Lightweight compound polysaccharide loading body with regular honeycomb porous structure

By combining microbial extracellular polysaccharides with silica nanoparticles and hydroxypropyl methylcellulose, a lightweight composite polysaccharide carrier with a regular honeycomb porous structure is prepared, which solves the problem of poor stability of existing dressings when releasing bioactive substances. solve the problem and achieve high stability and non-toxic wound surface dressings suitable for wound healing needs.

CN118772478APending Publication Date: 2024-10-15YILI NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410755070.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing wound surface dressings have poor stability when releasing bioactive substances, and the materials are not easily absorbed by the human body, resulting in unnecessary pain and secondary injuries during the wound healing process.

Method used

Using microbial extracellular polysaccharide combined with silica nanoparticles and hydroxypropyl methylcellulose, through gradient elution, vacuum drying and whipping followed by liquid nitrogen freeze-drying, a lightweight composite polysaccharide with a regular honeycomb porous structure was prepared. A load-bearing body that enhances foam stability and forms a three-dimensional framework.

Benefits of technology

It improves the stability and compressive strength of the foam, forms a uniform and fine pore structure, ensures the stable release of biologically active substances and the light breathability of the material, and the raw materials are non-toxic and pollution-free, and the preparation process is simple.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004889205350000081
    Figure BDA0004889205350000081
  • Figure BDA0004889205350000091
    Figure BDA0004889205350000091
Patent Text Reader

Abstract

The invention relates to a light composite polysaccharide loading body with a regular honeycomb porous structure, and belongs to the technical field of colloid and interface chemistry, and the light composite polysaccharide loading body is prepared by the following steps: carrying out gradient elution on microbial exopolysaccharide with an ethanol solution, and then carrying out vacuum drying and sieving for later use; mixing silicon dioxide nanoparticles with cellulose to obtain modified cellulose; s2, mixing modified cellulose with the product in the step S1, stirring, freezing with liquid nitrogen, and drying to finally obtain the light compound polysaccharide loading body with the regular honeycomb porous structure; according to the technical scheme, the microbial extracellular polysaccharide is combined with the modified cellulose, so that the silicon dioxide nanoparticles, the hydroxypropyl methyl cellulose and the microbial extracellular polysaccharide are connected together to jointly stabilize foam, the foam stability of the hydroxypropyl methyl cellulose is improved by the silicon dioxide nanoparticles and the microbial extracellular polysaccharide, and the foam stability of the hydroxypropyl methyl cellulose is improved by the modified cellulose. The prepared light compound polysaccharide loading body has a regular honeycomb porous structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of colloid and interface chemistry, and in particular relates to a light composite polysaccharide carrier with a regular honeycomb porous structure. Background Art

[0002] Traditional wound dressings are mostly gauze or sponges. The purpose of using these materials is to take advantage of their light weight and breathability. Gauze has good light weight and breathability, but it does not have a load function, such as loading nutrients, antibiotics and other bioactive substances. Although some foam sponges have a honeycomb structure, there is no pore structure on the bubble surface membrane, and even if they are loaded with bioactive ingredients, they cannot be released. Moreover, these materials cannot be absorbed by the human body. After the wound heals, the dressing needs to be removed because the dressing is bonded to the liquid secreted by the wound. The removal process is not only a second injury to the wound, but also brings unnecessary pain to the injured. Lightweight and breathable dressings that can be absorbed by the human body are needed by the market. The honeycomb structure is a common structure of surface-active substances after drying, but the regularity and mechanical properties of this structure vary depending on the raw materials.

