Polyfluorinated heterocyclic polyarylether resin containing phthalazinone structure, paint and preparation method thereof, coating and preparation method thereof, and product

By using a coating composed of a polyfluoroheterocyclic polyaryl ether resin containing a diazinone structure and an organic solvent, the constraints on the liquid oxygen compatibility and low-temperature toughness of the composite liquid oxygen tank are solved, and liquid Improvement of liquid oxygen compatibility and low temperature performance of oxygen storage tanks.

CN118772402APending Publication Date: 2024-10-15DALIAN UNIV OF TECH

Patent Information

Application Number
CN202411007605.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-10-16
Filing Date
2024-07-25
Publication Date
2024-10-15

Smart Images

  • Figure CN118772402A_ABST
    Figure CN118772402A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, in particular to polyfluorinated heterocyclic polyarylether resin containing a phthalazinone structure, paint, a preparation method of the paint, a coating, a preparation method of the coating and a product of the coating, and the polyfluorinated heterocyclic polyarylether resin containing the phthalazinone structure comprises a polymer with the structure shown in the formula I: # imgabs0 #, m and n are mutually independent natural numbers between 0 and 40, and m and n are not 0 at the same time; # imgabs 1 # represents one or a combination of more of a direct bond, O, S, an alkylene group, an arylene group, a heteroalkylene group, and a heteroarylene group; and Ar is an aromatic connecting part formed by connecting one or more of groups with the following structure: # imgabs2. A coating adopting the resin provided by the invention as a matrix has good liquid oxygen compatibility and low-temperature toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure, a coating and a preparation method thereof, a coating and a preparation method thereof, and a product thereof. Background Art

[0002] In the field of aerospace, in order to reduce the weight of aircraft, resin-based composite materials are generally used to manufacture some of the components, and the most commonly used is carbon fiber reinforced epoxy resin-based composite materials. For example, the liquid oxygen tank of a rocket is made of such a composite material. However, the liquid oxygen tank made of such a composite material still has problems such as poor compatibility with liquid oxygen and low-temperature leakage. Studies have found that the liquid oxygen compatibility of the liquid oxygen tank made of the composite material is greatly affected by the molding process and the internal and external structure of the material. Generally speaking, a material system with good flame retardant properties may not necessarily meet the liquid oxygen compatibility requirements. There is a problem of mutual restriction in modifying the liquid oxygen compatibility and low-temperature toughness of the composite material. Although various modification methods have been carried out on the epoxy resin system of the composite tank to achieve the purpose of toughening, etc., the improvement of its intrinsic performance still does not meet the requirements. This makes the use of toughness coatings to improve the liquid oxygen compatibility of low-temperature composite tanks a possible technical means.

[0003] The core key feature of the coating used to improve the liquid oxygen compatibility of the composite liquid oxygen tank is that the resin matrix of the coating must not only have good liquid oxygen compatibility, but also have excellent low-temperature toughness. At present, some studies have reported benzoxazine resin systems, cyanate resin systems, and epoxy resin systems. These systems are conventional coating resin matrices. Although these resins can improve their liquid oxygen compatibility by improving their flame retardant properties, their low-temperature toughness does not meet practical requirements.

[0004] So far, there has been no report on using a coating based on a thermoplastic resin to improve the liquid oxygen compatibility of a composite liquid oxygen tank. Therefore, how to obtain a coating based on a thermoplastic resin with good liquid oxygen compatibility and low-temperature toughness is a technical problem that needs to be solved urgently in this technical field. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a polyfluoroheterocyclic polyarylether resin containing a diazinone structure, a coating and a preparation method thereof, a coating and a preparation method thereof and a product. The coating using the polyfluoroheterocyclic polyarylether resin containing a diazinone structure as a matrix has good liquid oxygen compatibility and low-temperature toughness, thereby improving the liquid oxygen compatibility of the composite liquid oxygen tank, and at the same time making the composite liquid oxygen tank also have excellent low-temperature toughness.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure, wherein the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure comprises a polymer having a structure shown in Formula I:

[0008]

[0009] in,

[0010] m and n are independently natural numbers between 0 and 40, and m and n are not 0 at the same time;

[0011] represents a direct bond, O, S, an alkylene group, an arylene group, a heteroalkylene group, and a heteroarylene group;

[0012] Ar is an aromatic linking moiety formed by connecting one or more groups having the following structures to each other:

[0013]

[0014] The coating using the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure provided by the present invention as a matrix has good liquid oxygen compatibility and low-temperature toughness, thereby improving the liquid oxygen compatibility of the composite liquid oxygen tank and at the same time making the composite liquid oxygen tank also have excellent low-temperature toughness.

[0015] In a second aspect, the present invention provides a polyfluoroheterocyclic polyarylether resin coating containing a diazinone structure, wherein the polyfluoroheterocyclic polyarylether resin coating containing a diazinone structure comprises the following components in percentage by weight: 10% to 25% of the polyfluoroheterocyclic polyarylether resin containing a diazinone structure described in the first aspect; and 75% to 90% of an organic solvent.

