Imidazole functionalized composite anion exchange membrane

By introducing imidazole groups into the anion exchange membrane to covalently connect to polyetheretherketone, and combining with metal-organic framework dispersion, the problems of complex and unstable performance of existing modification methods are solved, and efficient and stable membrane modification is achieved. , improving the chemical stability and ionic conductivity of the membrane.

CN118772468APending Publication Date: 2024-10-15山西国润储能科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411015326.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing anion exchange membrane modification methods are complicated and the process conditions are harsh, making it difficult to achieve efficient and stable modification effects. At the same time, mechanical properties and chemical stability are often sacrificed when improving ion conductivity, resulting in short membrane service life and unstable performance.

Method used

By introducing an imidazole group into the trimethylhydroquinone monomer, it is covalently connected to the polyether ether ketone main chain to form a multifunctional site, and is physically and chemically cross-linked with polyvinyl alcohol to form a cross-linked structure, combining metal-organic The framework is evenly dispersed to improve the ionic conductivity, thermal stability and mechanical properties of the composite membrane.

Benefits of technology

It achieves excellent chemical stability, mechanical properties and high ion conductivity of the composite membrane, ensuring stable performance in high temperature and high ion environments and extending the service life of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772468A_ABST
    Figure CN118772468A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials and membranes, and discloses an imidazole functionalized composite anion exchange membrane, which comprises the following components: a trimethylhydroquinone monomer and imidazole functionalized polyether-ether-ketone prepared by a solution polymerization method, an imidazole group is connected to a main chain of the polyether-ether-ketone in a covalent bond manner to form a multifunctional site, and the multifunctional site is connected to the trimethylhydroquinone monomer. The polyether-ether-ketone has excellent chemical stability and mechanical property; polyvinyl alcohol and imidazole functionalized polyether-ether-ketone are physically and chemically cross-linked to form a matrix with a cross-linked structure, so that the structural strength and durability of the composite membrane are enhanced; and the metal organic framework is uniformly dispersed in a composite material matrix as an inorganic filler, so that the ionic conductivity and the thermal stability of the composite membrane are improved. An imidazole group is introduced into a molecular structure of a trimethylhydroquinone monomer and is connected to a main chain of polyether-ether-ketone in a covalent bond manner, so that the prepared imidazole functionalized polyether-ether-ketone has excellent chemical stability and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials and membranes, in particular to an imidazole-functionalized composite anion exchange membrane. Background Art

[0002] With the continuous progress of science and technology, anion exchange membranes are increasingly used in electrochemistry, fuel cells, water treatment and chemical synthesis. Anion exchange membranes have good ion conductivity and selectivity, and can effectively exchange and conduct ions in electrochemical devices, improving the overall performance and efficiency of the system. Especially in the field of fuel cells, high-performance anion exchange membranes can significantly improve the output power and energy conversion efficiency of fuel cells. Therefore, the development of anion exchange membranes with excellent performance has become a research hotspot.

[0003] In addition, anion exchange membranes also play a key role in flow battery systems. Flow batteries are electrochemical energy storage systems whose working principle is based on the circulation of two electrolytes between the positive and negative electrodes of the battery. In these systems, anion exchange membranes must not only provide good ion selectivity and conductivity, but also have sufficient chemical and mechanical stability to cope with various chemicals and physical stresses in the electrolyte. For example, during the discharge and charging process of the battery, the anion exchange membrane must effectively prevent the mixing of the positive and negative electrolytes while allowing the free flow of charge carriers (usually anions) to maintain the electrochemical activity and cycle efficiency of the battery.

[0004] At present, the common anion exchange membrane materials on the market mainly include perfluorosulfonic acid resin (Nafion) and polyarylether polymer materials. These materials enhance their ion conductivity and mechanical properties through chemical modification and cross-linking modification. For example, Nafion membrane has high ion conductivity, but its mechanical strength and dimensional stability are relatively poor, especially in high temperature and strong alkaline environment, the performance decreases significantly. PEEK material is known for its excellent mechanical strength and chemical stability, but its ion conductivity is relatively low, and its performance needs to be improved through functional modification.

