Synthesis method of poly L-alanine with high polymerization degree
By introducing fluorinated alcohol solvents into the synthesis of polyamic acid, the problems of low polymerization degree of polyalanine and the use of explosive solvents were solved, and the synthesis of poly-L-alanine with high polymerization degree was achieved, and the intrinsic viscosity was improved. and avoid security risks.
Patent Information
- Application Number
- CN202310366438.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-15
AI Technical Summary
The degree of polymerization in existing polyalanine synthesis methods is not high, and the use of explosive solvent nitrobenzene poses safety risks.
A fluorinated alcohol solvent is introduced into the amino acid-N-carboxylic anhydride reaction system, and a fluorinated alcohol compound and an initiator are used to perform a ring-opening polymerization reaction to generate poly-L-alanine with a high degree of polymerization.
The molecular weight and intrinsic viscosity of the polymer are increased to 1.58dL/g, and the use of explosive solvents is avoided, making the process safer and more reliable.
Smart Images

Figure BDA0004166892460000011
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymers, and in particular to a method for synthesizing poly-L-alanine with a high degree of polymerization. Background Art
[0002] Polyamino acids are an important type of functional polymers with the advantages of low toxicity, good biocompatibility, biodegradability, easy absorption and metabolism by the body, etc. They have been widely used in the fields of food, medicine, agriculture and industry. In the medical field, they can be used for medical sutures, drug controlled release, artificial skin, etc. In agricultural production, they can be used as fertilizers and pesticide additives, etc. In industry, they can be used to make synthetic fibers, leather, food packaging films, bags, furniture, leather clothes and shoes, etc. In today's world where we pay attention to environmental protection and emphasize sustainable development, the production and application of this biodegradable functional polymer material will gain greater development.
[0003] As a biopolymer, the molecular weight of polyamino acids is directly related to their uses. In the synthesis method of polyamino acids, amino acids react with phosgene to generate amino acid N-carboxylic anhydride (NCAn), which is then ring-opened and polymerized. The main chain of the product is similar to the structure of polyamide:
[0004]
[0005] The relative molecular weight of the polyamino acid obtained by the ring-opening polymerization of NCAn is easier to control and has a larger relative molecular weight, which can produce a polymer with spinnability and film-forming properties. After Robert Neal Macdonald et al. synthesized a polymer with a high relative molecular weight using α-amino acid-NCAn in 1951, this method has been widely used in the synthesis of polyamino acids.
[0006] The most reported polyamino acids are polyglutamic acid, polyaspartic acid and polyleucine, while there are few reports on polyalanine, the main polyamino acid in silk protein. In recent years, the application research of silk protein as a natural biomedical polymer material has attracted extensive attention. Silk protein is actually a segment copolymer composed of different amino acid units (mainly alanine and glycine units). People use chemical synthesis to introduce β-pleated sheets, polyalanine segments or helical structures into the main chain or side chain of the molecule, and finally synthesize main chain biomimetic segment copolymers or side chain biomimetic polymers, thereby enriching the research content of natural spider silk biomimetic materials. However, the molecular weight of the obtained biomimetic segment copolymer is much lower than that of natural spider silk protein, resulting in a large difference in the performance of the final synthesized biomimetic material and natural spider silk. Wang Tingwei et al. reported that L-alanine-N-carboxyl-cyclic anhydride (L-Ala-NCAn) was synthesized by slowly passing an excess of dry phosgene into a tetrahydrofuran suspension of alanine at 0°C and then heating the mixture to 30°C. L-alanine polymer was prepared using nitrobenzene as solvent and triethylamine as initiator. The degree of polymerization of the obtained product was not high, and the intrinsic viscosity was only [η] = 0.83 dL / g.
[0007] It can be seen that the polymerization degree of the polyalanine product in the prior art is not high, and the method uses nitrobenzene, an explosive solvent, which poses certain risks. Summary of the invention
[0008] One of the purposes of the present invention is to provide a method for synthesizing poly-L-alanine with a high degree of polymerization, by introducing a fluorinated alcohol solvent into the NCA reaction system to obtain poly-L-alanine with a high degree of polymerization.
[0009] The method for synthesizing poly-L-alanine provided by the present invention comprises the following steps: in the presence of an initiator, using a fluorinated alcohol compound as a solvent, and performing a ring-opening polymerization reaction of L-alanine-N-carboxyl-intracyclic acid anhydride to generate poly-L-alanine.
[0010] In the present invention, the source of L-alanine-N-carboxyl-intracyclic anhydride is not limited, and it can be prepared by existing methods such as phosgene method.
[0011] Preferably, the fluorinated alcohol compound includes at least one of hexafluoroisopropanol, 4-fluorobenzyl alcohol, 2,6-difluorobenzyl alcohol, 4-(trifluoromethyl)benzyl alcohol, and pentafluorobenzyl alcohol; preferably at least one of 4-fluorobenzyl alcohol, 2,6-difluorobenzyl alcohol, 4-(trifluoromethyl)benzyl alcohol, pentafluorobenzyl alcohol, and hexafluoroisopropanol.