[0016] Furthermore, the organic solvent includes a high boiling point organic solvent and a low boiling point organic solvent.

[0017] Furthermore, it is characterized in that the boiling point of the high boiling point organic solvent is 150-250°C, and the boiling point of the low boiling point organic solvent is not greater than 100°C;

[0018] And / or, the mass ratio of the high boiling point organic solvent to the low boiling point organic solvent is (1:1) to (1:5);

[0019] And / or, the high boiling point organic solvent includes at least one of cyclohexanone, propylene glycol methyl ether, and propylene glycol methyl ether acetate; the low boiling point organic solvent includes at least one of isopropanol, ethyl acetate, methyl isobutyl ketone, and acetone.

[0020] In a third aspect, the present invention provides a method for preparing a polyfluoroheterocyclic polyarylether resin coating containing a diazinone structure as described in the second aspect, the preparation method comprising the following steps: dissolving the polyfluoroheterocyclic polyarylether resin containing a diazinone structure as described in the first aspect in the high boiling point organic solvent, and then mixing the formed solution with the low boiling point organic solvent.

[0021] In a fourth aspect, the present invention provides a coating, wherein the coating comprises a coating formed by the polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure as described in the second aspect.

[0022] Furthermore, the coating has a thickness of 1 to 500 μm;

[0023] and / or, according to a drop weight impact test, the coating has a drop weight impact strength of not less than 50 cm;

[0024] and / or, the coating has a flexibility of no greater than 1 mm;

[0025] And / or, the coating has a liquid oxygen shock sensitivity coefficient of less than 1%.

[0026] In a fifth aspect, the present invention provides a method for preparing the coating according to the fourth aspect, the preparation method comprising the following steps:

[0027] Applying step: applying the polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure as described in the second aspect to a substrate to form a coating layer;

[0028] Drying step: performing a pre-drying step and a post-drying step on the coating layer to form a coating on the substrate, wherein the temperature of the pre-drying is lower than that of the post-drying.

[0029] Further, the substrate is selected from carbon fiber reinforced epoxy resin-based composite materials;

[0030] And / or, the applying comprises one of coating, casting, and tape casting;

[0031] And / or, the coating comprises one of brush coating, roller coating, scraper coating and spray coating;

[0032] and / or, the spraying pressure is 0.1-0.5 MPa;

[0033] And / or, the pre-drying method includes one of oven drying, infrared radiation drying, and continuously blowing hot non-reactive gas over the surface of the coating layer for drying;

[0034] And / or, the pre-drying temperature is 20-100°C;

[0035] And / or, the pre-drying time is 0.5 to 2 hours;

[0036] and / or, in the post-drying step, the post-drying temperature is 120 to 200° C.;

[0037] And / or, the post-drying time is 0.2 to 2 hours;

[0038] And / or, the post-drying method includes one of oven drying, infrared radiation drying, and continuously blowing hot non-reactive gas over the surface of the coating layer for drying;

[0039] And / or, after the drying step, the preparation method further comprises the following step: repeatedly implementing the applying step and the drying step one or more times until the formed coating has a thickness of 1 to 500 μm.

[0040] In a sixth aspect, the present invention provides an article with a coating, wherein the article comprises a substrate and a coating attached to the substrate, wherein the coating comprises the coating described in the fourth aspect or a coating prepared by the preparation method described in the fifth aspect.

[0041] Compared with the prior art, the beneficial effects of the present invention include at least one of the following:

[0042] (1) The coating using the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure as a matrix has good liquid oxygen compatibility and low-temperature toughness, thereby improving the liquid oxygen compatibility of the composite liquid oxygen tank and at the same time making the composite liquid oxygen tank also have excellent low-temperature toughness.

[0043] (2) The polyfluoroheterocyclic polyarylether thermoplastic resin containing a phthalazinone structure provided by the present invention can be used as a resin matrix for coatings of products used at low temperatures (e.g., cryogenic containers, especially liquid oxygen tanks). In particular, the polyfluoroheterocyclic polyarylether thermoplastic resin not only has excellent flame retardancy, low-temperature toughness and liquid oxygen compatibility, but can also be dissolved in certain organic solvents for the preparation of coatings. The coating prepared using the coating is resistant to low temperatures (especially ultra-low temperatures), so that the coating of the present invention can be applied to cryogenic containers to prevent cracks caused by low-temperature brittleness. In particular, in view of the problems of liquid oxygen incompatibility and low-temperature leakage in composite liquid oxygen tanks in the current prior art, the method of coating the thermoplastic structural coating of the present invention on its inner lining can make the tank have both low-temperature toughness and liquid oxygen compatibility, thereby comprehensively solving the problems. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0045] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0046] In a first aspect, the present invention provides a polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure, wherein the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure comprises a polymer having a structure shown in Formula I:

[0047]

[0048] in,

[0049] m and n are independently natural numbers between 0 and 40 (for example, 0, 3, 5, 10, 20, 30 or 40), and m and n are not 0 at the same time;

[0050] represents a direct bond, O, S, an alkylene group, an arylene group, a heteroalkylene group, and a heteroarylene group;

[0051] Ar is an aromatic linking moiety formed by connecting one or more groups having the following structures to each other:

[0052]

[0053] When m and n are greater than 1, the individual repeating units constituting the polymer may be distributed therein in a random, block or alternating manner.

