Silk fibroin microsphere with surface microporous structure as well as preparation method and application of silk fibroin microsphere
By spraying into liquid nitrogen and heating and annealing, silk fibroin microspheres based on an aqueous solution system are prepared, which solves the problems of biocompatibility and degradation rate in the existing technology and achieves water stability and rapid degradation of silk fibroin. Protein microspheres for a variety of biomedical applications.
Patent Information
- Application Number
- CN202410734854.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-07
AI Technical Summary
In the existing technology, the use of organic solvents in the preparation process of silk fibroin microspheres results in reduced biocompatibility, slow degradation rate, and lack of microspheres with rapid degradation and microporous structure.
Silk fibroin microspheres with surface microporous structure are prepared by spraying into liquid nitrogen to form microspheres, and through temperature annealing treatment, combined with freeze-drying or direct thawing, which is completely based on an aqueous solution system and does not require chemical reagents.
Silk fibroin microspheres have achieved water stability and rapid biodegradation, a porous surface structure and a high internal specific surface area, making them suitable for cell expansion, drug carriers and hemostatic powders.
Smart Images

Figure CN118772477A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biomaterials, and in particular to a silk fibroin microsphere with a surface microporous structure and a preparation method and application thereof. Background Art
[0002] Silk fibroin is a natural protein extracted from silkworm cocoons. In recent years, silk fibroin has attracted increasing attention in many biomedical applications such as drug delivery, tissue engineering or cell carriers due to its biocompatibility, biodegradability and ability to stabilize other biomolecules. Currently, the preparation of silk fibroin microspheres has been widely adopted by emulsification solvent evaporation method, phase separation method, high voltage electrostatic method and spray drying method.
[0003] Since the regenerated silk fibroin is water-soluble, in order to improve the water stability of silk fibroin microspheres, it is usually necessary to use organic solvents such as methanol and ethanol to induce the formation of β-sheet to obtain a stable silk II structure. However, the use of organic solvents will reduce the biocompatibility of the material and may even cause drug denaturation and changes in the morphology of the microspheres. Secondly, the surface of silk II silk fibroin microspheres induced by organic solvents such as ethanol is usually a dense structure, which limits the scope of use of silk fibroin microspheres. In addition, silk II microspheres contain a large amount of β-sheet structure, which slows the biodegradation rate of the material.
[0004] In the prior art, the patent with publication number CN108553690B provides a strontium-doped porous silk microsphere and a preparation method thereof. The patent provides a strontium-doped silk fibroin-based porous microsphere prepared by an emulsion method combined with freeze-drying technology using silk fibroin and strontium chloride as the main materials. The patent pours a mixed solution of silk fibroin and strontium chloride into a pre-cooled petroleum ether solution with an emulsifier added, and then places it in a freezing environment for static precipitation; and removes petroleum ether in a freezing atmosphere to obtain strontium-doped silk fibroin microspheres containing ice crystals, freezes the silk fibroin microspheres, and then freeze-dries to obtain dry strontium-doped silk fibroin microspheres. Finally, it is treated with alcohol to make it insoluble in water. The microspheres are prepared by an emulsification method, and alcohol is used to induce silk fibroin to transform into a silk II crystalline structure. The residual organic solvent will greatly reduce the biocompatibility of the material, and the degradation rate of silk II material is slow, which may affect the effective utilization rate of the drug.
[0005] In the prior art, the patent with publication number CN 106637969 B provides a tussah silk fibroin microsphere containing a three-dimensional pore structure and a preparation method thereof. The patent adds a foaming agent and a cross-linking agent to a tussah silk fibroin solution, stands, stirs, and centrifuges to form tussah silk fibroin particles; adds the tussah silk fibroin particles to a sodium chloride solution, heats and stirs, centrifuges to precipitate, washes with ethanol, takes out, dries, and then places it in a low-temperature freeze-drying process to obtain tussah silk fibroin microspheres with a three-dimensional pore structure. The method obtains a pore structure by adding a foaming agent and a cross-linking agent, and uses ethanol treatment to make the silk fibroin microspheres water-stable. However, the use of organic solvents and cross-linking agents greatly reduces the biocompatibility of the material and affects the degradation rate of the silk fibroin microspheres. In addition, there is a document (Materials, 2018, 11 (8): 1280.) reporting the addition of glycerol to a silk fibroin solution and the preparation of porous silk fibroin microspheres by electrostatic differentiation. Although the silk microspheres prepared in this article are also water-stable, this method adds glycerol to the silk solution in the initial stage, so that the obtained microspheres have a silk II structure and are rich in a large amount of β-sheet, resulting in a slow degradation rate of the silk microspheres. At the same time, the presence of glycerol limits its application.
