness suitable for the diglycidyl terephthalate curing system. The polyester resin is mainly obtained by polymerization using 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone, dimethylmalonic acid, 3-dimethylamino-1,2-propylene glycol, terephthalic acid, ethylene glycol, 1,4-succinic acid, nitrilotriacetic acid and the like as raw materials. Short-chain diols and dibasic acids are used in the designed chain segments to increase the number of ester groups to improve adhesion to the substrate. At the same time, special monomers introduced into the chain segments, such as 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone and inactive nitrogen atoms in nitrilotriacetic acid, can also enhance adhesion to the metal substrate. 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone is used as a tetrafunctional starting material, and is matched with other suitable dibasic acids and diols. The resulting polyester resin has high functionality and strong chain segment rigidity. It is finally cured with a low-functionality diglycidyl terephthalate curing agent. The prepared powder coating not only has good storage stability, but also has excellent hardness and adhesion. Therefore, the product better solves the problem that it is difficult to find a matching polyester resin for a low-functionality diglycidyl terephthalate curing agent.

[0004] The present invention relates to a polyester resin for powder coating, which comprises raw materials composed of the following molar parts:

[0005]

[0006] The raw materials also include catalyst and antioxidant; the amount of catalyst is 0.05-0.07% of the total molar amount of the raw materials; the amount of antioxidant is 0.02-0.04% of the total molar amount of the raw materials.

[0007] Furthermore, the catalyst is tetrabutyl titanate; and the antioxidant is antioxidant 1010.

[0008] The method for preparing the polyester resin for powder coating as described above comprises the following steps:

[0009] A. Add the formulated amount of 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone and the catalyst into the reaction kettle, heat it to 120-125°C, stir and mix thoroughly, add the formulated amount of dimethylmalonic acid, and heat it to 150-160°C to carry out heat preservation esterification grafting reaction;

[0010] B. Take samples to test the hydroxyl value of the esterified product. When the hydroxyl value of the esterified product is lower than 10 mgKOH / g, it means that all the hydroxyl groups on 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone have been esterified and grafted. At this time, add the formulated amount of ethylene glycol and terephthalic acid, gradually raise the temperature to 190-195°C, and then carry out heat preservation polymerization reaction;

[0011] C. Take samples to test the acid value of the polymer. When the acid value reaches 90-98 mgKOH / g, add the formulated amount of 3-dimethylamino-1,2-propylene glycol and 1,4-butanedioic acid, and gradually raise the temperature to 215-220°C to carry out heat preservation polymerization reaction;

[0012] D. When the acid value of the polymer reaches 35-43 mgKOH / g, add the formulated amount of antioxidant, then start the vacuum system, and raise the temperature to 220-225°C for vacuum polycondensation reaction;

[0013] E. When the acid value of the polymer is reduced to 12-18 mgKOH / g, stop the vacuum system, add the formulated amount of nitrilotriacetic acid, and raise the temperature to 225-230°C to carry out carboxyl end-capping reaction on the polyester resin. When the acid value of the polyester resin is 24-30 mgKOH / g, stop the reaction, discharge the material while hot, cool the polyester resin, and then crush and granulate it to obtain the polyester resin.

[0014] The obtained product has the appearance of colorless and transparent particles, an acid value of 24-30 mgKOH / g, and a softening point of 114-122°C.

[0015] Preferably, in step B, the temperature is gradually increased to 190-195°C at a heating rate of 12-15°C / h; preferably, in step C, the temperature is gradually increased to 215-220°C at a heating rate of 8-10°C / h; preferably, in step D, the vacuum degree is maintained at -0.096Mpa to -0.098Mpa; preferably, in step E, the polyester resin is cooled with a steel belt with condensed water.

[0016] The present invention also relates to the use of the polyester resin for powder coating as described above or the polyester resin for powder coating prepared by the preparation method in a diglycidyl terephthalate curing system.

[0017] The powder coating formula with diglycidyl terephthalate as a curing agent may include titanium dioxide, barium sulfate, leveling agent, brightener, benzoin, etc. in addition to the polyester resin and diglycidyl terephthalate prepared above. The coating preparation method is as follows: the materials are mixed according to the powder coating formula, extruded, tableted, and crushed by a twin-screw extruder, and then the tablets are crushed and sieved to form a powder coating. The powder coating is sprayed on the tinplate substrate after surface treatment by an electrostatic spray gun, and the coating is obtained after curing.

