Preparation method of biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical property
By using sodium carboxymethyl starch, sodium alginate and microcrystalline cellulose materials, combined with the plasticizing effect of glycerol, and adjusting the pH to improve the mechanical and hydrophobic properties of the film, the problem of insufficient mechanical and hydrophobic properties of starch-based materials is solved. Problem, the preparation of biodegradable films with high mechanical properties and good hydrophobic properties has been achieved, which has potential application prospects for degradable plastics.
Patent Information
- Application Number
- CN202410998817.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-15
AI Technical Summary
Traditional starch-based materials have deficiencies in mechanical and hydrophobic properties, making it difficult to be widely used in the field of biodegradable films.
Using sodium carboxymethyl starch, sodium alginate and microcrystalline cellulose as the main materials, by adjusting the pH of the mixed solution and adding glycerin as a plasticizer, the mechanical strength and hydrophobic properties of the film are improved, and hydrogen bonds are used to enhance intermolecular interactions. , enhance mechanical properties and hydrophobicity.
A biodegradable carboxymethyl starch sodium-based hydrophobic film with high mechanical properties and good hydrophobic properties is prepared. The tensile strength reaches 36.10MPa, the elongation at break reaches 156.15%, and the water contact angle reaches 96.57°. It is low-cost and has potential The application prospects of degradable plastics.
Smart Images

Figure CN118772461A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium starch-based film preparation, and in particular relates to a method for preparing a biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical properties. Background Art
[0002] Plastics play an important role in our daily life and production, bringing great convenience to mankind. However, traditional petroleum-based plastic products are difficult to degrade, which brings many adverse environmental problems. These problems have become the main driving force for people to find biodegradable alternatives. Among the many degradable materials, starch-based materials have the advantages of wide sources, non-toxicity, strong controllability of performance, good thermal processability and strong compatibility with other materials, and have attracted widespread attention from scientific researchers. However, due to its polyhydroxy structure, starch-based materials have disadvantages such as poor mechanical and hydrophobic properties and are difficult to be applied on a large scale. At present, in order to improve the overall performance of starch-based materials, scientists are actively studying the types and addition methods of various reinforcing materials and additives, which has become a hot research direction in the field of materials science.
[0003] Carboxymethyl starch (CMS) is an anionic starch derivative. Compared with native starch, it has the advantages of being soluble in cold water, having no tendency to reversal (recrystallization), and having higher thermal stability. It is non-toxic, biodegradable, and compatible with human biotechnology, and is widely used in many fields, such as pharmaceuticals and medicine, food industry, cosmetics, and environmental protection. Sodium alginate (SA) has a wide range of sources and is mainly extracted from brown algae. It is a linear polysaccharide with good film-forming properties, biocompatibility, and biodegradability. Sodium alginate is favored by many researchers in the fields of food industry, biomedicine, water treatment, and food packaging. For the selection of reinforcing materials, microcrystalline cellulose (MCC) has the advantages of abundant sources, high mechanical properties, non-toxicity, high specific surface area, and good biocompatibility. In order to improve the flexibility of the composite film, a plasticizer is usually added to the film-forming solution. Glycerol has been widely used as a plasticizer for starch-based films, which can effectively improve the flexibility of the film, and has the advantages of low cost and no safety hazards.
[0004] The present invention selects natural, green and non-toxic glycerol as a plasticizer and microcrystalline cellulose as a reinforcing material. The molecules of the microcrystalline cellulose contain a large number of hydroxyl groups, which can form crosslinks with hydroxyl groups in starch molecules through hydrogen bonds, thereby improving the mechanical strength and toughness of the film. At the same time, the pH of the mixed solution is adjusted. Under acidic conditions, the carboxylic acid groups of CMS / SA are protonated to form -COOH, which reduces charge repulsion and enhances the interaction between molecules, thereby increasing hydrophobicity. At the same time, more hydroxyl groups participate in the formation of hydrogen bonds, which increases the interaction between molecules, and can effectively improve the mechanical and hydrophobic properties of the CMS / SA blend. The obtained film has potential application prospects in the field of degradable plastics, and there is currently no relevant report in this regard. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a method for preparing a biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical properties and simple process and low cost. The method uses CMS as the main material of the film, SA as an additive of the CMS-based film, and improves the mechanical properties and hydrophobicity by adjusting the pH of the mixed solution. MCC and glycerol are used as reinforcing materials and plasticizers of the CMS-based film, and the mixed material is mechanically stirred at room temperature to promote uniform mixing of the materials, and then coated on a polytetrafluoroethylene plate and dried to obtain the biodegradable sodium carboxymethyl starch-based hydrophobic film. The biodegradable sodium carboxymethyl starch-based hydrophobic film has the advantages of high mechanical properties, good hydrophobic properties and the like.