[0006] In view of this, it is necessary to design a silk microsphere with a microporous structure, rapid degradation, no need for other chemical reagents in the preparation process, and water stability to solve the above problems. Summary of the invention
[0007] In view of the defects of the above-mentioned prior art, the object of the present invention is to provide a silk fibroin microsphere with a surface microporous structure and a preparation method and application thereof. The preparation method does not need to add chemical reagents, and the prepared microsphere has a large number of porous structures on the surface and a nanoscale hierarchical structure inside, has water stability, and can be rapidly biodegraded. The prepared silk fibroin microsphere can be added with other polymer substances and small molecule drugs. Because the silk fibroin microsphere has the advantages of green preparation, a large number of micropores on the surface, a high internal specific surface area, and rapid degradability, it can be applied to the fields of cell expansion, hemostatic powder, cell microscaffold, drug carrier, etc.
[0008] To achieve the above object, the present invention provides a method for preparing silk fibroin microspheres with surface microporous structure, comprising the following steps:
[0009] S1. Prepare silk fibroin solution for later use;
[0010] S21, spraying the silk fibroin solution obtained in step S1 into liquid nitrogen to form microspheres; then subjecting the microspheres to a temperature-raising annealing treatment, and finally freeze-drying or directly thawing, to obtain silk fibroin microspheres having a surface microporous structure; or
[0011] S22, mixing the silk fibroin solution obtained in step S1 with a water-soluble polymer solution to obtain a mixed solution, and then spraying the mixed solution into liquid nitrogen to form microspheres; then subjecting the microspheres to a temperature-raising annealing treatment, and finally freeze-drying or directly thawing, to obtain silk fibroin microspheres with a surface microporous structure.
[0012] Furthermore, in steps S21 and S22, the spraying method is electrostatic differentiation, ultrasonic atomization, high-pressure airflow spray or microfluidics technology, etc.
[0013] Furthermore, the temperature-raising annealing treatment refers to freezing the microspheres taken out from liquid nitrogen at a temperature of -20°C to 0°C for 12h to 96h. The thawing includes melting at a temperature of 4 to 60°C.
[0014] Furthermore, the freeze drying refers to drying under reduced pressure at -50°C.
[0015] Furthermore, in steps S21 and S22, the mass percentage of the silk fibroin solution is 0.05-20wt%.
[0016] Furthermore, in step S22, the concentration of the water-soluble polymer solution is 0.05-5.0 wt%; the water-soluble polymer is one or more of hyaluronic acid and its sodium salt, alginate, gelatin, chondroitin sulfate, cellulose derivatives, starch and its derivatives.
[0017] Furthermore, in step S22, the amount of the water-soluble polymer is 1-50% of the quality of the silk.
[0018] Furthermore, in step S1, the silk fibroin solution is a regenerated silk fibroin solution obtained by degumming, dissolving and dialysis of silk or silk cocoons. The silk or silk cocoons are derived from mulberry silkworms and tussah silkworms.
[0019] Furthermore, the silk microspheres obtained after freeze-drying or direct thawing can be further screened to obtain silk microspheres with relatively uniform sizes; the mesh size used for screening is 15 to 40 meshes.
[0020] To achieve the above object, the present invention further provides a silk fibroin microsphere with a surface microporous structure, which is prepared by the preparation method described in any of the technical solutions in the aforementioned technical solutions.
[0021] The aforementioned silk fibroin microspheres with surface microporous structures can be used in the fields of cell expansion, drug carriers, cell microscaffolds, hemostatic powders, etc.