[0054] When both m and n are not 0, the present invention can improve the solubility and heat resistance of the polyfluoroheterocyclic polyarylether resin by including a segment corresponding to n.

[0055] The coating using the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure provided by the present invention as a matrix has good liquid oxygen compatibility and low-temperature toughness, thereby improving the liquid oxygen compatibility of the composite liquid oxygen tank and at the same time making the composite liquid oxygen tank also have excellent low-temperature toughness.

[0056] The present invention adopts a polyfluorinated nitrogen-containing heterocyclic thermoplastic resin (polyfluorinated heterocyclic polyarylether resin containing a diazinone structure) with better low-temperature toughness and higher flame retardancy as the resin matrix of the liquid oxygen tank coating, wherein the polyfluorinated nitrogen-containing heterocyclic thermoplastic resin has excellent flame retardancy and liquid oxygen compatibility, and can be dissolved in certain organic solvents, can be used to make coatings, and has excellent low-temperature toughness. The ultra-low temperature resistant coating developed by the resin is applied to the composite liquid oxygen tank, which can take into account both low-temperature toughness and liquid oxygen compatibility. At the same time, the present invention can be extended to other types of low-temperature containers to prevent cracks caused by low-temperature brittleness, etc.

[0057] In the above-mentioned polyfluoroheterocyclic polyarylether resin containing a diazinone structure, as an optional embodiment, m+n is 1 to 80 (for example, it can be 1, 10, 20, 30, 40, 50, 60, 70 or 80), preferably 5 to 75, more preferably 10 to 70, and most preferably 50 to 60.

[0058] In a second aspect, the present invention provides a polyfluoroheterocyclic polyarylether resin coating containing a diazinone structure, wherein the polyfluoroheterocyclic polyarylether resin coating containing a diazinone structure comprises the following components in percentage by weight: 10% to 25% (for example, 10%, 13%, 15%, 17%, 20% or 25%) of the polyfluoroheterocyclic polyarylether resin containing a diazinone structure described in the first aspect; and 75% to 90% (for example, 75%, 80%, 83%, 85%, 87% or 90%) of an organic solvent.

[0059] The organic solvent is not particularly limited, as long as the solvent can fully dissolve the polyfluoroheterocyclic polyarylether resin containing a diazinone structure under the defined concentration conditions. It can be a single solvent or a mixture of two or more organic solvents. In the polyfluoroheterocyclic polyarylether resin coating containing a diazinone structure, as a preferred embodiment, the organic solvent includes a high boiling point organic solvent and a low boiling point organic solvent. The high boiling point and low boiling point organic solvents can be mixed to form an azeotropic organic solvent, reduce the boiling point, and can also adjust the resin viscosity and improve the processability.

[0060] In the above polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure, as an optional embodiment, the boiling point of the high boiling point organic solvent is 150-250°C, for example, 150°C, 170°C, 200°C, 220°C or 250°C.

[0061] In the above polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure, as an optional implementation, the boiling point of the low-boiling-point organic solvent is not greater than 100°C.

[0062] In the above-mentioned polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure, as an optional embodiment, the mass ratio of the high boiling point organic solvent to the low boiling point organic solvent is (1:1) to (1:5), for example, the mass ratio can be 1:1, 1:2, 1:3, 1:3.5, 1:4 or 1:5, etc. Too much or too little low boiling point organic solvent may make it difficult to completely remove the solvent, difficult to dissolve the resin, and the coating viscosity is not suitable for spraying.

[0063] In the above-mentioned polyfluoroheterocyclic polyarylether resin coating containing a diazinone structure, as an optional implementation, the high boiling point organic solvent includes at least one of cyclohexanone, propylene glycol methyl ether, and propylene glycol methyl ether acetate; the low boiling point organic solvent includes at least one of isopropanol, ethyl acetate, methyl isobutyl ketone, and acetone.

[0064] In a third aspect, the present invention provides a method for preparing a polyfluoroheterocyclic polyarylether resin coating containing a diazinone structure as described in the second aspect, the preparation method comprising the following steps: dissolving the polyfluoroheterocyclic polyarylether resin containing a diazinone structure as described in the first aspect in the high boiling point organic solvent, and then mixing the formed solution with the low boiling point organic solvent.

[0065] The preparation method of the polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure provided by the invention can accelerate the dissolution rate of the resin.

[0066] In a fourth aspect, the present invention provides a coating, wherein the coating comprises a coating formed by the polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure as described in the second aspect.