[0018] Beneficial effects:

[0019] The polyester resin for powder coating of the present invention is obtained by polymerization using 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone, dimethylmalonic acid, 3-dimethylamino-1,2-propylene glycol, terephthalic acid, ethylene glycol, 1,4-succinic acid, nitrilotriacetic acid and the like as main raw materials. According to the design of the present invention, short-chain diols and dibasic acids are used in the chain segments to increase the number of ester groups, thereby improving the adhesion to the substrate; at the same time, special monomers introduced in the chain segments, such as 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone, 3-dimethylamino-1,2-propylene glycol and inactive nitrogen atoms in nitrilotriacetic acid, can also enhance the adhesion to the metal substrate, and 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone is used as a tetrafunctional starting material, and is matched with other suitable dibasic acids and diols. The polyester resin finally obtained has high functionality and strong chain segment rigidity, and is finally cured with a low-functionality diglycidyl terephthalate curing agent. The prepared powder coating not only has good storage stability, but also has a coating gloss of more than 93%, and has excellent hardness and adhesion. There is no obvious change on the coating surface after boiling in boiling water for 5 hours. It can be seen that the use of the polyester resin for powder coatings of the present invention in the diglycidyl terephthalate curing system can better solve the problem that it is difficult to find a matching polyester resin for the low-functionality diglycidyl terephthalate curing agent.

[0020] The present invention has been described in detail above, but the above embodiments are only illustrative in nature and are not intended to limit the present invention. In addition, this article is not limited by any theory described in the above prior art or invention content or the following examples. DETAILED DESCRIPTION

[0021] The present invention is further described below in conjunction with examples. It should be noted that the following examples are provided for illustrative purposes only and do not constitute a limitation on the scope of protection claimed for the present invention.

[0022] Unless otherwise specified, the raw materials, reagents, methods, etc. used in the examples are conventional raw materials, reagents, methods in the art.

[0023] Preparation Example 1

[0024] A polyester resin for powder coating, comprising the following raw materials in molar proportions:

[0025]

[0026]

[0027] The catalyst is tetrabutyl titanate, and the amount used is 0.05% of the total molar amount of the raw materials;

[0028] The antioxidant is antioxidant 1010, and the amount used is 0.02% of the total molar amount of the raw materials.

[0029] The method for preparing the polyester resin for powder coating as described above comprises the following steps:

[0030] A. Add the formulated amount of 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone and the catalyst into the reaction kettle, heat it to 125°C, stir and mix thoroughly, add the formulated amount of dimethylmalonic acid, and heat it to 150°C to carry out the esterification grafting reaction;

[0031] B. Take samples to test the hydroxyl value of the esterified product. When the hydroxyl value of the esterified product is lower than 10 mgKOH / g, it means that all the hydroxyl groups on 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone have been esterified and grafted. At this time, add the formulated amount of ethylene glycol and terephthalic acid, and gradually heat the reaction to 195°C at a heating rate of 12°C / h, and then carry out heat preservation polymerization reaction;

[0032] C. Take samples to test the acid value of the polymer. When the acid value reaches 90-98 mgKOH / g, add the formulated amount of 3-dimethylamino-1,2-propylene glycol and 1,4-butanedioic acid, and gradually increase the temperature to 215°C at a rate of 10°C / h to carry out heat preservation polymerization reaction;

[0033] D. When the acid value of the polymer reaches 35-43 mgKOH / g, add the formulated amount of antioxidant, then start the vacuum system, keep the vacuum degree at -0.098Mpa, and raise the temperature to 220°C for vacuum polycondensation reaction;

[0034] E. When the acid value of the polymer is reduced to 12-18 mgKOH / g, stop the vacuum system, add the formulated amount of nitrilotriacetic acid, and heat to 230°C to carry out carboxyl end-capping reaction on the polyester resin. When the acid value of the polyester resin reaches the expected value, stop the reaction, discharge the material while hot, cool the polyester resin with a steel belt with condensed water, and then crush and granulate it to obtain the polyester resin.

[0035] The acid value of the prepared polyester resin is 29 mgKOH / g and the softening point is 116°C.

[0036] Preparation Example 2

[0037] A polyester resin for powder coating, comprising the following raw materials in molar proportions:

[0038]

[0039]

[0040] The catalyst is tetrabutyl titanate, and the amount used is 0.07% of the total molar amount of the raw materials;

[0041] The antioxidant is antioxidant 1010, and the amount used is 0.04% of the total molar amount of the raw materials.