[0003] Surfactant refers to a substance that can significantly change the interfacial state of its solution system when added in small amounts. Although some small molecule surfactants have excellent foaming properties, the biological changes caused by surfactants and their metabolites in the body may cause certain toxic side effects to the body; although large molecular organic substances such as certain proteins also have excellent foaming properties and high safety, their properties are sensitive and prone to denaturation. Their foaming properties are easily affected by their own factors such as the properties and concentration of protein molecules, as well as environmental factors such as acid, alkali, salt, and temperature; hydroxypropyl methylcellulose aqueous solution has good surface activity and can form a large number of bubbles after whipping, but the foam stability is extremely poor, and the whipped foam will completely break within minutes or even seconds. Summary of the invention

[0004] The object of the present invention is to provide a light composite polysaccharide carrier with a regular honeycomb porous structure. The method comprises the following steps: gradiently eluting microbial extracellular polysaccharides with an ethanol solution, vacuum drying, sieving and setting aside the mixture so as to remove insoluble impurities such as cell walls; mixing silica nanoparticles with cellulose to obtain modified cellulose. The addition of silica nanoparticles can enhance the foam stability of hydroxypropyl methylcellulose, and the silica nanoparticles can form a three-dimensional framework on the surface of bubbles, making it more difficult for foam to be discharged, the membrane to be broken and the bubbles to be coarsened; mixing the modified cellulose with the product in step S1, whipping the mixture, freezing the mixture with liquid nitrogen and drying the mixture, and finally obtaining a light composite polysaccharide carrier with a regular honeycomb porous structure. The microbial extracellular polysaccharide is used as a foam stabilizer to further enhance the foam stability of hydroxypropyl methylcellulose, so that the silica nanoparticles, hydroxypropyl methylcellulose and the microbial extracellular polysaccharide are interconnected to stabilize the foam together, and the obtained light composite polysaccharide carrier has a regular honeycomb porous structure.

[0005] The technical problem to be solved by the present invention is that although some small molecule surfactants have excellent foaming properties, the biological changes caused by the surfactants and their metabolites in the body may cause certain toxic side effects to the body; although macromolecular organic substances such as certain proteins also have excellent foaming properties and high safety, their properties are sensitive and easy to denature, and their foaming properties are easily affected by their own factors such as the properties and concentration of protein molecules, as well as environmental factors such as acid, alkali, salt, and temperature; hydroxypropyl methylcellulose aqueous solution has good surface activity and can form a large number of bubbles after whipping, but the foam stability is extremely poor, and the whipped foam is completely broken within minutes or even seconds.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a lightweight composite polysaccharide carrier having a regular honeycomb porous structure comprises the following steps:

[0008] S1: After the microbial exopolysaccharide is gradiently eluted with an ethanol solution, it is vacuum dried, sieved, and set aside;

[0009] S2: mixing silica nanoparticles with cellulose to obtain modified cellulose;

[0010] S3: The modified cellulose is mixed with the product in step S1, and after whipping, it is frozen with liquid nitrogen and dried to finally obtain a lightweight composite polysaccharide carrier with a regular honeycomb porous structure.

[0011] Further, in step S1, specifically the following steps are included:

[0012] The microbial extracellular polysaccharide was gradiently eluted with 50%, 75%, 85%, 95%, and 100% ethanol solutions, wherein 50% and 75% ethanol were respectively washed twice, and after vacuum drying at 55-65°C for 4-8h, it was sieved through a 90-105 mesh sieve to remove insoluble impurities such as cell walls, and set aside.

[0013] Furthermore, the microbial extracellular polysaccharide is Brunei gum or xanthan gum.

[0014] Furthermore, step S2 specifically includes the following steps:

[0015] Silica nanoparticles are added to a sodium hydroxide solution (pH 10.5), and ultrasonically treated at 15-25°C for 15-25 minutes (ultrasonic frequency is 40kHz) to obtain a suspension, and then cellulose is added to the suspension and stirred for 2-4 hours. After filtering, the suspension is washed with deionized water and dried at room temperature to obtain modified cellulose, wherein the amount ratio of the silica nanoparticles, the sodium hydroxide solution and the cellulose is 0.9-1.1g:15-25mL:0.05-0.1g.

[0016] Furthermore, the cellulose is hydroxypropyl methylcellulose.

[0017] Furthermore, the hydroxypropyl methylcellulose has a methoxy content of 28-30%, a hydroxypropyl content of 7-12%, and a viscosity of a 2wt% hydroxypropyl methylcellulose aqueous solution of 50mPa.s-400Pa.s at 20°C.

