Alkyl silicone oil for immersed cooling medium of data center and preparation method of alkyl silicone oil
By performing an addition reaction under a platinum catalyst and a ring-opening reaction under an acid catalyst, an alkyl silicone oil that is clear, transparent and fluid at low temperatures is prepared, which solves the problem of insufficient performance of existing cooling media at low temperatures. A cooling medium with low SiH residual content and high compatibility is achieved, which is suitable for data center immersion cooling.
Patent Information
- Application Number
- CN202410979915.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Existing fluid cooling media are not clear, transparent and fluid at low temperatures, and have a high residual amount of SiH, which affects performance and cannot meet the needs of data center immersed cooling media.
The addition reaction of tetramethylcyclotetrasiloxane and olefins under a platinum catalyst is carried out, followed by a ring-opening reaction with an end-capping agent under an acid catalyst, and the alkyl silicone oil prepared through distillation and impurity removal steps is used to control the SiH residue. The amount is less than 1ppm, ensuring dielectric performance and compatibility.
The prepared alkyl silicone oil is clear, transparent and has good fluidity at -30°C or -40°C. It has low SiH residual content, improves dielectric properties and compatibility, is suitable for data center immersion cooling media, and reduces energy consumption.
Smart Images

Figure CN118772409A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of cooling media, and more specifically, to an alkyl silicone oil used as an immersion cooling medium for a data center and a preparation method thereof. Background Art
[0002] In order to reduce energy consumption, the PUE value of the data center must be reduced to a certain level. Traditional air cooling consumes a lot of energy and is noisy. The immersion liquid cooling solution, which uses a fluid cooling medium in direct contact with the data center equipment, can reduce the PUE to a level close to 1. This is also the most effective solution to reduce data center energy consumption. This solution requires a fluid cooling medium to transfer heat.
[0003] Existing fluid cooling media include fluorinated liquid, mineral oil and silicone oil. Fluorinated liquid has a high density and a low boiling point; mineral oil is cheap but has poor compatibility and poor anti-aging performance; ordinary silicone oil has good anti-aging performance, but its dielectric constant is large and cannot meet the requirements. Therefore, the modification of silicone oil to obtain a cooling medium with better performance is a direction that current researchers are more interested in. For example, patent CN 116438502A mentions a method for preparing a side-chain alkyl silicone oil, and also mentions the basic properties of the direct cooling fluid, but the alkyl silicone oil obtained by the preparation method mentioned in the document has a high SiH residual content. DOWSIL publicly sold on the market TM When the temperature of ICL-1000Fluid coolant is lower than 25℃, the silicone oil sold becomes turbid, which limits its application. Summary of the invention
[0004] The first purpose of the present invention is to provide an alkyl silicone oil for use as an immersion cooling medium in a data center. The alkyl silicone oil is clear and transparent at low temperatures (for example, -30°C) and still has fluidity (preferably, it is clear and transparent and still has fluidity at -40°C), which can meet more application scenarios. The process of the present invention is simple and the viscosity of the silicone oil can be flexibly adjusted according to market demand.
[0005] The alkyl silicone oil used as a cooling medium for immersion in a data center includes a substance having the following molecular structure formula (I):
[0006] (CH3)3SiO[(C n H 2n+1 (CH3)SiO] m Si(CH3)3
[0007] Formula (I)
[0008] Wherein, n is 8 or 10, and m is a positive integer not less than 4.
[0009] In a preferred embodiment of the present invention, n is 8 or 10, and m is 8 or 12.
[0010] In a preferred embodiment of the present invention, n is 8 and m is 12. The alkyl silicone oil having the structural formula is clear and transparent at -40°C and still has fluidity, which can better meet the requirements of immersion cooling medium in data centers.
[0011] Those skilled in the art will appreciate that, in the present invention, the value of m refers to an average value.
[0012] The alkyl silicone oil provided by the present invention is clear and transparent at -30°C and still has fluidity, and can effectively meet the requirement of reducing energy consumption.
[0013] Another object of the present invention is to provide a method for preparing an alkyl silicone oil, wherein the SiH residual content of the alkyl silicone oil prepared by the method is less than 1 ppm, which effectively improves the performance of the obtained alkyl silicone oil.