[0042] The preparation method is the same as Example 1.

[0043] The obtained product is light yellow transparent particles with an acid value of 27 mgKOH / g and a softening point of 119°C.

[0044] Preparation Example 3

[0045] A polyester resin for powder coating, comprising the following raw materials in molar proportions:

[0046] The catalyst is tetrabutyl titanate, and the amount used is 0.06% of the total molar amount of the raw materials;

[0047] The antioxidant is antioxidant 1010, and the dosage is 0.03% of the total molar amount of the raw materials.

[0048] The preparation method is the same as Example 1.

[0049] The obtained product is light yellow transparent particles with an acid value of 30 mgKOH / g and a softening point of 115°C.

[0050] Preparation Example 4

[0051] A polyester resin for powder coating, comprising the following raw materials in molar proportions:

[0052]

[0053]

[0054] The catalyst is tetrabutyl titanate, and the amount used is 0.07% of the total molar amount of the raw materials;

[0055] The antioxidant is antioxidant 1010, and the amount used is 0.04% of the total molar amount of the raw materials.

[0056] The preparation method is the same as Example 1.

[0057] The obtained product is light yellow transparent particles with an acid value of 25 mgKOH / g and a softening point of 121°C.

[0058] Comparative Preparation Example 1

[0059] The commercially available TGIC curing system general-purpose polyester resin has an acid value of 33 mgKOH / g and a softening point of 108°C. Model SJ4214 comes from Anhui Shenjian New Materials Co., Ltd.

[0060] Comparative Preparation Example 2

[0061] A commercially available finished product PT910 curing agent powder coating was used as a comparison, purchased from Anhui Xinyou Polymer New Material Technology Co., Ltd.

[0062] Examples 1-4 and Comparative Examples 1 and 2 (polyester resins are obtained by the above corresponding examples or comparative examples)

[0063] According to the powder coating formula using diglycidyl terephthalate as the curing agent, the formula in parts by weight is as follows:

[0064]

[0065] Preparation of coating: Mix all materials according to the above powder coating formula, extrude, tablet and crush with a twin-screw extruder, and then crush and sieve the tablets to make powder coating. The powder coating is sprayed on the surface treated tinplate substrate with an electrostatic spray gun, and cured at 200℃ / 10min to obtain the coating.

[0066] Performance comparison

[0067] Coating index testing is based on GB / T 21776-2008 "Standard Guide for Testing of Powder Coatings and Their Coatings". Pencil hardness testing is based on GB / T 6739-2006 "Determination of Film Hardness by Pencil Method for Paints and Varnishes". The pencil hardness parameters are 2B-B-HB-FH-2H-3H-4H, and the hardness level increases from left to right. Adhesion test: Based on GB / T9286-1998 "Scratching Test for Paint and Varnish Films", where the smaller the number, the better the adhesion.

[0068] The polyester resin prepared in the above examples and comparative examples was used to prepare coatings according to the coating formula provided by the present invention. The coating performance results are shown in Table 1 below, and the storage stability of the powder coating is shown in Table 2.

[0069] Table 1 Coating properties of powder coatings

[0070]

[0071] Table 2 Storage stability of powder coatings

[0072]