[0018] Furthermore, step S3 specifically includes the following steps:

[0019] The product in step S1 is dissolved in ultrapure water to obtain a system A with a mass concentration of 0.1-2%, and the modified cellulose is dissolved in ultrapure water to obtain a system B with a mass concentration of 0.1-2%. Substance A is stirred in a water bath at 20-30°C for 110-130 minutes, and substance B is stirred at 35-45°C for 110-130 minutes with a magnetic stirrer, and then substance A:substance B is mixed at a ratio of 10:0, 8:2,

[0020] The mixture is mixed in a weight ratio of 6:4, 4:6, 2:8, and 0:10, and stirred at a rotation speed of 200-500 rpm for 1-2 hours to obtain a mixed system. The mixed system is whipped at a rotation speed of 8000-15000 rpm for 5-15 minutes, frozen with liquid nitrogen and dried to finally obtain a lightweight composite polysaccharide carrier with a regular honeycomb porous structure.

[0021] Furthermore, the product in step S1 is microbial extracellular polysaccharide with a mass fraction of 75-85%.

[0022] Furthermore, the drying is performed by vacuum freeze drying.

[0023] Furthermore, the vacuum freeze-drying time is 10-40 hours.

[0024] Beneficial effects of the present invention:

[0025] (1) In the technical scheme of the present invention, the microbial extracellular polysaccharide is gradiently eluted with an ethanol solution, vacuum dried, sieved, and set aside to remove insoluble impurities such as cell walls; the silica nanoparticles are mixed with cellulose to obtain modified cellulose. Although hydroxypropyl methylcellulose has good foaming ability, its foam stability is poor. The foam stability of hydroxypropyl methylcellulose can be enhanced by adding silica nanoparticles. The silica nanoparticles and hydroxypropyl methylcellulose can slow down the aggregation and disproportionation of bubbles by adsorbing on the bubble surface and increasing the viscosity of the cell wall paste, thereby preventing gas transfer and hindering physical drainage between the gas phase and the liquid phase. The silica nanoparticles can form a three-dimensional framework on the bubble surface, making it more difficult to discharge the foam, break the membrane, and coarsen the bubbles, thereby greatly improving the stability of the foam.

[0026] (2) In the technical scheme of the present invention, modified cellulose is mixed with the product in step S1, whipped, frozen with liquid nitrogen and dried to obtain a light composite polysaccharide carrier with a regular honeycomb porous structure. The microbial extracellular polysaccharide is Brunei gum or xanthan gum, both of which are anionic extracellular polysaccharides. Brunei gum has better rheological properties. At a lower concentration, the solution of Brunei gum has a higher viscosity and a stronger dependence on shear rate. It has extremely strong tolerance and its molecular structure does not change at 150°C. The microbial extracellular polysaccharide acts as a foam stabilizer to further enhance the foam stability of hydroxypropyl methylcellulose. By combining the microbial extracellular polysaccharide with the modified cellulose, the silica nanoparticles, hydroxypropyl methylcellulose and the microbial extracellular polysaccharide are interconnected to stabilize the foam. The silica nanoparticles are firmly attached to the outer surface of the bubbles, which also enhances the compressive strength of the foam and produces a more uniform and finer pore structure.

[0027] (3) In the technical scheme of the present invention, silica nanoparticles are mixed with cellulose and then mixed with microbial extracellular polysaccharides, and then freeze-dried in vacuum to obtain a lightweight composite polysaccharide carrier with a regular honeycomb porous structure. The combination of silica nanoparticles, hydroxypropyl methylcellulose and microbial extracellular polysaccharides not only has good foaming properties, but also has high foam stability. The raw materials used in the preparation are non-toxic and pollution-free, and the preparation process is relatively simple. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The specific parameters of the raw materials used in the present invention are as follows:

[0030] Silica nanoparticles ( Wacker) has an average diameter of 30-40nm and a specific surface area of ​​110-140m 2 / g, this silica nanoparticle is a hydrophobic amorphous flue gas silica, modified by dimethylsiloxane, with a residual silanol content of 50%, and the hydrophobicity is conducive to the adsorption of silica nanoparticles on the bubble surface; Brunei gum, its content is ≥95%, the particle size is 80 mesh, the water content is 8.9%, and the average molecular weight measured by GPC is 1.103×10 6 (±6.407%), purchased from Shandong Fengkai Biotechnology Co., Ltd. (Shandong, China).