[0022] The beneficial effects of the present invention are:
[0023] 1. The method for preparing silk fibroin microspheres with a surface microporous structure provided by the present invention comprises spraying a silk fibroin solution or a mixture of a silk fibroin solution and a water-soluble polymer solution into liquid nitrogen to form microspheres, then performing annealing and crystallization by heating, and finally directly thawing or freeze-drying to form silk fibroin microspheres with a water-stable silk I structure. The present invention provides a method completely based on an aqueous solution system without the use of chemical additives or organic solvents.
[0024] 2. The silk fibroin microspheres prepared by the present invention have micron-scale macropores on the surface and nanoscale hierarchical structures inside, and have water stability; and compared with silk II silk fibroin microspheres, the silk fibroin microspheres prepared by the present invention can achieve rapid biodegradation.
[0025] 3. The silk fibroin microspheres prepared by the present invention can be added with other polymer substances and small molecule drugs. Based on the advantages of green preparation, a large number of micropores on the surface, high internal specific surface area, and rapid degradability, the silk fibroin microspheres can be applied to the fields of cell expansion, drug carriers, cell microscaffolds, hemostatic powders, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is an electron microscope morphology image of the silk I silk fibroin microspheres with a surface microporous structure provided in Example 1 at a scale of 500 μm.
[0027] Figure 2 This is an electron microscope morphology image of the silk I silk fibroin microspheres with surface microporous structure provided in Example 1 at a scale of 150 μm. The image shows that the microspheres have a nanoscale hierarchical structure inside.
[0028] Figure 3 This is an electron microscope morphology image of the material provided for Comparative Example 1 at a scale of 150 μm.
[0029] Figure 4 These are actual pictures of the stability of the materials provided in Example 1 and Comparative Example 1 in water; wherein a is a actual picture of Example 1, and b is a actual picture of Comparative Example 1.
[0030] Figure 5 The electron microscope morphology of the silk fibroin microspheres with a silk II structure obtained by ethanol treatment provided in Comparative Example 2 at a scale of 100 μm shows that there is no microporous structure on the surface of the microspheres.
[0031] Figure 6 The XRD curves of the silk microspheres provided in Example 1 and Comparative Example 2.
[0032] Figure 7The degradation curves of the silk fibroin microspheres provided in Example 1 and Comparative Example 2 after 14 days of degradation.
[0033] Figure 8 These are morphological images of the endothelial cells provided in Example 1 proliferating on the microporous silk I microspheres for one day and seven days under a laser confocal microscope at a magnification of 200 times.
[0034] Fig. 9 This is a quantitative schematic diagram of the proliferation of endothelial cells on the microporous silk microspheres provided in Example 1 using CCK-8.
[0035] Fig.10 This is an electron microscope morphology image of the material provided for Comparative Example 3 at a scale of 1 μm. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0037] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0038] The present invention provides a method for preparing silk fibroin microspheres with a surface microporous structure, comprising the following steps:
[0039] S1. Prepare silk fibroin solution for later use;
[0040] S21, spraying the silk fibroin solution obtained in step S1 into liquid nitrogen to form microspheres; then subjecting the microspheres to a temperature-raising annealing treatment, and finally freeze-drying or directly thawing, to obtain silk fibroin microspheres having a surface microporous structure; or
[0041] S22, mixing the silk fibroin solution obtained in step S1 with a water-soluble polymer solution to obtain a mixed solution, and then spraying the mixed solution into liquid nitrogen to form microspheres; then subjecting the microspheres to a temperature-raising annealing treatment, and finally freeze-drying or directly thawing, to obtain silk fibroin microspheres with a surface microporous structure.
[0042] In step S1, the fibroin solution is a regenerated fibroin solution obtained by degumming, dissolving and dialysis of silk or silk cocoons. The silk or silk cocoons are derived from mulberry silkworms and tussah silkworms. In steps S21 and S22, the mass percentage of the fibroin solution is 0.05 to 20 wt%.