[0014] The preparation method of the alkyl silicone oil comprises the following steps:
[0015] 1) tetramethylcyclotetrasiloxane and olefin undergo addition reaction in the presence of a platinum catalyst, and distill to obtain an alkyl ring body;
[0016] 2) subjecting the alkyl ring body obtained in step 1) and the end-capping agent to a ring-opening reaction in the presence of an acid catalyst to obtain the alkyl silicone oil after removing impurities.
[0017] In a specific embodiment of the present invention, the olefin may be a common olefin in the art. In a preferred embodiment of the present invention, the above preparation method may be used to prepare an alkyl silicone oil having the above structural formula (I), that is, the olefin is preferably octene or decene.
[0018] That is, the present invention provides a method for preparing the alkyl silicone oil having the above structural formula, comprising the following steps:
[0019] 1) tetramethylcyclotetrasiloxane and olefin undergo addition reaction in the presence of a platinum catalyst, and distill to obtain an alkyl ring body; the olefin is octene or decene;
[0020] 2) subjecting the alkyl ring body obtained in step 1) and the end-capping agent to a ring-opening reaction in the presence of an acid catalyst to obtain the alkyl silicone oil after removing impurities.
[0021] In a preferred embodiment of the present invention, in order to reduce the residual Si-H bonds and improve the performance of the obtained alkyl silicone oil, in step 1), the molar ratio of tetramethylcyclotetrasiloxane to olefin is 1:(4-4.6).
[0022] In a specific embodiment of the present invention, a platinum catalyst commonly used in the art can be used, for example, chloroplatinic acid-isopropanol, chloroplatinic acid-triphenylphosphine or KARSTEDT catalyst, preferably KARSTEDT catalyst. Wherein, the platinum catalyst is preferably 5 to 20 ppm of the total mass of tetramethylcyclotetrasiloxane and olefin in terms of platinum, and more preferably 9 to 10 ppm.
[0023] In a preferred embodiment of the present invention, in step 1), the temperature of the addition reaction is 60-150° C., and the time is 2-6 hours.
[0024] In a preferred embodiment of the present invention, in step 1), the olefin and the platinum catalyst may be first mixed, activated under nitrogen protection, tetramethylcyclotetrasiloxane may be added dropwise, and after the addition is completed, the mixture may be reacted at 60-150° C. for 2-6 hours.
[0025] After the addition reaction in step 1) is completed, distillation can be performed at a reflux ratio of 10:5 to obtain an alkyl ring body.
[0026] In a preferred embodiment of the present invention, in step 2), the acid catalyst can be sulfuric acid, acetic acid, solid acid or cationic resin, preferably solid superacid. Solid superacids commonly used in the art can be used in the present invention, such as solid superacid HND-580.
[0027] In a preferred embodiment of the present invention, the end-capping agent is hexamethyldisiloxane.
[0028] In a preferred embodiment of the present invention, in step 2), the mass ratio of the alkyl ring body and the end-capping agent is (5-20): 1, preferably (9-15): 1, and more preferably (9-10): 1. The mass ratio of the acid catalyst is 1% to 10% of the total mass of the alkyl ring body and the end-capping agent, preferably 1.9 to 3%.
[0029] In one embodiment of the present invention, in step 2), the ring-opening reaction temperature is 50-120°C and the time is 6-12 hours. More preferably, the ring-opening reaction temperature is 100°C and the time is 10 hours.
[0030] In a specific embodiment of the present invention, after the ring-opening reaction in step 2) is completed, the catalyst is removed, and then the low-boiling substances are removed (for example, by distillation at 200-240° C.), and after cooling to room temperature, the odor is removed (for example, using an adsorbent to remove odor, etc.), and the color is removed to obtain alkyl silicone oil.