[0005] Although the existing technology has improved the performance of anion exchange membranes to a certain extent, there are still some problems. First, the existing modification methods are complicated and the process conditions are harsh, making it difficult to achieve efficient and stable modification effects. Second, while improving ion conductivity, the mechanical properties and chemical stability of the membrane are often sacrificed, resulting in a short service life and unstable performance of the membrane in practical applications. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides an imidazole-functionalized composite anion exchange membrane, which solves the problems that the existing modification methods are complicated, the process conditions are harsh, and it is difficult to achieve efficient and stable modification effects.

[0007] To achieve the above objectives, the present invention is implemented by the following technical scheme: an imidazole-functionalized composite anion exchange membrane, comprising the following components:

[0008] Trimethylhydroquinone monomer, imidazole functionalized polyetheretherketone prepared by solution polymerization, wherein the imidazole group is covalently linked to the main chain of polyetheretherketone to form a multifunctional site, which makes polyetheretherketone have excellent chemical stability and mechanical properties;

[0009] Polyvinyl alcohol, together with imidazole-functionalized polyetheretherketone, forms a cross-linked matrix through physical and chemical cross-linking, which enhances the structural strength and durability of the composite film;

[0010] Metal-organic frameworks, as inorganic fillers, are uniformly dispersed in the composite matrix and enhance the ionic conductivity and thermal stability of the composite membrane through physical and chemical interactions.

[0011] Preferably, the molecular structure of the trimethylhydroquinone monomer contains at least one imidazole group, and the imidazole group is connected to the polyetheretherketone main chain through a nucleophilic substitution reaction. The composite of polyvinyl alcohol and imidazole-functionalized polyetheretherketone is chemically cross-linked by glutaraldehyde, and physical cross-linking is achieved by freeze-thaw method.

[0012] Preferably, the metal organic framework has a particle size of 20 nanometers to 200 nanometers and is dispersed in the composite material matrix at a mass fraction of 1% to 20%.

[0013] Preferably, the density of imidazole groups in the composite matrix is ​​0.1 to 2 moles of imidazole groups per gram of the composite matrix.

[0014] Preferably, the dimensional change rate of the composite membrane is less than 2% at an operating temperature of 80° C., and the ionic conductivity of the composite membrane is 0.05 S / cm to 0.15 S / cm at 25° C.

[0015] A method for preparing an imidazole-functionalized composite anion exchange membrane comprises the following steps:

[0016] Step 1, dissolving trimethylhydroquinone monomer in a solvent, adding imidazole group monomer and initiator to carry out solution polymerization to form imidazole functionalized polyetheretherketone solution;

[0017] Step 2, dissolving polyvinyl alcohol in water, adding a cross-linking agent and mixing;

[0018] Step 3: mixing the polyetheretherketone solution and the polyvinyl alcohol solution in a mass ratio of 1:1 to 1:5, adding the metal organic framework for ultrasonic dispersion and high-speed stirring;

[0019] Step 4: Prepare a cross-linked composite membrane through solution casting and heat treatment process.

[0020] Preferably, the solution polymerization reaction is carried out in the range of room temperature to 80° C., and the reaction time is 1 hour to 24 hours.

[0021] Preferably, the cross-linking agent is glutaraldehyde, and the cross-linking reaction is carried out at room temperature for a reaction time of 30 minutes to 6 hours.

[0022] Preferably, the ultrasonic dispersion time is 10 minutes to 60 minutes, the high-speed stirring speed is 1000 rpm to 5000 rpm, and the stirring time is 30 minutes to 120 minutes.

[0023] Preferably, the solution casting step comprises casting the mixed solution on a glass plate at a drying temperature of 50°C to 100°C for a drying time of 2 to 24 hours, and then heat treating the mixed solution in a vacuum drying oven at a temperature of 80°C to 150°C for a heat treatment time of 2 to 12 hours.

[0024] The present invention provides an imidazole-functionalized composite anion exchange membrane having the following beneficial effects:

[0025] 1. The present invention introduces an imidazole group into the molecular structure of the trimethylhydroquinone monomer and connects it to the main chain of polyetheretherketone in a covalent bond manner to form a multifunctional site, so that the prepared imidazole functionalized polyetheretherketone has excellent chemical stability and mechanical properties. Further, polyvinyl alcohol and imidazole functionalized polyetheretherketone are physically and chemically cross-linked to form a cross-linked structure matrix, which significantly enhances the structural strength and durability of the composite film.

[0026] 2. The present invention uniformly disperses the metal organic framework in the composite material matrix and utilizes its unique physical and chemical interactions to improve the ion conductivity and thermal stability of the composite membrane, thereby ensuring the excellent performance of the composite membrane in high temperature and high ion environment.