[0043] In steps S21 and S22, the spraying method is electrostatic differentiation, ultrasonic atomization, high-pressure airflow spray or microfluidics technology.
[0044] The temperature-raising annealing treatment refers to freezing the microspheres taken out from liquid nitrogen at a temperature of -20°C to 0°C for 12h to 96h. The thawing includes melting at a temperature of 4 to 60°C.
[0045] The freeze drying refers to drying under reduced pressure at -50°C.
[0046] In step S22, the concentration of the water-soluble polymer solution is 0.05-5.0 wt%; the water-soluble polymer is one or more of hyaluronic acid and its sodium salt, alginate, gelatin, chondroitin sulfate, cellulose derivatives, starch and its derivatives.
[0047] In step S22, the amount of the water-soluble polymer used is 1-50% of the quality of the silk.
[0048] Furthermore, the silk microspheres obtained after freeze-drying or direct thawing can be further screened to obtain silk microspheres with relatively uniform sizes; the mesh size used for screening is 15 to 40 meshes.
[0049] The preparation method of the silk fibroin microspheres with surface microporous structure provided by the present invention is described below with reference to specific embodiments.
[0050] Example 1
[0051] This embodiment provides a method for preparing silk fibroin microspheres with a surface microporous structure, comprising the following steps:
[0052] S1. Prepare silk fibroin solution for later use;
[0053] Specifically, the following process can be used: immerse 100g of mulberry silk in 5L of 0.1% sodium carbonate solution, boil at 98-100℃ for 30min, repeat three times to degumming the cocoons, and obtain pure silk fiber after thorough washing and drying. Immerse the treated silk fiber in 9.3M lithium bromide solution and dissolve at 60℃ for one hour. After cooling, pour the dissolved solution into a dialysis bag with a molecular weight cutoff of 9-14kDa and dialyze with deionized water. After the dialysis, filter with gauze to obtain a silk solution, and determine its concentration by the dry mass method. In order to obtain a solution with a higher concentration, the silk solution contained in the dialysis membrane is placed in a PEG solution, and the silk solution is reverse dialyzed. Pour the prepared silk protein solution into a centrifuge tube, remove aggregates and bubbles by centrifugation, and store it in a 4℃ refrigerator for later use;
[0054] S2, diluting the silk protein solution to 1% by mass, spraying the solution into liquid nitrogen by electrostatic differentiation to obtain microspheres; then transferring the microspheres to a -4°C refrigerator for annealing for 48 hours to induce the transformation of their crystalline structure. Finally, freeze drying (i.e., drying under reduced pressure at -50°C for 48 hours) is performed to obtain silk I silk microspheres with a surface microporous structure; then screening is performed by sieving with 18-mesh and 25-mesh sample sieves in turn to obtain silk I silk microspheres with a surface microporous structure of relatively uniform size.
[0055] The final prepared silk I silk fibroin microspheres with surface microporous structure have scanning electron microscope morphology images with scales of 500 μm and 150 μm, respectively. Figure 1 and Figure 2 As shown, compared with silk II microspheres, the microspheres have a large number of porous structures on the surface and nanoscale hierarchical structures inside, which can provide a better three-dimensional growth environment for subsequent cell growth.
[0056] The stability in water (immersed in water for 14 days) test results are as follows Figure 4 As shown in a, it can be seen that the microspheres can still maintain their shape in water and will not dissolve after being immersed in water for 14 days.
[0057] After endothelial cells were placed on the silk I microspheres with a microporous structure obtained in step S2 and proliferated for one day, the state of the cells under a laser confocal microscope was as follows: Figure 8 As shown in a, the results show that the cells are growing well (green represents the cytoskeleton, and the more green, the better the cell growth). After the endothelial cells proliferated on the silk I microspheres with a multi-porous structure for seven days, the state under the laser confocal microscope is as follows Figure 8 As shown in middle b, the results show that as time goes by, the cell growth remains in a good condition.