[0012] In the present invention, the fluorinated alcohol compounds include but are not limited to the above compounds. Fluorinated alcohols have good solubility for the product poly-L-alanine.
[0013] Preferably, the initiator is triethylamine or n-butylamine or a combination thereof.
[0014] Preferably, the mass ratio of the L-alanine-N-carboxyl-cyclic anhydride to the solvent is 1:10-50; preferably 1:20-40.
[0015] Preferably, the molar ratio of the L-alanine-N-carboxyl-cyclic anhydride to the initiator is 1:10-60; preferably 1:30-50.
[0016] Preferably, the reaction temperature of the ring-opening polymerization reaction is 10-80° C., and the reaction time is 2-10 h; preferably, the reaction temperature is 20-50° C., and the reaction time is 4-8 h.
[0017] Preferably, the method specifically comprises the following steps:
[0018] S1, add L-alanine-N-carboxyl-cyclic anhydride and fluorinated alcohol compound into the reaction vessel, then add initiator, heat in a water bath at a constant temperature, and stir to react;
[0019] S2, adding anhydrous ethanol to the reaction system of S1 to terminate the reaction and obtain a white suspension;
[0020] S3. Filter the suspension, soak and wash with ethyl acetate, and vacuum dry to obtain poly-L-alanine.
[0021] Another object of the present invention is to provide a poly-L-alanine with a high degree of polymerization prepared by the above method.
[0022] Beneficial effects: The present invention introduces fluorinated alcohol solvents into the NcAn reaction system, which not only increases the solubility of the product, but also may play a role in catalyzing the reaction, thereby obtaining poly-L-alanine with a high degree of polymerization, which has a high molecular weight, a characteristic viscosity [η] of up to 1.58 dL / g, and a high yield. The present invention solves the problem of poor product solubility by using fluorinated alcohol solvents, while avoiding the use of explosive reagent nitrobenzene, making the process safer and more reliable; and poly-L-alanine has a high degree of polymerization and a high molecular weight, which provides good support for subsequent material applications. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is described in detail below through specific embodiments.
[0024] Comparative Example 1
[0025] Add 5 g of L-Ala-NCAn and 100 mL of nitrobenzene solvent and 0.11 g of triethylamine into a four-necked flask, slowly heat to 40°C in a constant temperature bath, stir to dissolve, react for 5 h, add anhydrous ethanol to terminate the reaction, filter the product, soak and wash with ethyl acetate, and vacuum dry to obtain 3.8 g of a white solid with a yield of 76%.
[0026] The polymer prepared above was dissolved in dichloroacetic acid, and a solution with a mass concentration of 5 mg / mL was prepared in a 50 mL volumetric flask. The intrinsic viscosity of the polymer was measured by the dilution method using an Ubbelohde viscometer (tube diameter 0.78 mm, t0>100 s) at a temperature of (30±0.05)° C. The intrinsic viscosity was measured to be [η]=0.83 dL / g.
[0027] The results of Comparative Example 1 show that, using nitrobenzene as solvent and triethylamine as initiator, L-Ala-NCAn monomer can be ring-opened polymerized to generate poly-L-alanine, and the intrinsic viscosity of the polymer is [η]=0.83 dL / g.
[0028] Example 1
[0029] Add 5 g of L-Ala-NCAn and 100 mL of 4-fluorobenzyl alcohol solvent and 0.11 g of triethylamine into a four-necked flask, slowly heat to 40°C in a constant temperature bath, stir to dissolve, react for 5 h, add anhydrous ethanol to terminate the reaction, filter the product, soak and wash with ethyl acetate, and vacuum dry to obtain 4.2 g of a white solid with a yield of 84%.
[0030] The polymer prepared above was dissolved in dichloroacetic acid, and a solution with a mass concentration of 5 mg / mL was prepared in a 50 mL volumetric flask. The intrinsic viscosity of the polymer was measured by the dilution method using an Ubbelohde viscometer (tube diameter 0.78 mm, t0>100 s) at a temperature of (30±0.05)° C. The intrinsic viscosity was measured to be [η]=0.90 dL / g.
[0031] The results of Example 1 show that using 4-fluorobenzyl alcohol as a solvent and triethylamine as an initiator, L-Ala-NCAn monomer can be ring-opening polymerized to generate poly-L-alanine, and the intrinsic viscosity of the polymer is [η] = 0.90 dL / g, indicating that 4-fluorobenzyl alcohol as a solvent can effectively increase the degree of polymerization of the polymer.
[0032] Example 2
[0033] Add 5 g of L-Ala-NCAn and 100 mL of 2,6-difluorobenzyl alcohol solvent and 0.11 g of triethylamine into a four-necked flask, slowly heat to 40°C in a constant temperature bath, stir to dissolve, react for 5 h, add anhydrous ethanol to terminate the reaction, filter the product, soak and wash with ethyl acetate, and vacuum dry to obtain 4.3 g of a white solid with a yield of 86%.
[0034] The polymer was dissolved in dichloroacetic acid, and a solution with a mass concentration of 5 mg / mL was prepared in a 50 mL volumetric flask. The intrinsic viscosity of the polymer was measured by the dilution method using an Ubbelohde viscometer (tube diameter 0.78 mm, t0>100 s) at a temperature of (30±0.05)°C. The intrinsic viscosity was measured to be [η] = 1.23 dL / g.
