Vulcanized rubber composition, vulcanized rubber and tire
By using a specific combination of vulcanized rubber compositions in tires and utilizing the conjugated delocalized molecular orbitals of polyaniline and the synergistic effect of nitrogen atoms and carbon black, the problem of tires having low heat generation, low resistance and aging resistance is solved. Achieved low resistance and improved aging resistance.
Patent Information
- Application Number
- CN202411009077.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult for existing tires to balance low heat generation, low resistance and aging resistance. Especially when white carbon black is used to replace carbon black, the conductive properties limit its application and lead to a decrease in the aging resistance of the rubber compound.
A vulcanized rubber composition is used, including natural rubber, styrene-butadiene rubber, butadiene rubber, carbon black, white carbon black, silane coupling agent, polyaniline and sulfur, through the conjugated delocalized molecular orbitals and nitrogen atoms of polyaniline. The synergistic effect with carbon black reduces the conductive percolation threshold, improves conductive properties, and improves the dispersion effect and aging resistance of silica through the hydrogen bonding and -NH- structure of polyaniline and silica.
It achieves low heat generation, low resistance and aging resistance of vulcanized rubber, is suitable for ordinary extrusion equipment and processes, and improves the safety and service life of tires.
Smart Images

Figure BDA0004963886440000061 
Figure BDA0004963886440000071 
Figure BDA0004963886440000081
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of tires, and in particular to a vulcanized rubber composition, a vulcanized rubber and a tire. Background Art
[0002] As competition in the tire industry becomes increasingly fierce, the performance requirements for tires are becoming more and more stringent, especially in terms of fuel economy and environmental protection. In order to reduce fuel consumption and reduce pollution to the environment, the requirements for the heat generation performance of tires are becoming higher and higher. At present, the conventional measures in the industry to reduce the heat generation of tire rubber include the use of low-heat-generating modified rubber, a large amount of white carbon black replacing carbon black, high-activity silane and various low-heat-generating modification additives, etc. Among them, the more economical and environmentally friendly measure is to replace carbon black with a large amount of white carbon black. When white carbon black replaces carbon black, as the amount of white carbon black replacement increases, the heat generation performance of the rubber is significantly improved. However, since white carbon black is not conductive, when the white carbon black content is high, the resistance of the tire will be greatly increased, and the static electricity in the tire cannot be discharged in time, thereby causing safety accidents. Therefore, the conductive performance greatly limits the application of white carbon black. In addition, after a large amount of white carbon black replaces carbon black, it will also cause the aging resistance of the rubber to decline.
[0003] The Chinese patent application with patent application publication number CN109627779A discloses a silicone rubber composition for integrated circuits, which is prepared from the following substances: vinyl-terminated polysiloxane containing white carbon black, low-viscosity vinyl-terminated polysiloxane, hydroxy silicone oil, ultrafine hollow silica, polyaniline / metal quantum dot composite material, Si-O-based linear polymethylmethoxysiloxane crosslinking agent, platinum catalyst and other materials, mainly to provide a silicone rubber composition with good flame retardant properties and low dielectric constant, but polyaniline only solves the problem of low dielectric constant and cannot simultaneously meet the low heat generation performance.
[0004] A Chinese patent application with patent application publication number CN102132358A discloses a conductive coating composition, the characteristic of which is that the binder contains silica sol dispersed in a polymerizable monomer, which is obtained by dispersing colloidal silica in a polymerizable organic compound monomer. A conductive film with high transparency and excellent strength is prepared from the composition, but the conductive film cannot achieve the excellent properties of low heat generation and high conductivity at the same time.
[0005] The Chinese patent with the patent authorization announcement number CN112409657B uses carbon nanotubes and graphene as the main conductive fillers, and uses plasticizers to improve the dispersion effect of the fillers in the rubber compound, overcoming the problem that it is difficult for carbon nanotubes and the rubber matrix to form an effective interface bonding, and realizes the uniform dispersion of carbon nanotubes in the rubber matrix. The prepared rubber has good electrical conductivity and mechanical properties, and significantly improves the electromagnetic shielding performance in the high-frequency band, but the heat generation of the rubber compound is still relatively high.