[0058] In addition, the proliferation of endothelial cells on the microspheres prepared in Example 1 was statistically analyzed. Fig. 9 As shown. It can be seen that the proliferation of endothelial cells on the silk I microspheres with a microporous structure prepared in Example 1 is as follows: the proliferation of endothelial cells on days 1, 3, and 7 is relatively stable and grows steadily, further confirming that the silk I microspheres with a microporous structure prepared in Example 1 can be used as an excellent carrier for cell growth and proliferation.
[0059] Example 2
[0060] The only difference between Example 2 and Example 1 is that in step S2, the microspheres after the temperature-raising annealing treatment are placed at room temperature 25°C for thawing to obtain a silk microsphere suspension with good dispersibility. The rest is substantially the same as Example 1 and will not be described again.
[0061] Example 3
[0062] The only difference between Example 3 and Example 1 is that in step S2, the microspheres are subjected to annealing treatment at a high temperature for 72 hours. The rest is substantially the same as Example 1 and will not be described in detail here.
[0063] Example 4
[0064] The only difference between Example 4 and Example 1 is that in step S2, the silk fibroin solution is sprayed into liquid nitrogen by ultrasonic atomization to obtain microspheres. The rest is substantially the same as Example 1 and will not be described again.
[0065] Embodiment 5-7
[0066] The difference between Example 5-7 and Example 1 is that the mass fraction of the silk fibroin solution in step S2 is changed, and the other parts are substantially the same as Example 1, which will not be described in detail here. The mass fractions of the silk fibroin solution in Examples 5-7 are shown in the following table.
[0067] project Mass fraction of silk fibroin solution Example 1 1wt% Example 5 0.05wt% Example 6 10wt% Example 7 20wt%
[0068] Example 8
[0069] The main difference between Example 8 and Example 1 is that the solvent system for preparing the silk fibroin solution is different, as follows:
[0070] S1. Prepare silk fibroin solution for later use;
[0071] Specifically, the following process can be used: 100g of mulberry silk is immersed in 5L of 0.1% sodium carbonate solution, boiled at 98-100℃ for 30min, repeated three times, the cocoons are degummed, and pure silk fibers are obtained after thorough washing and drying. The treated silk fibers are immersed in a ternary solution of CaCl2 / CH3CH2OH / H2O with a molar ratio of 1:2:8, and dissolved at 72℃ for one hour. After cooling, the dissolved solution is poured into a dialysis bag with a molecular weight cutoff of 9-14kDa and dialyzed with deionized water. After the dialysis, the silk solution is obtained by filtering with gauze, and its concentration is determined by the dry mass method. In order to obtain a solution with a higher concentration, the silk solution contained in the dialysis membrane is placed in a PEG solution, and the silk solution is reverse dialyzed. The prepared silk protein solution is poured into a centrifuge tube, the aggregates and bubbles are removed by centrifugation, and it is stored in a refrigerator at 4℃ for standby use;
[0072] S2 is substantially the same as step S2 of embodiment 1 and will not be described in detail here.
[0073] Example 9
[0074] The only difference between Example 9 and Example 8 is that in step S2, the microspheres after the temperature-raising annealing treatment are placed at room temperature 25°C for thawing to obtain a silk microsphere suspension with good dispersibility. The rest is substantially the same as Example 8 and will not be described again.
[0075] Example 10
[0076] The only difference between Example 10 and Example 8 is that in step S2, the microspheres are subjected to annealing treatment at a high temperature for 72 hours. The rest is substantially the same as Example 8 and will not be described in detail here.
[0077] Examples 11-13
[0078] The difference between Example 11-13 and Example 8 is that the mass fraction of the silk fibroin solution in step S2 is changed, and the other parts are substantially the same as Example 8, which will not be described in detail here. The mass fractions of the silk fibroin solution in Examples 11-13 are shown in the following table.
[0079] project Mass fraction of silk fibroin solution Example 8 1wt% Embodiment 11 0.05wt% Example 12 10wt% Embodiment 13 20wt%
[0080] Embodiment 14
[0081] The main difference between Example 14 and Example 1 is that the sources of silk cocoons for preparing the silk fibroin solution are different, specifically, tussah silkworm cocoons are used in step S1. The rest is roughly the same as Example 1 and will not be repeated here.