[0035] The results of Example 2 show that, using 2,6-difluorobenzyl alcohol as solvent and triethylamine as initiator, L-Ala-NCAn monomer can be ring-opened polymerized to generate poly-L-alanine, and the intrinsic viscosity of the polymer is [η] = 1.23 dL / g, indicating that the increase of fluorine content can promote the growth of polymer chains.
[0036] Example 3
[0037] Add 5 g of L-Ala-NCAn and 100 mL of hexafluoroisopropanol solvent and 0.11 g of triethylamine into a four-necked flask, slowly heat to 40°C in a constant temperature bath, stir to dissolve, react for 5 h, add anhydrous ethanol to terminate the reaction, filter the product, soak and wash with ethyl acetate, and vacuum dry to obtain 4.5 g of a white solid with a yield of 90%.
[0038] The polymer was dissolved in dichloroacetic acid, and a solution with a mass concentration of 5 mg / mL was prepared in a 50 mL volumetric flask. The intrinsic viscosity of the polymer was measured by the dilution method using an Ubbelohde viscometer (tube diameter 0.78 mm, t0>100 s) at a temperature of (30±0.05)°C. The intrinsic viscosity was measured to be [η] = 1.58 dL / g.
[0039] The results of Example 3 show that, using hexafluoroisopropanol as solvent and triethylamine as initiator, L-Ala-NCAn monomer can be ring-opened polymerized to generate poly-L-alanine, and the intrinsic viscosity of the polymer is [η] = 1.58 dL / g, indicating that the growth of the polymer chain can be promoted with the increase of fluorine content.
[0040] Example 4
[0041] Add 5 g of L-Ala-NCAn and 150 mL of hexafluoroisopropanol solvent and 0.11 g of triethylamine into a four-necked flask, slowly heat to 50°C in a constant temperature bath, stir to dissolve, react for 4 h, add anhydrous ethanol to terminate the reaction, filter the product, soak and wash with ethyl acetate, and vacuum dry to obtain 4.6 g of a white solid with a yield of 92%.
[0042] The polymer was dissolved in dichloroacetic acid, and a solution with a mass concentration of 5 mg / mL was prepared in a 50 mL volumetric flask. The intrinsic viscosity of the polymer was measured by the dilution method using an Ubbelohde viscometer (tube diameter 0.78 mm, t0>100 s) at a temperature of (30±0.05)°C. The intrinsic viscosity was measured to be [η] = 1.60 dL / g.
[0043] The results of Example 4 show that, using hexafluoroisopropanol as solvent and triethylamine as initiator, L-Ala-NCAn monomer can be ring-opened polymerized to generate poly-L-alanine, and the intrinsic viscosity of the polymer is [η] = 1.60 dL / g. This indicates that increasing the amount of solvent used and raising the temperature are conducive to the generation of poly-L-alanine with a high degree of polymerization.
[0044] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for synthesizing poly-L-alanine with a high degree of polymerization, characterized in that: In the presence of an initiator and with a fluorinated alcohol compound as a solvent, L-alanine-N-carboxyl-intracyclic acid anhydride undergoes a ring-opening polymerization reaction to generate poly-L-alanine.
2. The method according to claim 1, characterized in that: The fluorinated alcohol compound includes at least one of hexafluoroisopropanol, 4-fluorobenzyl alcohol, 2,6-difluorobenzyl alcohol, 4-(trifluoromethyl)benzyl alcohol, and pentafluorobenzyl alcohol; preferably at least one of 4-fluorobenzyl alcohol, 2,6-difluorobenzyl alcohol, 4-(trifluoromethyl)benzyl alcohol, pentafluorobenzyl alcohol, and hexafluoroisopropanol.
3. The method according to claim 1 or 2, characterized in that: The initiator is triethylamine or n-butylamine or a combination thereof.
4. The method according to any one of claims 1 to 3, characterized in that: The mass ratio of the L-alanine-N-carboxyl-cyclic anhydride to the solvent is 1:10-50, preferably 1:20-40.
5. The method according to any one of claims 1 to 4, characterized in that: The molar ratio of the L-alanine-N-carboxyl-cyclic anhydride to the initiator is 1:10-60, preferably 1:30-50.
6. The method according to any one of claims 1 to 5, characterized in that: The reaction temperature of the ring-opening polymerization reaction is 10-80° C., and the reaction time is 2-10 hours; preferably, the reaction temperature is 20-50° C., and the reaction time is 4-8 hours.
7. The method according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, add L-alanine-N-carboxyl-cyclic anhydride and fluorinated alcohol compound into the reaction vessel, then add initiator, heat in a water bath at a constant temperature, and stir to react; S2, adding anhydrous ethanol to the reaction system of S1 to terminate the reaction and obtain a white suspension; S3. Filter the suspension, soak and wash with ethyl acetate, and vacuum dry to obtain poly-L-alanine.
8. Poly-L-alanine prepared by the method according to any one of claims 1 to 7.