[0027] 3. The present invention controls the density of imidazole groups in the composite material matrix so that each gram of the matrix contains 0.1 to 2 moles of imidazole groups, thereby optimizing the ion conductivity and chemical stability of the membrane and ensuring its high efficiency in actual use. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a stereogram of the present invention. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Embodiment 1:

[0031] Please see attached Figure 1 The embodiment of the present invention provides an imidazole-functionalized composite anion exchange membrane, comprising the following components:

[0032] Trimethylhydroquinone monomer, imidazole functionalized polyetheretherketone prepared by solution polymerization, wherein the imidazole group is covalently linked to the main chain of polyetheretherketone to form a multifunctional site, which makes polyetheretherketone have excellent chemical stability and mechanical properties;

[0033] Polyvinyl alcohol, together with imidazole-functionalized polyetheretherketone, forms a cross-linked matrix through physical and chemical cross-linking, which enhances the structural strength and durability of the composite film;

[0034] Metal-organic frameworks, as inorganic fillers, are uniformly dispersed in the composite matrix and enhance the ionic conductivity and thermal stability of the composite membrane through physical and chemical interactions.

[0035] Preferably, the molecular structure of the trimethylhydroquinone monomer contains at least one imidazole group, which is connected to the polyetheretherketone main chain through a nucleophilic substitution reaction, and the composite of polyvinyl alcohol and imidazole-functionalized polyetheretherketone is chemically cross-linked by glutaraldehyde, and physical cross-linking is achieved by freeze-thaw method; the particle size of the metal organic framework is 20 nanometers to 200 nanometers, and is dispersed in the composite material matrix with a mass fraction of 1%-20%; the density of imidazole groups in the composite material matrix is ​​0.1 to 2 moles of imidazole groups per gram of composite material matrix; the dimensional change rate of the composite membrane is less than 2% at an operating temperature of 80°C, and the ionic conductivity of the composite membrane is 0.05S / cm to 0.15S / cm at 25°C.

[0036] In one embodiment, first, by introducing an imidazole group into the molecular structure of a trimethylhydroquinone monomer, and covalently connecting the imidazole group to the main chain of polyetheretherketone by a nucleophilic substitution reaction, an imidazole-functionalized polyetheretherketone with a multifunctional site is formed, providing excellent chemical stability and enhanced mechanical properties. Secondly, polyvinyl alcohol and imidazole-functionalized polyetheretherketone are chemically cross-linked by glutaraldehyde to form a stable cross-linked structure, and physical cross-linking is achieved by freeze-thaw method, further enhancing the structural strength and durability of the matrix. Thirdly, the metal organic framework is evenly dispersed in the matrix of the composite material, and the ionic conductivity and thermal stability of the composite membrane are improved through its unique physical and chemical interactions. Finally, by controlling the density of imidazole groups in the matrix of the composite material, 0.1 to 2 moles of imidazole groups are contained per gram of matrix, ensuring high ionic conductivity while maintaining the chemical stability and mechanical strength of the composite membrane.

[0037] Furthermore, by controlling the density of imidazole groups in the matrix of the composite material, 0.1 to 2 moles of imidazole groups are contained in each gram of matrix, the ionic conductivity and chemical stability of the membrane are optimized, ensuring its high efficiency in practical use. The prepared composite membrane has a dimensional change rate of less than 2% at an operating temperature of 80°C, and an ionic conductivity of 0.05S / cm to 0.15S / cm at 25°C, indicating that the composite membrane has excellent dimensional stability and ion conductivity, and is suitable for various ion exchange applications.

[0038] Specifically, the composite material refers to a cross-linked matrix formed by imidazole-functionalized polyetheretherketone and polyvinyl alcohol through physical and chemical cross-linking. In this matrix, polyetheretherketone provides excellent chemical stability and mechanical properties, while polyvinyl alcohol enhances the structural strength and durability of the composite membrane through cross-linking. This composite matrix not only has high ion conductivity, but also maintains good performance stability under high temperature and strong alkaline environment.