[0082] Embodiment 15
[0083] The only difference between Example 15 and Example 14 is that in step S2, the silk fibroin solution is sprayed into liquid nitrogen by ultrasonic atomization to obtain microspheres. The rest is substantially the same as Example 14 and will not be described again.
[0084] Example 16
[0085] The only difference between Example 16 and Example 14 is that in step S2, the microspheres are subjected to annealing treatment at a high temperature for 72 hours. The rest is substantially the same as Example 14 and will not be described again.
[0086] Examples 17-19
[0087] The difference between Examples 17-19 and Example 14 is that the mass fraction of the silk fibroin solution in step S2 is changed, and the other parts are substantially the same as Example 14, which will not be described again. The mass fractions of the silk fibroin solution in Examples 17-19 are shown in the following table.
[0088] project Mass fraction of silk fibroin solution Embodiment 14 1wt% Embodiment 17 0.05wt% Embodiment 18 10wt% Embodiment 19 20wt%
[0089] Embodiment 20
[0090] The main difference between Example 20 and Example 14 is that the solvent system for preparing the silk fibroin solution is different, as follows:
[0091] S1. Prepare silk fibroin solution for later use;
[0092] Specifically, the following process can be used: 100g of tussah silkworm cocoons are immersed in 5L of 0.1% sodium carbonate solution, boiled at 98-100°C for 30min, repeated three times, the cocoons are degummed, and pure silk fibers are obtained after being fully washed and dried. The treated silk fibers are immersed in a ternary solution of CaCl2 / CH3CH2OH / H2O with a molar ratio of 1:2:8, and dissolved at 72°C for one hour. After cooling, the dissolved solution is poured into a dialysis bag with a molecular weight cutoff of 9-14kDa and dialyzed with deionized water. After the dialysis is completed, the silk solution is obtained by filtering with gauze, placed in a 4°C refrigerator for storage, and its concentration is determined by the dry mass method. The prepared silk protein solution is poured into a centrifuge tube and centrifuged to remove aggregates and bubbles.
[0093] S2 is substantially the same as step S2 of Example 14 and will not be described in detail here.
[0094] Embodiment 21
[0095] The only difference between Example 21 and Example 20 is that in step 2, the silk fibroin solution is sprayed into liquid nitrogen by ultrasonic atomization to obtain microspheres. The rest is basically the same as Example 20 and will not be repeated here.
[0096] Embodiment 22
[0097] The only difference between Example 22 and Example 21 is that in step 2, the microspheres are subjected to annealing treatment at a high temperature for 72 hours. The rest is substantially the same as Example 21 and will not be described herein.
[0098] Embodiment 23-25
[0099] The difference between Examples 23-25 and Example 20 is that the mass fraction of the silk fibroin solution in step S2 is changed, and the other parts are substantially the same as Example 20, which will not be described in detail here. The mass fractions of the silk fibroin solution in Examples 23-25 are shown in the following table.
[0100] project Mass fraction of silk fibroin solution Embodiment 20 1wt% Embodiment 23 0.05wt% Embodiment 24 10wt% Embodiment 25 20wt%
[0101] Embodiment 26
[0102] This embodiment provides a method for preparing a silk-based composite microsphere having a surface microporous structure, comprising the following steps:
[0103] S1 is the same as step S1 in Example 1 and will not be described in detail here;
[0104] S2, adding hyaluronic acid solution (the content of hyaluronic acid accounts for 1% of the mass of silk protein) to the solution in step S1, and stirring thoroughly to obtain a reaction solution; the reaction solution is subjected to electrostatic differentiation in liquid nitrogen to obtain microspheres; then the microspheres are transferred to a -4°C refrigerator for annealing treatment for 48 hours to induce the transformation of their crystalline structure. Finally, freeze drying (i.e., drying under reduced pressure at -50°C for 48 hours) is performed to obtain silk I silk-based composite microspheres with a microporous structure.
[0105] Embodiment 27
[0106] The difference between Example 27-28 and Example 26 is that the mass fraction of the silk fibroin solution in step S2, the type of water-soluble polymer, and the percentage of the amount of the water-soluble polymer to the silk mass are changed, as shown in the following table. The rest is substantially the same as Example 26 and will not be repeated here.