[0031] The hydroxypropyl methylcellulose used in the following examples and comparative examples has a methoxy content of 30% and a hydroxypropyl content of 12%. At 20° C., the viscosity of a 2 wt % hydroxypropyl methylcellulose aqueous solution is 400 Pa.s.

[0032] Example 1

[0033] S1: The Brunei gum was gradiently eluted with 50%, 75%, 85%, 95%, and 100% ethanol solutions, wherein 50% and 75% ethanol were respectively washed twice, and after vacuum drying at 55°C for 4 hours, the mixture was passed through a 90-mesh sieve to remove insoluble impurities such as cell walls, and then used for standby;

[0034] S2: 0.9 g of silica nanoparticles was added to 15 mL of sodium hydroxide solution (pH 10.5), and ultrasonically treated at 15 ° C for 15 min (ultrasonic frequency was 40 kHz) to obtain a suspension, and then 0.05 g of hydroxypropyl methylcellulose was added to the suspension and stirred for 2 h. After filtering, it was washed with 30 mL of deionized water and dried at room temperature to obtain modified cellulose;

[0035] S3: The product in step S1 is dissolved in ultrapure water to obtain a system A with a mass concentration of 1%, and the modified cellulose is dissolved in ultrapure water to obtain a system B with a mass concentration of 1%. Substance A is stirred in a 20°C water bath with an electric mechanical stirrer (HD2010W, Shanghai Sile Instrument Co., Ltd.) for 110 min, and substance B is stirred at 35°C for 110 min with a magnetic stirrer. Then, substance A:substance B are mixed in a weight ratio of 8:2, and stirred at a speed of 200 rpm for 1 h to obtain a mixed system. The mixed system is whipped at a speed of 8000 rpm for 5 min, quickly frozen with liquid nitrogen, and vacuum freeze-dried for 10 h to finally obtain a lightweight composite polysaccharide carrier with a regular honeycomb porous structure, wherein the product in step S1 is Brunei gum with a mass fraction of 75%.

[0036] Example 2

[0037] S1: The Brunei gum was gradiently eluted with 50%, 75%, 85%, 95%, and 100% ethanol solutions, wherein 50% and 75% ethanol were respectively washed twice, and after vacuum drying at 60°C for 6 hours, the Brunei gum was sieved with a 100-mesh sieve to remove insoluble impurities such as cell walls, and then used for standby;

[0038] S2: 1 g of silica nanoparticles was added to 20 mL of sodium hydroxide solution (pH 10.5), and ultrasonically treated at 20 ° C for 20 min (ultrasonic frequency was 40 kHz) to obtain a suspension, and then 0.08 g of hydroxypropyl methylcellulose was added to the suspension and stirred for 3 h. After filtering, it was washed with 30 mL of deionized water and dried at room temperature to obtain modified cellulose;

[0039] S3: The product in step S1 is dissolved in ultrapure water to obtain a system A with a mass concentration of 1%, and the modified cellulose is dissolved in ultrapure water to obtain a system B with a mass concentration of 1%. Substance A is stirred in a 25°C water bath with an electric mechanical stirrer (HD2010W, Shanghai Sile Instrument Co., Ltd.) for 120 min, and substance B is stirred at 40°C for 120 min with a magnetic stirrer. Then, substance A:substance B are mixed in a weight ratio of 8:2, and stirred at a speed of 300 rpm for 1.5 h to obtain a mixed system. The mixed system is whipped at a speed of 10000 rpm for 10 min, quickly frozen with liquid nitrogen, and vacuum freeze-dried for 20 h to finally obtain a lightweight composite polysaccharide carrier with a regular honeycomb porous structure, wherein the product in step S1 is Brunei gum with a mass fraction of 80%.