[0067] The present invention uses a polyfluoroheterocyclic polyarylether thermoplastic resin with good liquid oxygen compatibility and good toughness at liquid oxygen temperature as the base of the coating, dissolves the resin in an organic solvent by stirring to prepare the coating, and obtains the desired coating by a specific spraying process. The coating has high mechanical properties, resistance to high and low temperature environmental impact, and excellent liquid oxygen compatibility, and can be applied to high and low temperature resistant containers in the aerospace field, and can effectively solve the problems of liquid oxygen leakage caused by low temperature brittle cracking of containers such as epoxy resin-based composite materials such as liquid oxygen tanks.

[0068] In the above coating, as an optional embodiment, the thickness of the coating is 1 to 500 μm, preferably 10 to 200 μm, more preferably 20 to 100 μm, and most preferably 45 to 85 μm, for example, it can be 45 μm, 50 μm, 55 μm, 60 μm, 70 μm or 85 μm, etc.

[0069] In the above coating, the coating should have sufficient impact strength. As an optional embodiment, according to a drop weight impact test, the coating has a drop weight impact strength of not less than 50 cm.

[0070] In the above coating, the coating should have sufficient flexibility. As an optional embodiment, the coating has a flexibility greater than 0.1 mm, preferably no greater than 1 mm.

[0071] In the above coating, the coating should also have a sufficiently low liquid oxygen shock sensitivity coefficient. As an optional embodiment, the coating has a liquid oxygen shock sensitivity coefficient of less than 1%, and most preferably, has a liquid oxygen shock sensitivity coefficient of 0%.

[0072] In a fifth aspect, the present invention provides a method for preparing the coating according to the fourth aspect, the preparation method comprising the following steps:

[0073] Applying step: applying the polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure as described in the second aspect to a substrate to form a coating layer;

[0074] Drying step: performing a pre-drying step and a post-drying step on the coating layer to form a coating on the substrate, wherein the temperature of the pre-drying is lower than that of the post-drying.

[0075] Most of the low boiling point organic solvent can be evaporated and removed by pre-drying.

[0076] The present invention can keep the overall shape of the coating unchanged after low-temperature pre-drying. If it is directly dried at high temperature, the solvent will evaporate too quickly to cause bubbles in the film and defects after molding.

[0077] In the above-mentioned method for preparing the coating, the substrate can be a composite material commonly used to prepare low-temperature containers. As an optional embodiment, the substrate is selected from a carbon fiber reinforced epoxy resin-based composite material, preferably a carbon fiber reinforced epoxy resin-based composite material used to prepare a liquid oxygen tank of a rocket.

[0078] In the above-mentioned method for preparing the coating, as an optional implementation, the applying includes one of coating, casting, and tape casting.

[0079] In the above-mentioned method for preparing the coating, as an optional implementation, the coating includes one of brushing, roller coating, scraping and spraying.

[0080] In the above coating preparation method, as an optional implementation, the spraying pressure is 0.1 to 0.5 MPa, preferably 0.2 to 0.5 MPa.

[0081] In the above-mentioned method for preparing the coating, the pre-drying can be implemented in a variety of ways. As an optional implementation, the pre-drying method includes oven drying, infrared radiation drying, and continuously blowing hot non-reactive gas over the surface of the coating layer for drying.

[0082] In the above method for preparing the coating, as an optional embodiment, the pre-drying temperature is 20 to 100°C, preferably 30 to 90°C, more preferably 40 to 80°C, and most preferably 60°C.

[0083] In the above coating preparation method, as an optional embodiment, the pre-drying time is 0.5 to 2 hours, preferably 0.75 to 1.5 hours, more preferably 1 hour. If the time is too short, most of the low boiling point solvent cannot be evaporated and removed, and if the time is too long, energy will be consumed.

[0084] In the preparation method of the above-mentioned coating, in the post-drying step, the coating layer is post-dried at a temperature higher than the pre-drying temperature, so as to evaporate and remove most of the high-boiling point organic solvent. As an optional embodiment, the post-drying temperature is 120 to 200°C, preferably 130 to 180°C, more preferably 140 to 160°C, and most preferably 150°C.

[0085] In the above method for preparing the coating, as an optional implementation, the post-drying time is 0.2 to 2 hours, preferably 0.3 to 1.5 hours, and more preferably 0.5 to 1 hour.

[0086] In the above-mentioned method for preparing the coating, the post-drying can be implemented in a variety of ways. As an optional implementation, the post-drying method includes oven drying, infrared radiation drying, and continuously blowing hot non-reactive gas over the surface of the coating layer for drying.

[0087] In the above coating preparation method, as an optional implementation, after the drying step, the preparation method further comprises the following steps:

[0088] The applying step and the drying step are repeated one or more times until the formed coating reaches a thickness of 1 to 500 μm, preferably 10 to about 200 μm, more preferably 20 to 100 μm, and most preferably 45 to 85 μm.

[0089] In the above-mentioned method for preparing the coating, as an optional implementation, the applying step and the drying step are preferably repeated 1 to 6 times, for example, 2 times, 3 times, 5 times or 6 times.