[0006] The present invention adopts the following technical scheme to solve the above problems, a method for preparing a biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical properties, characterized in that the specific steps are: Step S1, dissolving sodium carboxymethyl starch in secondary water at room temperature, adding glycerol and mechanically stirring to mix evenly, and placing in a refrigerator for hydration to obtain material A; Step S2, dissolving sodium alginate in secondary water at room temperature, and then adding glycerol to mechanically stir and mix to obtain material B; Step S3, mixing material A and material B in a volume ratio of 1:2-4, and then adjusting the pH of the mixed solution to 4 with a hydrochloric acid solution to obtain material C; Step S4, dissolving microcrystalline cellulose in water and mixing by ultrasonication to obtain material D; Step S5, adding material D to material C and mechanically stirring and mixing to obtain material E; Step S6, coating material E on a polytetrafluoroethylene plate, and drying at 20-30° C. to obtain a target product, a biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical properties.
[0007] A method for preparing a biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical properties, characterized in that the specific steps are: Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature, adding 1.2 mL of glycerol and stirring to mix well to obtain material A1; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature, adding 0.6 mL of glycerol and stirring to mix well to obtain material B1; Step S3, mixing material A1 and material B1 in a volume ratio of 1:3, and then adjusting the pH of the mixed solution to 4 with a prepared 1M hydrochloric acid solution to obtain material C1; Step S4, dissolving 1 g of microcrystalline cellulose in 9 mL of secondary water and ultrasonically mixing for 1 h to obtain material D1; Step S5, adding material D1, wherein the content of microcrystalline cellulose is 3 wt %, into material C1, and mechanically stirring and mixing for 2 h to obtain material E1; Step S6, coating the material E1 on a polytetrafluoroethylene plate, and drying at 25° C. to obtain the target product, a biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical properties.
[0008] Compared with the prior art, the present invention has the following advantages and beneficial effects: 1. The present invention uses raw materials such as sodium carboxymethyl starch, sodium alginate, and microcrystalline cellulose, which have the advantages of being biodegradable and having low preparation cost; 2. The present invention can significantly improve the hydrophobicity of the sodium carboxymethyl starch-based film by adjusting the pH of the mixed solution, and its water contact angle can reach 96.57°; 3. The present invention can achieve the goal of improving the mechanical properties of the sodium carboxymethyl starch-based film by adding microcrystalline cellulose as a reinforcing material, so that its tensile strength reaches 36.10 MPa and its elongation at break reaches 156.15%. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 It is the infrared spectra of comparative example products H6~H9; Figure 2 IR spectra of Example products H1 to H5; Figure 3 It is the mechanical test diagram of comparative example products H6~H9; Figure 4 It is the mechanical test diagram of the example products H1~H5; Figure 5 The water contact angle test diagram of comparative example products H6~H9; Figure 6 The water contact angle test diagram of the products H1 to H5 of the examples; Figure 7 It is the mechanical test diagram of the example products H1~H5. DETAILED DESCRIPTION
[0010] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Example 1
[0011] Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature, adding 1.2 mL of glycerol and stirring to mix well to obtain material A1; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature, adding 0.6 mL of glycerol and stirring to mix well to obtain material B1; Step S3, mixing material A1 and material B1 in a volume ratio of 1:3, and then adjusting the pH of the mixed solution to 4 with a prepared 1M hydrochloric acid solution to obtain material C1; Step S4, dissolving 1 g of microcrystalline cellulose in 9 mL of secondary water and ultrasonicating for 1 h to obtain material D1; Step S5, adding material D1 to material C1, wherein the content of microcrystalline cellulose is 1 wt% (matrix), and mechanically stirring and mixing for 2 h to obtain material E1; Step S6, coating material E1 on a polytetrafluoroethylene plate and drying at 25° C. to obtain product H1. Example 2