[0040] Example 3

[0041] S1: The Brunei gum was gradiently eluted with 50%, 75%, 85%, 95%, and 100% ethanol solutions, wherein 50% and 75% ethanol were respectively washed twice, and after vacuum drying at 65°C for 8 hours, the mixture was sieved through a 105-mesh sieve to remove insoluble impurities such as cell walls, and then used for later use;

[0042] S2: 1.1 g of silica nanoparticles were added to 25 mL of sodium hydroxide solution (pH 10.5), and ultrasonically treated at 25 ° C for 25 min (ultrasonic frequency of 40 kHz) to obtain a suspension, and then 0.1 g of hydroxypropyl methylcellulose was added to the suspension and stirred for 4 h. After filtering, it was washed with 30 mL of deionized water and dried at room temperature to obtain modified cellulose;

[0043] S3: dissolving the product in step S1 in ultrapure water to obtain a system A with a mass concentration of 1%, dissolving modified cellulose in ultrapure water to obtain a system B with a mass concentration of 1%, stirring substance A in a 30°C water bath with an electric mechanical stirrer (HD2010W, Shanghai Sile Instrument Co., Ltd.) for 130 min, stirring substance B at 45°C with a magnetic stirrer for 130 min, and then mixing substance A:substance B in a weight ratio of 8:2, stirring at a speed of 500 rpm for 2 h to obtain a mixed system, beating the mixed system at a speed of 15000 rpm for 15 min, rapidly freezing it with liquid nitrogen and performing vacuum freeze drying for 40 h, and finally obtaining a lightweight composite polysaccharide carrier with a regular honeycomb porous structure, wherein the product in step S1 is Brunei gum with a mass fraction of 85%.

[0044] Comparative Example 1

[0045] The difference between this comparative example and Example 3 is that the Brunei gum in step S1 is replaced by guar gum, and the remaining steps and raw materials are the same as those in Example 3.

[0046] Comparative Example 2

[0047] The difference between this comparative example and Example 3 is that in step S3, substance A:substance B are mixed in a weight ratio of 6:4, and the remaining steps and raw materials are the same as those in Example 3.

[0048] Comparative Example 3

[0049] The difference between this comparative example and Example 3 is that in step S3, substance A:substance B are mixed in a weight ratio of 10:0, and the remaining steps and raw materials are the same as those in Example 3.

[0050] Comparative Example 4

[0051] The difference between this comparative example and Example 3 is that the product in step S1 is dissolved in ultrapure water to obtain system A with a mass concentration of 0.5%, and the modified cellulose is dissolved in ultrapure water to obtain system B with a mass concentration of 0.5%. The remaining steps and raw materials are the same as those in Example 3.

[0052] The light composite polysaccharide supports with regular honeycomb porous structures prepared in Examples 1-3 and Comparative Examples 1-4 were tested for hardness, brittleness, shear force, elasticity and resilience. The test results are shown in the following table:

[0053] Table 1

[0054]

[0055]

[0056] As can be seen from the data in Table 1 above, by comparing Comparative Example 1 with Example 3, it can be seen that the test results of the lightweight composite polysaccharide support having a regular honeycomb porous structure prepared by using guar gum are worse than those of Example 3, indicating that the use of Brunei gum mixed with modified cellulose can better enhance the stability of the foam and have better foaming performance;

[0057] From the comparison between Comparative Examples 2-3 and Example 3, it can be seen that the light composite polysaccharide carrier having a regular honeycomb porous structure is prepared by mixing substance A: substance B in a weight ratio of 6:4 or 10:0, and the test results are worse than those of Example 3, indicating that the mixture of substance A: substance B in a weight ratio of 8:2 has better foam stability;

[0058] By comparing Comparative Example 4 with Example 3, it can be seen that the product in step S1 and the modified cellulose are respectively dissolved in ultrapure water to obtain system A with a mass concentration of 0.5% and system B with a mass concentration of 0.5%, respectively. This indicates that dissolving the product in step S1 and the modified cellulose in ultrapure water to obtain system A with a mass concentration of 1% and system B with a mass concentration of 1%, respectively, can further improve the stability of the foam, and the prepared lightweight composite polysaccharide carrier has a regular honeycomb porous structure.