[0006] The Chinese patent with the patent authorization announcement number CN110591174B adds high cross-linking density cross-linked rubber and conductive filler to sulfur-cured olefin rubber. Due to the volume exclusion effect of the high cross-linking density cross-linked rubber, the conductive filler is selectively distributed in the olefin rubber matrix, thereby reducing the amount of conductive filler, improving the conductivity of the rubber while reducing its density. In addition, due to the formation of interfacial cross-linking between the olefin rubber and the high cross-linking density cross-linked rubber, based on the fluid mechanics volume effect and energy dissipation mechanism of the high cross-linking density cross-linked rubber, the addition of high cross-linking density cross-linked rubber can also simultaneously improve the modulus and strength of the rubber, but the heat generation of the rubber is still high.
[0007] At present, many companies in the tire industry use conductive rubber strips on the tire tread to conduct static electricity accumulated during driving, but this has high requirements for extrusion equipment and processes. Therefore, it is urgent to develop a rubber that is suitable for ordinary extrusion equipment and processes and has low heat generation, low resistance and aging resistance. Summary of the invention
[0008] The main purpose of the present invention is to provide a vulcanized rubber composition, a vulcanized rubber and a tire, so as to solve the problem that the tire in the prior art cannot have low heat generation, low resistance and aging resistance.
[0009] To achieve the above object, according to one aspect of the present invention, a vulcanized rubber composition is provided, which comprises, by weight, 10.0 to 50.0 parts of natural rubber, 10.0 to 70.0 parts of styrene-butadiene rubber, 10.0 to 50.0 parts of butadiene rubber, 10.0 to 30.0 parts of carbon black, 10.0 to 70.0 parts of white carbon black, 2.0 to 8.0 parts of silane coupling agent, 2.0 to 10.0 parts of polyaniline, 2.5 to 8.0 parts of activator and 0.8 to 2.0 parts of sulfur.
[0010] Furthermore, the vulcanized rubber composition comprises 10.0 to 40.0 parts of natural rubber, 10.0 to 60.0 parts of styrene-butadiene rubber, 10.0 to 40.0 parts of butadiene rubber, 10.0 to 25.0 parts of carbon black, 10.0 to 60.0 parts of white carbon black, 2.0 to 6.0 parts of silane coupling agent and 3.0 to 8.0 parts of polyaniline.
[0011] Furthermore, the average relative molecular mass of the polyaniline is 3000-9000; and / or the polyaniline is sulfonic acid group-modified polyaniline; and / or the mass content of sulfonic acid groups in the sulfonic acid group-modified polyaniline is 1.5%-4.5%.
[0012] Furthermore, the mass ratio of the polyaniline to the carbon black is 0.2-0.54:1.
[0013] Furthermore, the mass ratio of the polyaniline to white carbon black is 0.06-0.16:1.
[0014] Furthermore, the mass ratio of the natural rubber, styrene-butadiene rubber and butadiene rubber is 1-3:3-4:4-5.
[0015] Furthermore, the above-mentioned styrene-butadiene rubber is solution-polymerized styrene-butadiene rubber; preferably, the model of the solution-polymerized styrene-butadiene rubber is SOL5251H; and / or, the content of cis-butadiene in the butadiene rubber is ≥96.0%; preferably, the butadiene rubber is BR9000; and / or, the model of carbon black is selected from any one or more of N115, N134, N110, N234 and N220; and / or, the model of white carbon black is selected from any one or more of Z1165MP, Z1115MP and Z200MP; and / or, the model of the silane coupling agent is selected from any one or more of Si75, Si69 and Si747.
[0016] Furthermore, the activator is stearic acid and zinc oxide, the weight proportion of stearic acid is 1.0-3.0 parts, and the weight proportion of zinc oxide is 1.5-5.0 parts; and / or, the vulcanized rubber composition further comprises 0.8-2.0 parts of protective wax, 1.6-5 parts of chemical antioxidant, 0.8-3.5 parts of accelerator and 0.1-0.2 parts of scorch retarder.
[0017] According to another aspect of the present invention, a vulcanized rubber is provided. The vulcanized rubber is prepared from the aforementioned vulcanized rubber composition.
[0018] According to another aspect of the present invention, a tire is provided, wherein the tire contains the aforementioned vulcanized rubber.