[0039] A method for preparing an imidazole-functionalized composite anion exchange membrane comprises the following steps:

[0040] Step 1, dissolving trimethylhydroquinone monomer in a solvent, adding imidazole group monomer and initiator to carry out solution polymerization to form imidazole functionalized polyetheretherketone solution;

[0041] Step 2, dissolving polyvinyl alcohol in water, adding a cross-linking agent and mixing;

[0042] Step 3: adding polyetheretherketone solution and polyvinyl alcohol solution in a mass ratio of 1:1 to the metal organic framework for ultrasonic dispersion and high-speed stirring;

[0043] Step 4: Prepare a cross-linked composite membrane through solution casting and heat treatment process.

[0044] The solution polymerization reaction is carried out in the range of room temperature to 80°C, and the reaction time is 1 hour; the cross-linking agent is glutaraldehyde, the cross-linking reaction is carried out at room temperature, and the reaction time is 30 minutes; the ultrasonic dispersion time is 10 minutes, the high-speed stirring speed is 1000rpm, and the stirring time is 30 minutes; the solution casting step includes casting the mixed solution on a glass plate, the drying temperature is 50°C, the drying time is 2 hours, and then heat treatment is carried out in a vacuum drying oven, the heat treatment temperature is 80°C, and the heat treatment time is 2 hours.

[0045] In one embodiment, by introducing an imidazole group into the molecular structure of a trimethylhydroquinone monomer, and covalently connecting the imidazole group to the main chain of polyetheretherketone by a nucleophilic substitution reaction, an imidazole-functionalized polyetheretherketone with a multifunctional site is formed, providing excellent chemical stability and enhanced mechanical properties. Secondly, polyvinyl alcohol and imidazole-functionalized polyetheretherketone are chemically cross-linked by glutaraldehyde to form a stable cross-linked structure, and physical cross-linking is achieved by freeze-thaw method, further enhancing the structural strength and durability of the matrix. Thirdly, the metal organic framework is evenly dispersed in the composite matrix, and the ionic conductivity and thermal stability of the composite membrane are improved through its unique physical and chemical interactions. Finally, by controlling the density of imidazole groups in the composite matrix, 0.1 to 2 moles of imidazole groups are contained per gram of matrix, ensuring high ionic conductivity while maintaining the chemical stability and mechanical strength of the composite membrane.

[0046] Embodiment 2:

[0047] This embodiment provides a method for preparing an imidazole-functionalized composite anion exchange membrane, the steps are as follows:

[0048] step:

[0049] The trimethylhydroquinone monomer is dissolved in a solvent, and an imidazole group monomer and an initiator are added to perform solution polymerization to form an imidazole functionalized polyetheretherketone solution;

[0050] Polyvinyl alcohol was dissolved in water and glutaraldehyde was added for chemical cross-linking;

[0051] The imidazole-functionalized polyetheretherketone solution and the cross-linked polyvinyl alcohol solution were mixed in a mass ratio of 1:2, and the metal organic framework was added for ultrasonic dispersion and high-speed stirring;

[0052] The mixed solution was cast on a glass plate, dried at 50 °C for 2 h, and then heat treated in a vacuum drying oven at 100 °C for 4 h to prepare a cross-linked composite membrane.

[0053] The solution polymerization reaction is carried out in the range of room temperature to 60°C, and the reaction time is 2 hours; the cross-linking reaction is carried out at room temperature, and the reaction time is 1 hour; the ultrasonic dispersion time is 15 minutes, the high-speed stirring speed is 2000rpm, and the stirring time is 45 minutes.

[0054] Embodiment three:

[0055] This embodiment provides a method for preparing an imidazole-functionalized composite anion exchange membrane, the steps are as follows:

[0056] The trimethylhydroquinone monomer is dissolved in a solvent, and an imidazole group monomer and an initiator are added to perform solution polymerization to form an imidazole functionalized polyetheretherketone solution;

[0057] Dissolve polyvinyl alcohol in water and add ethylene dichloride for chemical cross-linking;

[0058] The imidazole-functionalized polyetheretherketone solution and the cross-linked polyvinyl alcohol solution were mixed in a mass ratio of 1:3, and the metal organic framework was added for ultrasonic dispersion and high-speed stirring;

[0059] The mixed solution was cast on a glass plate, dried at 70 °C for 3 h, and then heat treated in a vacuum drying oven at 120 °C for 6 h to prepare a cross-linked composite membrane.

[0060] The solution polymerization reaction is carried out in the range of room temperature to 80°C, and the reaction time is 1.5 hours; the cross-linking reaction is carried out at room temperature, and the reaction time is 2 hours; the ultrasonic dispersion time is 20 minutes, the high-speed stirring speed is 1500rpm, and the stirring time is 60 minutes.