[0090] In a sixth aspect, the present invention provides an article with a coating, which comprises a substrate and a coating attached to the substrate, wherein the coating comprises the coating described in the fourth aspect or a coating prepared by the preparation method described in the fifth aspect.

[0091] In the above-mentioned coated product, as an optional embodiment, the substrate is selected from a carbon fiber reinforced epoxy resin-based composite material, preferably a carbon fiber reinforced epoxy resin-based composite material used to prepare a liquid oxygen tank of a rocket.

[0092] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0093] In the following examples and comparative examples:

[0094] The impact strength of the coating is tested according to GB / T 1732-2020 paint film impact resistance determination method. The test plate is taken out and the paint film on the test plate is observed for cracks, wrinkles and peeling. The results are expressed as the maximum height (cm) at which no cracks, wrinkles or peeling are observed in three tests. The impact strength of 50cm means that after the test plate is impacted by a 50cm high hammer, there is no obvious change on the coating surface.

[0095] The flexibility of the coating is tested according to the GB / T 6742-2007 paint and varnish bending test to observe whether the paint film has reticulation, cracks and peeling. Flexibility 1mm means: after testing on a shaft with a shaft diameter of 1mm, the coating has no obvious changes.

[0096] Liquid oxygen impact sensitivity test of the coating: The coating in the embodiment and the comparative example is applied to an aluminum sheet, and the material of the "aluminum sheet + coating" is subjected to a normal pressure liquid oxygen impact test. According to the test standard "Test method for mechanical impact sensitivity of materials in liquid oxygen and pressurized environment" (QJ3177-2003), the mechanical impact test of the samples in a liquid oxygen environment is carried out in batches (20 per batch), and the test results are observed and recorded. The test equipment is a FYDZ-3 liquid oxygen impact testing machine, the test temperature is 28°C, the humidity is 80%, and the impact energy is 98J.

[0097] Low temperature bending performance test: According to the national standard GB / T 2567-2008 "Resin casting performance test method". The specimens were polished with fine sandpaper and placed in a drying oven to eliminate residual thermal stress. The samples were kept dry before testing. The tensile test was conducted on a universal testing machine in a low temperature environment box. During the test, the temperature of the environment box was kept at 90K by liquid nitrogen. The test speed was set to 2mm / min.

[0098] Bending strength f The calculation formula for (MPa) is as follows

[0099]

[0100] Among them, P represents the maximum load borne by the specimen (N); L represents the lower support span in the bending test (mm); b represents the width of the specimen (mm); h represents the thickness of the specimen (mm).

[0101] Example 1

[0102] The molecular structure formula of the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure provided in this embodiment is as follows:

[0103]

[0104] in, Indicates a direct key.

[0105] The 5% thermal weight loss temperature of the polyfluoroheterocyclic polyarylether resin is 466° C., and the glass transition temperature (Tg) is 295° C.

[0106] The synthesis steps of polyfluoroheterocyclic polyarylether resin are as follows:

[0107]

[0108] The monomer DOPO-DHPZ was purchased from Dalian Baolimo New Materials Co., Ltd., and DFBP, DCS, DMAc, toluene and K2CO3 were purchased from Shanghai MacLean Biochemical Technology Co., Ltd.

[0109] In a 250ml three-necked flask equipped with mechanical stirring, oil bath, reflux water separation device and nitrogen protection device, add 0.04molDFBP, 0.10molDOPO-DHPZ, 0.06molDCS, 0.14molK2CO3, 50mLDMAc and 100mltoluene. Under nitrogen protection, raise the system temperature to 130℃, reflux with water for 2h to promote the salt-forming reaction of bisphenol monomer, and use toluene reflux to remove the water in the system. After the water is removed, cool down to 110℃ and continue the reaction. The degree of reaction is judged by sampling and observation. After the polymerization reaches the appropriate degree, add solvent DMAc to the polymerization system to reduce the viscosity of the system, and pour the polymer solution into hot water while stirring rapidly to obtain a white flocculent polymer.

[0110] The polyfluoroheterocyclic polyarylether resin coating containing diazonium ketone structure provided in this embodiment comprises the following components by mass: 4 g of the polyfluoroheterocyclic polyarylether resin containing diazonium ketone structure provided in this embodiment, 13 g of cyclohexanone, and 13 g of acetone.

[0111] The preparation method of the polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure provided in this embodiment comprises the following steps:

[0112] 4 g of the polyfluoroheterocyclic polyarylether resin containing a diazinone structure provided in this embodiment was fully dissolved in 13 g of cyclohexanone (analytical grade) as a high boiling point organic solvent at room temperature, and impurities were filtered out. Then, the mixture was slowly added to 13 g of acetone (analytical grade) as a low boiling point organic solvent, and the mixture was fully stirred. The system was bubbling by ultrasound and vacuum extraction, and the coating preparation was completed.