[0031] The alkyl silicone oil provided by the present invention is clear and transparent at -30°C (preferably -40°C) and still has fluidity, and can cope with more application scenarios. The method for preparing the alkyl silicone oil provided by the present invention can control the residual amount of SiH to below 1ppm (preferably not higher than 0.1ppm) and reduce the hydrocarbon residue content to below 0.5%. The alkyl silicone oil obtained by the preparation method provided by the present invention and used as an immersion cooling medium for data centers does not contain -(CH3)2SiO- segments, thereby improving the dielectric properties of the alkyl silicone oil and the compatibility with other materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is the H NMR spectrum of tetraoctyltetramethylcyclotetrasiloxane in Example 1;
[0033] Figure 2 is the gas phase spectrum of tetraoctyltetramethylcyclotetrasiloxane in Example 1;
[0034] Figure 3 This is the H NMR spectrum of tetradecyltetramethylcyclotetrasiloxane in Example 2. DETAILED DESCRIPTION
[0035] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0036] Example 1
[0037] 1)Tetraoctyltetramethylcyclotetrasiloxane ([(C8H 17 Preparation of )(CH3)SiO]4)
[0038] 246.4 g of octene and 0.73 g of 5000 ppm KARSTEDT catalyst were added to a three-necked flask, nitrogen was passed through, and the mixture was activated at 50°C for 1 h. Then, 120 g of tetramethylcyclotetrasiloxane was added dropwise through a dropping funnel, and the temperature was controlled to avoid temperature surge. After the addition was completed, the mixture was kept at 100°C for 2 h, and then distilled at a reduced pressure of -0.098 MPa at a reflux ratio of 10:5. After the top temperature was stabilized at 245°C, the product was collected by intermediate distillation to obtain tetraoctyltetramethylcyclotetrasiloxane.
[0039] The product is colorless and transparent. No SiH bonds were detected in the H NMR spectrum of the product. Figure 1 The gas phase peaks are typical peaks of four isomers of tetracyclic ring. Figure 2 , and in the gas phase spectrum Figure 3 No characteristic peak of octene was observed at .2 min, indicating that the content of hydrocarbon residues was less than the sensitivity of the machine.
[0040] 2) Octyl silicone oil ((CH3)3SiO[(C8H 17)(CH3)SiO] 12 Preparation of Si(CH3)3)
[0041] 106.2 g of tetraoctyltetramethylcyclotetrasiloxane, 8.1 g of hexamethyldisiloxane and 2.3 g of solid superacid HND-580 were mixed and reacted at 100°C for 10 h. After the reaction, the catalyst was separated and low-boiling substances were removed under high vacuum conditions at 240°C. After cooling to room temperature, activated carbon was added for deodorization and decolorization to finally obtain colorless and transparent octyl silicone oil. The properties of the octyl silicone oil are shown in Table 1.
[0042] Example 2
[0043] 1) Tetradecyltetramethylcyclotetrasiloxane ([(C 10 H 21 Preparation of )(CH3)SiO]4)
[0044] 308g of decene and 0.856g of 5000ppm of KARSTEDT catalyst were added to a three-necked flask, nitrogen was passed through, and activated at 50℃ for 1h. Then 120g of tetramethylcyclotetrasiloxane was added dropwise through a dropping funnel, and the temperature was controlled to avoid temperature surge. After the addition was completed, the mixture was kept at 100℃ for 2h, and the reflux ratio was controlled to be 10:5 and the product was distilled under reduced pressure-0.098MPa. After the top temperature was stable, the product was collected at 265℃ to obtain the product tetradecyltetramethylcyclotetrasiloxane. The product was colorless and transparent, and the nuclear magnetic hydrogen spectrum was shown in Figure 3 After integral calculation, the SiH bond in the product has a hydrogen content of 0.1ppm.
[0045] 2) Decyl silicone oil ((CH3)3SiO[(C 10 H 21 Preparation of )(CH3)SiO]8Si(CH3)3)
[0046] 160g of tetradecyltetramethylcyclotetrasiloxane, 16.2g of hexamethyldisiloxane and 3.5g of solid superacid HND-580 were mixed and reacted at 100°C for 10h. After the reaction, the catalyst was separated and the low boiling point was removed under high vacuum at 240°C. After cooling to room temperature, activated carbon was added for deodorization and decolorization to finally obtain colorless and transparent decyl silicone oil. The properties of the decyl silicone oil are shown in Table 1.
[0047] The testing methods of various properties and parameters in the present invention are as follows:
[0048] The viscosity was determined at 40°C using a NDJ-79 viscometer.
[0049] Use a 50 ml standard specific gravity cup and an analytical balance to determine the density at 20°C, referring to standard GB / T 4472-2011.
[0050] Use ZC36 high insulation resistance tester to determine the resistance at 250V.
[0051] Flash point was determined using a Cleveland open cup flash point tester.
[0052] The dielectric constant was determined using a microwave network analyzer and an AC capacitance tester at 1000 Hz and 23°C, with reference to standard GB / T 5654-2007.
[0053] Use SFY-01A trace moisture meter to determine the moisture content.