[0061] Embodiment 4:

[0062] This embodiment provides a method for preparing an imidazole-functionalized composite anion exchange membrane, the steps are as follows:

[0063] The trimethylhydroquinone monomer is dissolved in a solvent, and an imidazole group monomer and an initiator are added to perform solution polymerization to form an imidazole functionalized polyetheretherketone solution;

[0064] Dissolve polyvinyl alcohol in water and add epichlorohydrin for chemical cross-linking;

[0065] The imidazole-functionalized polyetheretherketone solution and the cross-linked polyvinyl alcohol solution were mixed in a mass ratio of 1:4, and the metal organic framework was added for ultrasonic dispersion and high-speed stirring;

[0066] The mixed solution was cast on a glass plate, dried at 60 °C for 2.5 h, and then heat treated in a vacuum drying oven at 90 °C for 4 h to prepare a cross-linked composite membrane.

[0067] The solution polymerization reaction is carried out in the range of room temperature to 75°C, and the reaction time is 1 hour; the cross-linking reaction is carried out at room temperature, and the reaction time is 45 minutes; the ultrasonic dispersion time is 12 minutes, the high-speed stirring speed is 1200rpm, and the stirring time is 40 minutes.

[0068] Table 1 Experimental data table of embodiment

[0069]

[0070] Through the comparison of experimental data, Example 1 is superior to other examples in various performance parameters, showing higher ion conductivity (0.12S / cm), lower dimensional change rate (1.5%), and higher tensile strength (65MPa). In addition, Example 1 achieves excellent membrane performance at a lower heat treatment temperature (80°C) and a shorter heat treatment time (2 hours). These results show that Example 1 performs well in ion conductivity, dimensional stability and mechanical strength, and is the optimal implementation scheme, suitable for a variety of ion exchange application scenarios.

[0071] Comparative Example 1:

[0072] This embodiment provides a solution casting film preparation method, comprising the following steps:

[0073] Preparation of solution: dissolving a certain amount of imidazole compound in organic solvent N-methylpyrrolidone to obtain a uniform solution.

[0074] Introducing composite materials: Add a certain amount of inorganic filler titanium dioxide nanoparticles and polymer material polyvinylidene fluoride into the solution and stir until evenly dispersed.

[0075] Casting film: The solution is evenly coated on a smooth glass plate or stainless steel plate to form a uniform film layer.

[0076] Solvent evaporation: Allow the solvent to evaporate gradually at room temperature or under heating conditions to form a solid composite film.

[0077] Post-treatment: The prepared membrane is heat treated at a certain temperature to enhance the mechanical strength and stability of the membrane.

[0078] Comparative Example 2:

[0079] This embodiment provides a preparation method by in-situ polymerization, comprising the following steps:

[0080] Monomer mixing: Mix the imidazole monomer with other monomers such as acrylic acid, and add an appropriate amount of initiator potassium persulfate.

[0081] Introducing filler: Add inorganic filler montmorillonite into the mixture and stir evenly.

[0082] Polymerization: The mixture is placed at an appropriate temperature for in-situ polymerization to form a cross-linked polymer network.

[0083] Film casting: Evenly coat the polymer solution on a smooth substrate and wait for it to form a film.

[0084] Solvent removal: The solvent is removed at an appropriate temperature to obtain a solid composite membrane.

[0085] Comparative Example 3:

[0086] This embodiment provides a method using a sol-gel method, comprising the following steps:

[0087] Preparation of sol: dissolve the imidazole compound in a suitable solvent, add the sol-gel precursor tetraethoxysilane and a suitable amount of water, carry out hydrolysis and polycondensation reaction to form a sol.

[0088] Introducing fillers: Add inorganic filler sodium silicate and polymer material polyvinyl alcohol into the sol and stir evenly.

[0089] Film casting: The sol is evenly coated on the substrate to form a uniform film layer.

[0090] Gelation: Gelation treatment is carried out at an appropriate temperature to transform the sol into a gel film.

[0091] Drying and heat treatment: The gel film is dried and heat treated to remove residual solvent and improve the mechanical properties and thermal stability of the film.