[0113] The method for preparing the coating provided in this embodiment comprises the following steps:

[0114] Application step: spray the coating prepared in this example on the carbon fiber reinforced epoxy resin-based composite tank lining through a spray gun at a spray pressure of 0.2 MPa to form a coating layer, with the nozzle 20 cm away from the carbon fiber reinforced epoxy resin-based composite tank lining;

[0115] Drying step: Dry the coating layer to form a coating on the lining of the carbon fiber reinforced epoxy resin-based composite tank. The specific process parameters of the drying are: blow 60°C hot air from the upper manhole cover of the carbon fiber reinforced epoxy resin-based composite tank, blow it continuously over the coating surface, and dry it for 1 hour, then increase the hot air temperature to 150°C, continue to blow and dry it for 1 hour, and the hot air is naturally released from the lower manhole cover of the carbon fiber reinforced epoxy resin-based composite tank. After the drying is completed, repeat the above application and drying steps 3 times.

[0116] The final thickness of the obtained coating is 45μm, and the impact strength of the coating is 50cm (drop hammer impact); the flexibility is 1mm, the liquid oxygen impact sensitivity coefficient of the coating is 0%, and the bending strength at low temperature of 90K is 140.3MPa. Table 1 shows the experimental results tested in accordance with the provisions of the standard "Experimental Method for the Sensitivity of Materials to Mechanical Shock in Liquid Oxygen and Pressurized Oxygen Environments" (QJ3177-2003). The results show that when the number of tests is 20, no obvious fading, burning, flashing and explosion phenomena are observed in the test samples after each test. It shows that the coating of the present invention meets the requirements for the liquid oxygen impact sensitivity of composite materials in a normal pressure liquid oxygen environment. The liquid oxygen impact sensitivity coefficient is calculated according to the experimental results according to the formula shown in Formula 1:

[0117]

[0118] Wherein, N is the number of independent repeated impact tests of the sample, n is the total number of a certain type of impact phenomenon, Ci is the impact sensitivity weighting coefficient, and the weighting coefficient is specified as follows: Sustaining combustion C1=1; Explosion C2=0.9; Spark C3=0.7; Spark C4=0.6; Charred spots C5=0.4. For example, assuming that a certain material has 2 explosions, 5 sparks, and 6 charred spots in 20 impacts in the liquid oxygen shock sensitivity test, the corresponding impact sensitivity coefficient is: IRS=(0*1+2*0.9+5*0.7+0*0.6+6*0.4) / 20=38.5%.

[0119] Table 1

[0120]

[0121]

[0122] Example 2

[0123] The molecular structure formula of the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure provided in this embodiment is as follows:

[0124]

[0125] in, Indicates a direct key.

[0126] The 5% thermal weight loss temperature of the polyfluoroheterocyclic polyarylether resin is 492° C., and the glass transition temperature (Tg) is 290° C.

[0127] The synthesis steps of polyfluoroheterocyclic polyarylether resin are as follows:

[0128]

[0129] The monomer DOPO-DHPZ was purchased from Dalian Baolimo New Materials Co., Ltd., and DFBP, DFK, DMAc, toluene, and K2CO3 were purchased from Shanghai MacLean Biochemical Technology Co., Ltd.;

[0130] In a 250ml three-necked flask equipped with mechanical stirring, oil bath, reflux water separation device and nitrogen protection device, add 0.058molDFBP, 0.10molDOPO-DHPZ, 0.043molDFK, 0.14molK2CO3, 50mLDMAc (dimethylacetamide) and 100ml toluene. Under nitrogen protection, raise the system temperature to 130℃, reflux with water for 2h to promote the salt-forming reaction of bisphenol monomer, and use toluene reflux to remove the water in the system. After the water is removed, cool down to 110℃ and continue the reaction. The degree of reaction is judged by sampling and observation. After the polymerization reaches the appropriate degree, add solvent DMAc to the polymerization system to reduce the viscosity of the system. Pour the polymer solution into hot water while stirring rapidly to obtain a white flocculent polymer.

[0131] The polyfluoroheterocyclic polyarylether resin coating containing diazinone structure provided in this embodiment comprises the following components by weight: 4 g of the polyfluoroheterocyclic polyarylether resin containing diazinone structure provided in this embodiment, 10 g of cyclohexanone, and 10 g of ethyl acetate.

[0132] The preparation method of the polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure provided in this embodiment comprises the following steps:

[0133] 4 g of the polyfluoroheterocyclic polyarylether resin containing a diazinone structure provided in this embodiment was fully dissolved in 10 g of cyclohexanone (analytical grade) as a high boiling point organic solvent at room temperature, and impurities were filtered out. Then, the mixture was slowly added to 10 g of ethyl acetate (analytical grade) as a low boiling point organic solvent, and the mixture was fully stirred. The system was evacuated by ultrasound and vacuum, and the coating was prepared.