[0107]
[0108] The water-soluble polymer may also be one or more of chondroitin sulfate, cellulose derivatives, starch and derivatives thereof.
[0109] Experiments show that Examples 2-28 can all produce silk fibroin microspheres with surface microporous structures.
[0110] Comparative Example 1
[0111] The difference between Comparative Example 1 and Example 1 is that the silk fibroin solution is placed in liquid nitrogen, instead of being sprayed into liquid nitrogen by electrostatic differentiation, and no temperature rise annealing treatment is performed. The details are as follows:
[0112] S1 is the same as step S1 in Example 1 and will not be described in detail here;
[0113] S2. Dilute the silk fibroin solution obtained in step S1 to a mass percentage of 1%, and then freeze the silk fibroin solution under liquid nitrogen conditions, followed by freeze drying (ie, drying under reduced pressure at -50°C for 48 hours).
[0114] The final prepared material has a scanning electron microscope morphology with a scale of 300 μm. Figure 3 As shown. It can be seen that this method cannot obtain silk microspheres with surface microporous structure, which is a porous sponge; the stability in water (immersed in water for 5 minutes) test results are as follows Figure 4As shown in b, it can be seen that the material will dissolve immediately in water and cannot maintain its shape.
[0115] Comparative Example 2
[0116] The difference between Comparative Example 2 and Example 1 is that no temperature rise annealing treatment is performed.
[0117] S1 is the same as step S1 in Example 1 and will not be described in detail here;
[0118] S2, diluting the solution to 1%, obtaining microspheres in liquid nitrogen by electrostatic differentiation; then freeze-drying the microspheres (i.e., drying under reduced pressure at -50°C for 48 hours), treating the dried silk microspheres with 75% ethanol for 2 hours, and then freeze-drying again to obtain silk microspheres with silk II structure. Finally, sieving with 18-mesh and 25-mesh sieves in turn to obtain silk II silk microspheres with relatively uniform size.
[0119] The final prepared silk II silk microspheres have a scanning electron microscope morphology with a scale of 100 μm. Figure 5 As shown, it can be seen that the material surface is dense and has a non-porous structure.
[0120] Figure 6 The XRD curves of the silk microspheres provided by Example 1 and Comparative Example 2. It can be seen that the material obtained by Example 1 is a silk I structure, and the material obtained by Comparative Example 2 is a silk II structure.
[0121] Figure 7 The degradation curves of the silk fibroin microspheres provided in Example 1 and Comparative Example 2 for 14 days are shown. It can be seen that the material obtained in Example 1 degraded by about 80% in 14 days, while the material obtained in Comparative Example 2 only degraded by about 30%, which further proves that the material prepared by the method provided by this patent can achieve rapid degradation.
[0122] Comparative Example 3
[0123] The difference between Comparative Example 3 and Example 1 is that the silk fibroin solution is placed in liquid nitrogen instead of being sprayed into the liquid nitrogen by electrostatic differentiation.
[0124] S1 is the same as step S1 in Example 1 and will not be described in detail here;
[0125] S2, diluting the silk fibroin solution obtained in step S1 to a mass percentage of 1%, then freezing the silk fibroin solution under liquid nitrogen conditions, then transferring it to a -4°C refrigerator for annealing treatment for 48 hours, and finally freeze-drying it (i.e., drying it under reduced pressure at -50°C for 48 hours). The scanning electron microscope morphology of the final prepared material with a scale of 1 μm is shown as follows: Fig.10 As shown, it can be seen that this method cannot prepare silk microspheres with surface microporous structure.
[0126] In summary, the present invention provides a silk I silk fibroin microsphere with a microporous structure and a preparation method and application thereof. The silk I silk fibroin microsphere with water stability obtained by the method is completely based on an aqueous solution system, without the need for any chemical reagent addition and post-treatment. In addition, the microsphere surface has a large number of porous structures and an internal nanoscale hierarchical structure, which can be rapidly biodegraded. In addition, other polymer substances and small molecule drugs can be added to the silk fibroin microsphere. Because the silk fibroin microsphere has the advantages of green preparation, a large number of micropores on the surface, a high internal specific surface area, and rapid degradability, it can be applied to the fields of cell amplification, drug carriers, cell microscaffolds, hemostatic powders, etc.