[0073] As can be seen from Table 1 above, after the powder coatings prepared from the polyester resin product of the present invention and the difunctional diglycidyl terephthalate curing agent are fully cured at 200°C / 10min, the coatings have a smooth surface and a gloss of 93.7% or more. The hardness of the coatings is 2H, and the adhesion is also relatively good, both at level 0. There is no obvious change on the surface after boiling in boiling water for 5h, and the comprehensive application performance is excellent. Comparative Example 1 uses a commercially available general-purpose polyester resin of the TGIC curing system. Since the TGIC curing agent is trifunctional, the powder coating prepared by the polyester resin and the diglycidyl terephthalate curing agent is not compatible with the diglycidyl terephthalate curing agent due to the insufficient functionality and structural design of the polyester resin, resulting in not only poor appearance, gloss and impact resistance, but also poor hardness, adhesion and water boiling resistance. Comparative Example 2 uses the finished PT910 powder coating, which has better coating appearance and impact resistance, but a slightly lower coating gloss, less than 93%, and average gloss uniformity, and basically meets the requirements for hardness, adhesion and water boiling resistance. As can be seen from Table 2, the powder coating prepared by the polyester resin of the present invention and diglycidyl terephthalate has excellent storage stability at 45°C for up to 180 days, good dispersibility, and no agglomeration phenomenon, which is related to the structural design of the polyester resin of the present invention and the high melting point of diglycidyl terephthalate itself, while the powder coating prepared by using the commercially available TGIC curing system universal polyester resin and diglycidyl terephthalate in Comparative Example 1 showed slight agglomeration phenomenon in 180 days, and the PT910 finished powder coating of Comparative Example 2 had general dispersibility at 45°C / 90 days, slight agglomeration appeared at 150 days, and obvious agglomeration appeared after 180 days, making the powder coating difficult to use. Therefore, the powder coating prepared by matching the polyester resin product of the present invention with the diglycidyl terephthalate curing agent has overcome the defects of conventional PT910 powder coating such as storage stability, gloss and complicated preparation, and has better hardness and adhesion, and has good market application prospects.

[0074] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents, without departing from the spirit and essence of the claims of the present invention; and these modifications or replacements are still within the scope defined by the claims of the present invention.

Claims

1. A polyester resin for powder coating, characterized in that: The raw materials comprising the following molar compositions: The raw materials also include catalyst and antioxidant; the amount of catalyst is 0.05-0.07% of the total molar amount of the raw materials; the amount of antioxidant is 0.02-0.04% of the total molar amount of the raw materials.

2. A polyester resin for powder coating as claimed in claim 1, further characterized in that the catalyst is tetrabutyl titanate.

3. The polyester resin for powder coating according to claim 1, further characterized in that the antioxidant is antioxidant 1010.

4. A method for preparing a polyester resin for powder coating according to any one of claims 1 to 3, characterized in that: The following steps are involved: A. Add the formulated amount of 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone and the catalyst into the reaction kettle, heat it to 120-125°C, stir and mix thoroughly, add the formulated amount of dimethylmalonic acid, and heat it to 150-160°C to carry out heat preservation esterification grafting reaction; B. Take samples to test the hydroxyl value of the esterified product. When the hydroxyl value of the esterified product is lower than 10 mgKOH / g, it means that all the hydroxyl groups on 4,5-dihydroxy-1,3-bis(hydroxymethyl)-2-imidazolidinone have been esterified and grafted. At this time, add the formulated amount of ethylene glycol and terephthalic acid, gradually raise the temperature to 190-195°C, and then carry out heat preservation polymerization reaction; C. Take samples to test the acid value of the polymer. When the acid value reaches 90-98 mgKOH / g, add the formulated amount of 3-dimethylamino-1,2-propylene glycol and 1,4-butanedioic acid, and gradually raise the temperature to 215-220°C to carry out heat preservation polymerization reaction; D. When the acid value of the polymer reaches 35-43 mgKOH / g, add the formulated amount of antioxidant, then start the vacuum system, and raise the temperature to 220-225°C for vacuum polycondensation reaction; E. When the acid value of the polymer is reduced to 12-18 mgKOH / g, stop the vacuum system, add the formulated amount of nitrilotriacetic acid, and raise the temperature to 225-230°C to carry out carboxyl end-capping reaction on the polyester resin. When the acid value of the polyester resin is 24-30 mgKOH / g, stop the reaction, discharge the material while hot, cool the polyester resin, and then crush and granulate it to obtain the polyester resin.

5. The method for preparing a polyester resin for powder coatings according to claim 4, further characterized in that in step B, the temperature is gradually increased to 190-195°C at a heating rate of 12-15°C / h.

6. The method for preparing a polyester resin for powder coatings according to claim 4, further characterized in that in step C, the temperature is gradually increased to 215-220°C at a heating rate of 8-10°C / h.

7. The method for preparing a polyester resin for powder coating according to claim 4, further characterized in that in step D, the vacuum degree is maintained at -0.096 MPa to -0.098 MPa.

8. The method for preparing a polyester resin for powder coating according to claim 4, further characterized in that in step E, the polyester resin is cooled by a steel belt with condensed water.

9. Use of the polyester resin for powder coatings according to any one of claims 1 to 3 or the polyester resin for powder coatings prepared by the preparation method according to any one of claims 4 to 8 in a diglycidyl terephthalate curing system.