[0134] The method for preparing the coating provided in this embodiment comprises the following steps:

[0135] Application step: spray the coating prepared in this example on the carbon fiber reinforced epoxy resin-based composite tank lining through a spray gun at a spray pressure of 0.5 MPa to form a coating layer, with the nozzle 20 cm away from the carbon fiber reinforced epoxy resin-based composite tank lining;

[0136] Drying step: Dry the coating layer to form a coating on the lining of the carbon fiber reinforced epoxy resin-based composite tank. The specific process parameters of the drying are: blow 60°C hot air from the upper manhole cover of the carbon fiber reinforced epoxy resin-based composite tank, blow it continuously over the coating surface, and dry it for 1 hour, then increase the hot air temperature to 150°C, continue to blow and dry it for 1 hour, and the hot air is naturally released from the lower manhole cover of the carbon fiber reinforced epoxy resin-based composite tank. After the drying is completed, repeat the above application and drying steps once more.

[0137] The final thickness of the obtained coating is 85 μm, the impact strength of the coating is 50 cm (drop hammer impact), the flexibility is 1 mm, the liquid oxygen impact sensitivity coefficient of the coating is 0%, and the bending strength at low temperature of 90K is 135.8 MPa.

[0138] Example 3

[0139] The molecular structure formula of the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure provided in this embodiment is as follows:

[0140]

[0141] The 5% thermal weight loss temperature of the polyfluoroheterocyclic polyarylether resin is 407° C., and the glass transition temperature (Tg) is 241° C.

[0142] The polyfluoroheterocyclic polyarylether resin was synthesized with reference to Example 1.

[0143] The polyfluoroheterocyclic polyarylether resin coating containing diazonium ketone structure provided in this embodiment comprises the following components by mass: 4 g of the polyfluoroheterocyclic polyarylether resin containing diazonium ketone structure provided in this embodiment, 13 g of cyclohexanone, and 13 g of acetone.

[0144] The preparation method of the polyfluoroheterocyclic polyarylether resin coating containing diazinone structure provided in this embodiment is basically the same as that in Example 1, except that the polyfluoroheterocyclic polyarylether resin containing diazinone structure provided in Example 1 is replaced by the polyfluoroheterocyclic polyarylether resin containing diazinone structure provided in this embodiment.

[0145] The coating was prepared according to the coating preparation method provided in Example 1.

[0146] The final thickness of the obtained coating is 45 μm, the impact strength of the coating is 45 cm (drop hammer impact); the flexibility is 1 mm, the liquid oxygen impact sensitivity coefficient of the coating is 0%, and the bending strength at low temperature of 90K is 138.9 MPa.

[0147] Comparative Example 1

[0148] The molecular structure formula of the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure provided in this comparative example is as follows:

[0149]

[0150] in, Indicates a direct key.

[0151] Referring to Example 1, a coating and a coating comprising the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure provided in this comparative example were prepared.

[0152] The final thickness of the obtained coating is 45 μm, the impact strength of the coating is 20 cm (drop hammer impact); the flexibility is 5 mm, the liquid oxygen impact sensitivity coefficient of the coating is 20%, and the bending strength at low temperature 90K is 70.2 MPa.

[0153] Compared with Example 1, when the P-containing group is replaced by a Br substituent, the impact strength, room temperature toughness, liquid oxygen compatibility, and low temperature toughness of the coating are all reduced.

[0154] Comparative Example 2

[0155] The polyfluoroheterocyclic polyarylether resin coating containing diazonium ketone structure provided in this comparative example comprises the following components by mass: 4 g of the polyfluoroheterocyclic polyarylether resin containing diazonium ketone structure provided in Example 1 and 26 g of cyclohexanone.

[0156] The coatings and coatings were prepared according to Example 1.

[0157] The final thickness of the obtained coating is 45 μm, the impact strength of the coating is 25 cm (drop hammer impact); the flexibility is 4 mm, the liquid oxygen impact sensitivity coefficient of the coating is 27.5%, and the bending strength at low temperature of 90K is 120.1 MPa.

[0158] Compared with Example 1, when all the organic solvents in the coating are high-boiling point organic solvents, the impact strength, room temperature toughness, liquid oxygen compatibility, and low temperature toughness of the coating are all reduced. In the process of preparing the coating, the film quality is poor, the coating cracks, and the surface is rough.

[0159] Comparative Example 3

[0160] The polyfluoroheterocyclic polyarylether resin coating containing diazonium ketone structure provided in this comparative example comprises the following components by mass: 4 g of the polyfluoroheterocyclic polyarylether resin containing diazonium ketone structure provided in Example 1, and 26 g of acetone.

[0161] The coatings and coatings were prepared according to Example 1.

[0162] The final thickness of the obtained coating is 45 μm, the impact strength of the coating is 20 cm (drop hammer impact); the flexibility is 5 mm, the liquid oxygen impact sensitivity coefficient of the coating is 22.5%, and the bending strength at low temperature 90K is 30.5 MPa.

[0163] Compared with Example 1, when all the organic solvents in the coating are low-boiling point organic solvents, the impact strength, room temperature toughness, liquid oxygen compatibility, and low-temperature toughness of the coating are all reduced.

[0164] Comparative Example 4

[0165] The preparation method of the coating provided in this comparative example is basically the same as that of Example 1, except that in the drying step, the hot air temperature is directly increased to 150° C. and dried for 1.5 hours.