[0059] It can be seen from Table 1 above that the lightweight composite polysaccharide carrier with a regular honeycomb porous structure prepared in Examples 1-3 is compared with Comparative Examples 1-4. The modified cellulose is obtained by mixing silica nanoparticles with cellulose, and then mixed with microbial extracellular polysaccharides. After whipping, it is frozen with liquid nitrogen and dried to obtain a lightweight composite polysaccharide carrier with a regular honeycomb porous structure. The foam stability is improved, the foaming property is good, and the test performance requirements are met. The lightweight composite polysaccharide carrier with a regular honeycomb porous structure prepared in Comparative Examples 1-4 does not meet the performance requirements. This shows that the lightweight composite polysaccharide carrier with a regular honeycomb porous structure prepared by the present invention has good foam stability and good foaming property, and the prepared raw materials are pollution-free and the operation is relatively simple.

[0060] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0061] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a lightweight composite polysaccharide carrier having a regular honeycomb porous structure, It is characterized in that The following steps are involved: S1: After the microbial exopolysaccharide is gradiently eluted with an ethanol solution, it is vacuum dried, sieved, and set aside; S2: The product in step S1 is mixed with modified cellulose, and after whipping, it is frozen with liquid nitrogen and dried to finally obtain a lightweight composite polysaccharide carrier with a regular honeycomb porous structure.

2. A method for preparing a lightweight composite polysaccharide carrier having a regular honeycomb porous structure according to claim 1, It is characterized in that Step S1 is specifically: The microbial extracellular polysaccharide was gradiently eluted with 50%, 75%, 85%, 95% and 100% ethanol solutions, wherein 50% and 75% ethanol were respectively washed twice, and vacuum dried at 55-65°C for 4-8h, and then passed through a 90-105 mesh sieve for use.

3. A method for preparing a lightweight composite polysaccharide carrier having a regular honeycomb porous structure according to claim 2, It is characterized in that The microbial extracellular polysaccharide is Brunei gum or xanthan gum.

4. A method for preparing a lightweight composite polysaccharide carrier having a regular honeycomb porous structure according to claim 1, It is characterized in that Step S2 is specifically as follows: The silica nanoparticles are added to a sodium hydroxide solution and ultrasonically treated at 15-25° C. for 15-25 minutes to obtain a suspension, and then cellulose is added to the suspension and stirred for 2-4 hours. After filtering, the suspension is washed with deionized water and dried at room temperature to obtain modified cellulose.

5. A method for preparing a lightweight composite polysaccharide carrier having a regular honeycomb porous structure according to claim 4, It is characterized in that The dosage ratio of the silicon dioxide nanoparticles, the sodium hydroxide solution and the cellulose is 0.9-1.1 g: 15-25 mL: 0.05-0.1 g.

6. The method for preparing a lightweight composite polysaccharide carrier having a regular honeycomb porous structure according to claim 4, wherein the cellulose is hydroxypropyl methylcellulose.

7. A method for preparing a lightweight composite polysaccharide carrier having a regular honeycomb porous structure according to claim 1, It is characterized in that Step S3 is specifically as follows: The product in step S1 is dissolved in ultrapure water to obtain a system A with a mass concentration of 0.1-2%, and the modified cellulose is dissolved in ultrapure water to obtain a system B with a mass concentration of 0.1-2%. Substance A is stirred in a water bath at 20-30°C for 110-130 minutes, and substance B is stirred at 35-45°C for 110-130 minutes using a magnetic stirrer. Substance A:substance B are mixed in weight ratios of 10:0, 8:2, 6:4, 4:6, 2:8, and 0:10, and stirred at a speed of 200-500 rpm for 1-2 hours to obtain a mixed system. The mixed system is whipped at a speed of 8000-15000 rpm for 5-15 minutes, frozen with liquid nitrogen, and dried to finally obtain a lightweight composite polysaccharide carrier with a regular honeycomb porous structure.

8. A method for preparing a lightweight composite polysaccharide carrier having a regular honeycomb porous structure according to claim 7, It is characterized in that The product in step S1 is microbial extracellular polysaccharide with a mass fraction of 75-85%.

9. The method for preparing a light composite polysaccharide carrier having a regular honeycomb porous structure according to claim 7, It is characterized in that The drying is performed by vacuum freeze drying.

10. A light composite polysaccharide carrier having a regular honeycomb porous structure obtained by the preparation method according to any one of claims 1 to 9.