[0012] Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature, adding 1.2 mL of glycerol and stirring to mix well to obtain material A2; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature, adding 0.6 mL of glycerol and stirring to mix well to obtain material B2; Step S3, mixing material A2 and material B2 in a volume ratio of 1:3, and then adjusting the pH of the mixed solution to 4 with a prepared 1M hydrochloric acid solution to obtain material C2; Step S4, dissolving 1 g of microcrystalline cellulose in 9 mL of secondary water and ultrasonicating for 1 h to obtain material D2; Step S5, adding material D2 into material C2, wherein the content of microcrystalline cellulose is 3 wt% (matrix), and mechanically stirring and mixing for 2 h to obtain material E2; Step S6, coating material E2 on a polytetrafluoroethylene plate and drying at 25° C. to obtain product H2. Example 3
[0013] Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature, adding 1.2 mL of glycerol and stirring to mix well to obtain material A3; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature, adding 0.6 mL of glycerol and stirring to mix well to obtain material B3; Step S3, mixing material A3 and material B3 in a volume ratio of 1:3, and then adjusting the pH of the mixed solution to 4 with a prepared 1M hydrochloric acid solution to obtain material C3; Step S4, dissolving 1 g of microcrystalline cellulose in 9 mL of secondary water and ultrasonicating for 1 h to obtain material D3; Step S5, adding material D3 into material C3, wherein the content of microcrystalline cellulose is 5 wt% (matrix), and mechanically stirring and mixing for 2 h to obtain material E3; Step S6, coating material E3 on a polytetrafluoroethylene plate and drying at 25° C. to obtain product H3. Example 4
[0014] Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature, adding 1.2 mL of glycerol and stirring to mix well to obtain material A4; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature, adding 0.6 mL of glycerol and stirring to mix well to obtain material B4; Step S3, mixing material A4 and material B4 in a volume ratio of 1:3, and then adjusting the pH of the mixed solution to 4 with a prepared 1M hydrochloric acid solution to obtain material C4; Step S4, dissolving 1 g of microcrystalline cellulose in 9 mL of secondary water and ultrasonicating for 1 h to obtain material D4; Step S5, adding material D4 to material C4, wherein the content of microcrystalline cellulose is 7 wt% (matrix), and mechanically stirring and mixing for 2 h to obtain material E4; Step S6, coating material E4 on a polytetrafluoroethylene plate and drying at 25° C. to obtain product H4. Example 5
[0015] Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature, adding 1.2 mL of glycerol and stirring to mix well to obtain material A5; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature, adding 0.6 mL of glycerol and stirring to mix well to obtain material B5; Step S3, mixing material A5 and material B5 in a volume ratio of 1:3, and then adjusting the pH of the mixed solution to 4 with a prepared 1M hydrochloric acid solution to obtain material C5; Step S4, dissolving 1 g of microcrystalline cellulose in 9 mL of secondary water and ultrasonicating for 1 h to obtain material D5; Step S5, adding material D5 to material C5, wherein the content of microcrystalline cellulose is 9 wt% (matrix), and mechanically stirring and mixing for 2 h to obtain material E5; Step S6, coating material E5 on a polytetrafluoroethylene plate and drying at 25° C. to obtain product H5.
[0016] Comparative Example 1 Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature, adding 1.2 mL of glycerol and stirring to obtain material A6; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature, adding 0.6 mL of glycerol and stirring to mix well to obtain material B6; Step S3, material A6 and material B6 are mixed evenly at a volume ratio of 1:3 to obtain material C6, and the pH value of the mixed solution is measured to be 6; Step S4, coating material C6 on a polytetrafluoroethylene plate and drying at 25° C. to obtain product H6.
[0017] Comparative Example 2 Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature, adding 1.2 mL of glycerol and stirring to mix well to obtain material A7; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature, adding 0.6 mL of glycerol and stirring to mix well to obtain material B7; Step S3, mixing material A7 and material B6 in a volume ratio of 1:3, and then adjusting the pH of the mixed solution to 4 with a prepared 1M hydrochloric acid solution to obtain material C7; Step S4, coating material C7 on a polytetrafluoroethylene plate and drying at 25° C. to obtain product H7.