[0166] The final thickness of the obtained coating is 45 μm, the impact strength of the coating is 30 cm (drop hammer impact); the flexibility is 4 mm, the liquid oxygen impact sensitivity coefficient of the coating is 41%, and the bending strength at low temperature of 90K is 43.3 MPa.

[0167] Compared with Example 1, during the coating preparation process, when one-step drying is used, the performance of the resulting coating is poor, the one-step drying affects the coating forming, there are bubbles inside the coating, there are holes after forming, and the impact strength, room temperature toughness, liquid oxygen compatibility and low-temperature toughness of the final coating are all reduced.

[0168] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure, characterized in that: The polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure comprises a polymer having a structure shown in Formula I: in, m and n are independently natural numbers between 0 and 40, and m and n are not 0 at the same time; represents a direct bond, O, S, an alkylene group, an arylene group, a heteroalkylene group, and a heteroarylene group; Ar is an aromatic linking moiety formed by connecting one or more groups having the following structures to each other:

2. A polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure, characterized in that: The polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure comprises the following components in percentage by mass: 10% to 25% of the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure as claimed in claim 1; and 75% to 90% of an organic solvent.

3. The polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure according to claim 2, characterized in that: The organic solvent includes a high boiling point organic solvent and a low boiling point organic solvent.

4. The polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure according to claim 3, characterized in that: The boiling point of the high boiling point organic solvent is 150-250°C, and the boiling point of the low boiling point organic solvent is not greater than 100°C; And / or, the mass ratio of the high boiling point organic solvent to the low boiling point organic solvent is (1:1) to (1:5); And / or, the high boiling point organic solvent includes at least one of cyclohexanone, propylene glycol methyl ether, and propylene glycol methyl ether acetate; the low boiling point organic solvent includes at least one of isopropanol, ethyl acetate, methyl isobutyl ketone, and acetone.

5. A method for preparing a polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure as claimed in any one of claims 2 to 4, characterized in that: The preparation method comprises the following steps: dissolving the polyfluoroheterocyclic polyarylether resin containing a phthalazinone structure as claimed in claim 1 in the high boiling point organic solvent, and then mixing the formed solution with the low boiling point organic solvent.

6. A coating, characterized in that The coating layer comprises a coating layer formed by the polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure according to any one of claims 2 to 4.

7. The coating according to claim 6, characterized in that The thickness of the coating is 1 to 500 μm; and / or, according to a drop weight impact test, the coating has a drop weight impact strength of not less than 50 cm; and / or, the coating has a flexibility of no greater than 1 mm; And / or, the coating has a liquid oxygen shock sensitivity coefficient of less than 1%.

8. A method for preparing a coating as claimed in claim 6 or 7, characterized in that: The preparation method comprises the following steps: Applying step: applying the polyfluoroheterocyclic polyarylether resin coating containing a phthalazinone structure as claimed in any one of claims 2 to 4 to a substrate to form a coating layer; Drying step: performing a pre-drying step and a post-drying step on the coating layer to form a coating on the substrate, wherein the temperature of the pre-drying is lower than that of the post-drying.

9. The method for preparing the coating according to claim 8, characterized in that: The substrate is selected from carbon fiber reinforced epoxy resin-based composite materials; And / or, the applying comprises one of coating, casting, and tape casting; And / or, the coating comprises one of brush coating, roller coating, scraper coating and spray coating; and / or, the spraying pressure is 0.1-0.5 MPa; And / or, the pre-drying method includes one of oven drying, infrared radiation drying, and continuously blowing hot non-reactive gas over the surface of the coating layer for drying; And / or, the pre-drying temperature is 20-100°C; And / or, the pre-drying time is 0.5 to 2 hours; and / or, in the post-drying step, the post-drying temperature is 120 to 200° C.; And / or, the post-drying time is 0.2 to 2 hours; And / or, the post-drying method includes one of oven drying, infrared radiation drying, and continuously blowing hot non-reactive gas over the surface of the coating layer for drying; And / or, after the drying step, the preparation method further comprises the following step: repeatedly implementing the applying step and the drying step one or more times until the formed coating has a thickness of 1 to 500 μm.

10. An article with a coating, the article comprising a substrate and a coating attached to the substrate, characterized in that: The coating comprises the coating according to claim 6 or 7 or the coating prepared by the preparation method according to claim 8 or 9.

Citation Information

Patent Citations

  • Polyarylether with phosphaphenanthrene structure and method for synthesizing the same

    CN101565503A

  • Method for synthesizing perfluoro-cyclobutyl polyarylether with phthalazinone structures

    CN109456435A

  • Copolymerized aryl ether sulfone containing bis (phthalazinone) structure and preparation method thereof

    CN113461943A

  • High Temperature Poly(aryl ether)s Containing a Phthalazinone Moiety

    US20110166317A1

Cited By

  • Preparation method of novel tough epoxy resin anticorrosive coating

    CN120137499A