[0054] The 1H spectrum was tested using Bruker Avance NEO 600 NMR and deuterated chloroform as solvent. The peak position of SiH in the spectrum was between 4.65 and 4.78 ppm. The SiH content was calculated by converting the integral area of SiH and the integral area of SiCH3 (near 0 ppm).
[0055] The residual hydrocarbons were tested by gas chromatography using the internal standard method with standards octene and decene.
[0056] Compatibility test: Cut the commercially available A56 hardness, translucent special silicone rubber for the electronic field (model SH-8160, hereinafter referred to as silicone rubber) and A71 hardness EPDM rubber (purchased from Haiba Rubber) into 5cm*0.5cm*0.2cm pieces respectively, record the initial data and immerse them in 50℃ modified silicone oil for 4 months, wipe them clean and measure the data, and finally evaluate them based on the change rate. A change rate of less than 15% is considered qualified.
[0057] Table 1 Properties of alkyl silicone oil
[0058]
[0059]
[0060] Finally, the method of the present invention is only a preferred embodiment and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An alkyl silicone oil used as a cooling medium for immersion in data centers, It is characterized in that The alkyl silicone oil includes a substance having the following molecular structure formula (I): (CH 3 , 3 SiO[(C n H 2n+1 (CH 3 )SiO] m Si(CH 3 , 3 Formula (I), Wherein, n is 8 or 10, and m is a positive integer not less than 4.
2. The alkyl silicone oil according to claim 1, It is characterized in that The n is 8 or 10, and the m is 8 or 12.
3. The alkyl silicone oil according to claim 2, It is characterized in that The n is 8 and the m is 12.
4. The alkyl silicone oil according to any one of claims 1 to 4, It is characterized in that The alkyl silicone oil is in a transparent fluid state at minus 30°C.
5. A method for preparing an alkyl silicone oil, It is characterized in that The steps include: 1) tetramethylcyclotetrasiloxane and olefin undergo addition reaction in the presence of a platinum catalyst, and distill to obtain an alkyl ring body; the olefin is octene or decene; 2) subjecting the alkyl ring body obtained in step 1) and the end-capping agent to a ring-opening reaction in the presence of an acid catalyst to obtain the alkyl silicone oil after removing impurities.
6. The preparation method according to claim 5, It is characterized in that In step 1), the molar ratio of tetramethylcyclotetrasiloxane to olefin is 1:(4-4.6); the platinum catalyst is 5-20 ppm of the total mass of tetramethylcyclotetrasiloxane and olefin in terms of platinum.
7. The preparation method according to claim 5, It is characterized in that In step 1), the temperature of the addition reaction is 60-150° C. and the time is 2-6 hours.
8. The preparation method according to any one of claims 5 to 7, It is characterized in that In step 2), the acid catalyst is a solid superacid; And / or, the end-capping agent is hexamethyldisiloxane.
9. The preparation method according to any one of claims 5 to 7, It is characterized in that In step 2), the mass ratio of the alkyl ring body and the end-capping agent is (5-20):1; And / or, the acid catalyst is 1% to 10% of the total mass of the alkyl ring body and the end-capping agent.
10. The preparation method according to any one of claims 5 to 7, It is characterized in that In step 2), the ring-opening reaction is carried out at a temperature of 50 to 120° C. and for a time of 6 to 12 hours.
Citation Information
Patent Citations
Phenyl alkyl silicone oil preparation method
CN104961897A
Solvent-free preparation method of octyl silicone oil at normal temperature
CN106866970A
Alkyl methylsiloxane liquid immersion cooling medium
CN116438502A
Immersed cooling liquid based on silicone oil for electronic components
CN116731689A
Modified silicone oil as well as preparation method and application thereof
CN118325095A
Cited By
Preparation method of alkyl modified silicone oil single-phase immersed cooling liquid and application of alkyl modified silicone oil single-phase immersed cooling liquid in cooling of data center
CN119613724A
Alkyl silicone oil for immersed cooling medium of data center and preparation method of alkyl silicone oil
CN120842580A
Alkyl silicone oil for data center immersion cooling medium and method of making
CN120842580B
Organic silicon immersed cooling liquid for data center and application method of organic silicon immersed cooling liquid
CN120924242A
Fluorine-free liquid coolant, preparation method therefor and use thereof
WO2025236415A1