[0018] Comparative Example 3 Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature and stirring to mix uniformly to obtain material A8; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature and stirring to mix uniformly to obtain material B8; Step S3, mixing material A8 and material B8 in a volume ratio of 1:3, and then adjusting the pH of the mixed solution to 4 with a prepared 1M hydrochloric acid solution to obtain material C8; Step S4, coating material C8 on a polytetrafluoroethylene plate and drying at 25° C. to obtain product H8.
[0019] Comparative Example 4 Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature, adding 1.2 mL of glycerol and stirring to mix well to obtain material A9; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature, adding 0.6 mL of glycerol and stirring to mix well to obtain material B9; Step S3, mixing material A9 and material B9 in a volume ratio of 1:3, and then adjusting the pH of the mixed solution to 3 with a prepared 1M hydrochloric acid solution to obtain material C9; Step S4, coating material C9 on a polytetrafluoroethylene plate and drying at 25° C. to obtain product H9.
[0020] The final products H1-H9 were cut into rectangles of 30 mm × 10 mm, and the tensile properties of the samples were tested using a microcomputer-controlled electronic universal testing machine. The effective length of the sample in the fixture was 5 mm, and the clamping part of the fixture protected the sample to prevent damage to the sample and cause inaccurate data.
[0021] The properties of the samples in all the examples are as follows: Figure 3 and Figure 4 As shown, the tensile curves of the example products H1~H5 and the comparative example products H6~H9, the tensile strengths are 23.10MPa, 36.10MPa, 23.90MPa, 17.23MPa, 19.80MPa, 16.38MPa, 18.08MPa, 20.92MPa, 17.67MPa, and the elongations at break are 211.92%, 156.15%, 178.06%, 181.04%, 150.23%, 196.32%, 146.85%, 115.12%, 178.30%, respectively; Figure 5 and Figure 6 As shown, the contact angles of the example products H1~H5 and the comparative example products H6~H9 are 94.92°, 96.57°, 89.79°, 87.14°, 86.24°, 82.53°, 86.02°, 93.65°, and 48.48°, respectively. The test results show that the mechanical properties and hydrophobic properties of the target product H2 are greatly improved. The above results show that the product H2 has excellent hydrophobicity and mechanical properties and has potential application prospects in the field of degradable plastics.
[0022] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. A method for preparing a biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical properties. Features The specific steps are: Step S1, dissolving sodium carboxymethyl starch in secondary water at room temperature, adding glycerol and mechanically stirring to mix evenly, and placing in a refrigerator for hydration to obtain material A; Step S2, dissolving sodium alginate in secondary water at room temperature, and then adding glycerol to mechanically stir and mix to obtain material B; Step S3, mixing material A and material B in a volume ratio of 1:2-4, and then adjusting the pH of the mixed solution to 4 with a hydrochloric acid solution to obtain material C; Step S4, dissolving microcrystalline cellulose in water and mixing by ultrasonication to obtain material D; Step S5, adding material D to material C and mechanically stirring and mixing to obtain material E; Step S6, coating material E on a polytetrafluoroethylene plate, and drying at 20-30° C. to obtain a target product, a biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical properties.
2. The method for preparing the biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical properties according to claim 1, Features The specific steps are: Step S1, dissolving 5 g of sodium carboxymethyl starch in 95 g of secondary water at room temperature, adding 1.2 mL of glycerol and stirring to mix well to obtain material A1; Step S2, dissolving 1.6 g of sodium alginate in 98.4 g of secondary water at room temperature, adding 0.6 mL of glycerol and stirring to mix well to obtain material B1; Step S3, mixing material A1 and material B1 in a volume ratio of 1:3, and then adjusting the pH of the mixed solution to 4 with a prepared 1M hydrochloric acid solution to obtain material C1; Step S4, dissolving 1 g of microcrystalline cellulose in 9 mL of secondary water and ultrasonically mixing for 1 h to obtain material D1; Step S5, adding material D1, wherein the content of microcrystalline cellulose is 3 wt %, into material C1, and mechanically stirring and mixing for 2 h to obtain material E1; Step S6, coating the material E1 on a polytetrafluoroethylene plate, and drying at 25° C. to obtain the target product, a biodegradable sodium carboxymethyl starch-based hydrophobic film with high mechanical properties.