[0127] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing silk fibroin microspheres having a surface microporous structure, characterized in that: The following steps are involved: S1. Prepare silk fibroin solution for later use; S21, spraying the silk fibroin solution obtained in step S1 into liquid nitrogen to form microspheres; then subjecting the microspheres to a temperature-raising annealing treatment, and finally freeze-drying or directly thawing, to obtain silk fibroin microspheres having a surface microporous structure; or S22, mixing the silk fibroin solution obtained in step S1 with a water-soluble polymer solution to obtain a mixed solution, and then spraying the mixed solution into liquid nitrogen to form microspheres; then subjecting the microspheres to a temperature-raising annealing treatment, and finally freeze-drying or directly thawing, to obtain silk fibroin microspheres with a surface microporous structure.
2. The method for preparing silk fibroin microspheres having a surface microporous structure according to claim 1, characterized in that: In steps S21 and S22, the spraying method is electrostatic differentiation, ultrasonic atomization, high-pressure airflow spray or microfluidics technology.
3. The method for preparing silk fibroin microspheres with surface microporous structure according to claim 1, characterized in that: The temperature-raising annealing treatment refers to freezing the microspheres taken out from liquid nitrogen at a temperature of -20°C to 0°C for 12h to 96h.
4. The method for preparing silk fibroin microspheres with surface microporous structure according to claim 1, characterized in that: The freeze drying refers to drying under reduced pressure at -50°C.
5. The method for preparing silk fibroin microspheres with surface microporous structure according to claim 1, characterized in that: In steps S21 and S22, the mass percentage of the silk fibroin solution is 0.05-20wt%.
6. The method for preparing silk fibroin microspheres with surface microporous structure according to claim 1, characterized in that: In step S22, the concentration of the water-soluble polymer solution is 0.05-5.0 wt%; the water-soluble polymer is one or more of hyaluronic acid and its sodium salt, alginate, gelatin, chondroitin sulfate, cellulose derivatives, starch and its derivatives.
7. The method for preparing silk fibroin microspheres with surface microporous structure according to claim 1, characterized in that: In step S22, the amount of the water-soluble polymer used is 1-50% of the quality of the silk.
8. The method for preparing silk fibroin microspheres with surface microporous structure according to claim 1, characterized in that: In step S1, the silk fibroin solution is a regenerated silk fibroin solution obtained by degumming, dissolving and dialysis of silk or silk cocoons.
9. A silk fibroin microsphere having a surface microporous structure, characterized in that: The silk fibroin microspheres with surface microporous structure are prepared according to the preparation method according to any one of claims 1 to 8.
10. Use of the silk fibroin microspheres with surface microporous structure obtained by the preparation method according to any one of claims 1 to 8 or the silk fibroin microspheres with surface microporous structure according to claim 9, characterized in that: The silk fibroin microspheres with surface microporous structures are used in the fields of cell expansion, drug carriers, cell micro-scaffolds and hemostatic powders.
Citation Information
Patent Citations
A microsphere of tussah silk fibroin with a three-dimensional porous structure and its preparation method
CN106637969B
A strontium-doped porous silk fibroin microsphere and its preparation method
CN108553690B
Methods and compositions for preparing a silk microsphere
CA2869967A1
Tussah fibroin protein microsphere including three-dimensional porous structure and production method thereof
CN106637969A
Fibroin micro-nano fiber microsphere as well as preparation method and application thereof
CN112316914A
Cited By
High-activity stable thrombin powder preparation and preparation method thereof
CN122097616A
Silk fibroin hard material with controllable mechanical property as well as preparation method and application of silk fibroin hard material
CN122163905A
Mechanical property controllable silk fibroin hard material, preparation method and application thereof
CN122163905B
Thrombin-loaded medical silk fibroin hemostatic sponge and preparation method thereof