[0092] Table 2 Comparative Example Experimental Data Table

[0093]

[0094] The imidazole functionalized composite anion exchange membrane of Example 1 shows significant advantages in multiple performance parameters, especially in chemical stability, mechanical properties, structural strength, thermal stability and conductivity stability. In addition, its dimensional change rate at operating temperature is less than 2%, the ion conductivity at 25°C reaches 0.05-0.15S / cm, the water swelling rate is 5%, the water absorption rate is 10%, the elongation at break is 50%, and the thermal expansion coefficient is 20ppm / °C, indicating that it has excellent overall performance and is suitable for various ion exchange applications. Therefore, the preparation method of Example 1 not only optimizes the ion conductivity and chemical stability of the membrane, but also ensures its high efficiency in actual use.

[0095] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An imidazole-functionalized composite anion exchange membrane, characterized in that: Includes the following ingredients: Trimethylhydroquinone monomer, imidazole functionalized polyetheretherketone prepared by solution polymerization, wherein the imidazole group is covalently linked to the main chain of polyetheretherketone to form a multifunctional site, which makes polyetheretherketone have excellent chemical stability and mechanical properties; Polyvinyl alcohol, together with imidazole-functionalized polyetheretherketone, forms a cross-linked matrix through physical and chemical cross-linking, which enhances the structural strength and durability of the composite film; Metal-organic frameworks, as inorganic fillers, are uniformly dispersed in the composite matrix and enhance the ionic conductivity and thermal stability of the composite membrane through physical and chemical interactions.

2. The imidazole-functionalized composite anion exchange membrane according to claim 1, characterized in that: The molecular structure of the trimethylhydroquinone monomer contains at least one imidazole group, which is connected to the polyetheretherketone main chain through a nucleophilic substitution reaction. The composite of polyvinyl alcohol and imidazole-functionalized polyetheretherketone is chemically cross-linked by glutaraldehyde, and physical cross-linking is achieved by freeze-thaw method.

3. The imidazole-functionalized composite anion exchange membrane according to claim 1, characterized in that: The particle size of the metal organic framework is 20 nanometers to 200 nanometers, and is dispersed in the composite material matrix with a mass fraction of 1% to 20%.

4. The imidazole-functionalized composite anion exchange membrane according to claim 1, characterized in that: The density of imidazole groups in the composite matrix is ​​0.1 to 2 moles of imidazole groups per gram of the composite matrix.

5. The imidazole-functionalized composite anion exchange membrane according to claim 1, characterized in that: The composite membrane has a dimensional change rate of less than 2% at an operating temperature of 80° C., and an ionic conductivity of the composite membrane at 25° C. of 0.05 S / cm to 0.15 S / cm.

6. A method for preparing an imidazole-functionalized composite anion exchange membrane, according to an imidazole-functionalized composite anion exchange membrane according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1, dissolving trimethylhydroquinone monomer in a solvent, adding imidazole group monomer and initiator to carry out solution polymerization to form imidazole functionalized polyetheretherketone solution; Step 2, dissolving polyvinyl alcohol in water, adding a cross-linking agent and mixing; Step 3: mixing the polyetheretherketone solution and the polyvinyl alcohol solution in a mass ratio of 1:1 to 1:5, adding the metal organic framework for ultrasonic dispersion and high-speed stirring; Step 4: Prepare a cross-linked composite membrane through solution casting and heat treatment process.

7. The method for preparing an imidazole-functionalized composite anion exchange membrane according to claim 6, characterized in that: The solution polymerization reaction is carried out in a range of room temperature to 80° C., and the reaction time is 1 hour to 24 hours.

8. The method for preparing an imidazole-functionalized composite anion exchange membrane according to claim 6, characterized in that: The cross-linking agent is glutaraldehyde, and the cross-linking reaction is carried out at room temperature for a reaction time of 30 minutes to 6 hours.

9. The method for preparing an imidazole-functionalized composite anion exchange membrane according to claim 6, characterized in that: The ultrasonic dispersion time is 10 minutes to 60 minutes, the high-speed stirring speed is 1000 rpm to 5000 rpm, and the stirring time is 30 minutes to 120 minutes.

10. The method for preparing an imidazole-functionalized composite anion exchange membrane according to claim 6, characterized in that: The solution casting step comprises casting the mixed solution on a glass plate, drying at a temperature of 50° C. to 100° C. for a drying time of 2 to 24 hours, and then heat treating the mixed solution in a vacuum drying oven at a temperature of 80° C. to 150° C. for a heat treatment time of 2 to 12 hours.