[0019] By using the technical solution of the present application, the sp occupied by the lone pair electrons of the nitrogen atom in the polyaniline in the vulcanized rubber composition of the present application is 3 Hybrid orbitals are larger than the sp occupied by the lone pair of electrons of the nitrogen atom in ammonia 3The hybrid orbital has more p orbital components, which can overlap with the π electron orbital of the benzene ring in polyaniline to some extent, forming a conjugated delocalized molecular orbital including nitrogen atoms and benzene rings. Electrons can move freely in the conjugated delocalized molecular orbital. At the same time, the nitrogen atom contains lone pairs of electrons. The lone pairs of electrons and the π electrons of the benzene ring can move in the conjugated delocalized molecular orbital, and have the free electrons necessary for conductivity. Therefore, polyaniline contains the electrons and moving orbits required for conductivity. At the same time, the molecular orbital of polyaniline and the molecular orbital of the aromatic ring of carbon black cooperate with each other. The electrons of polyaniline and the π electrons of the aromatic ring in the carbon black structure cooperate with each other, which helps to reduce the conductive percolation threshold of the vulcanized rubber, thereby helping to reduce the resistance of the rubber, and then helping to improve the conductive properties of the rubber. In addition, the -N= structure contained in polyaniline can form hydrogen bonds with the -OH on the surface of silica, which helps to reduce the polarity of the silica surface, thereby helping to improve the dispersion effect of silica in the rubber, and then helping to reduce the heat generation of the rubber. The -NH- structure contained in polyaniline has a synergistic effect with the diene vulcanized rubber, and can timely eliminate the peroxides formed by the reaction with oxygen during the thermal oxidation aging process of the diene vulcanized rubber, thereby helping to interrupt the autocatalytic oxidation process of the vulcanized rubber, and further helping to improve the aging resistance of the tire. Therefore, the vulcanized rubber prepared by using the vulcanized rubber composition of the present application has the advantages of low heat generation, low resistance and aging resistance. DETAILED DESCRIPTION
[0020] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0021] As analyzed in the background technology of the present application, the tires in the prior art cannot take into account the problems of low heat generation, low resistance and aging resistance. In order to solve this problem, the present application provides a vulcanized rubber composition, a vulcanized rubber and a tire.
[0022] In a typical embodiment of the present application, a vulcanized rubber composition is provided, which includes, by weight, 10.0 to 50.0 parts of natural rubber, 10.0 to 70.0 parts of styrene-butadiene rubber, 10.0 to 50.0 parts of butadiene rubber, 10.0 to 30.0 parts of carbon black, 10.0 to 70.0 parts of white carbon black, 2.0 to 8.0 parts of a silane coupling agent, 2.0 to 10.0 parts of polyaniline, 2.5 to 8.0 parts of an activator and 0.8 to 2.0 parts of sulfur.
[0023] The sp occupied by the lone pair electrons of the nitrogen atom in the polyaniline in the vulcanized rubber composition of the present application 3 Hybrid orbitals are larger than the sp occupied by the lone pair of electrons of the nitrogen atom in ammonia 3The hybrid orbital has more p orbital components, which can overlap with the π electron orbital of the benzene ring in polyaniline to some extent, forming a conjugated delocalized molecular orbital including nitrogen atoms and benzene rings. Electrons can move freely in the conjugated delocalized molecular orbital. At the same time, the nitrogen atom contains lone pairs of electrons. The lone pairs of electrons and the π electrons of the benzene ring can move in the conjugated delocalized molecular orbital, and have the free electrons necessary for conductivity. Therefore, polyaniline contains the electrons and moving orbits required for conductivity. At the same time, the molecular orbital of polyaniline and the molecular orbital of the aromatic ring of carbon black cooperate with each other. The electrons of polyaniline and the π electrons of the aromatic ring in the carbon black structure cooperate with each other, which helps to reduce the conductive percolation threshold of the vulcanized rubber, thereby helping to reduce the resistance of the rubber, and then helping to improve the conductive properties of the rubber. In addition, the -N= structure contained in polyaniline can form hydrogen bonds with the -OH on the surface of silica, which helps to reduce the polarity of the silica surface, thereby helping to improve the dispersion effect of silica in the rubber, and then helping to reduce the heat generation of the rubber. The -NH- structure contained in polyaniline has a synergistic effect with the diene vulcanized rubber, and can timely eliminate the peroxides formed by the reaction with oxygen during the thermal oxidation aging process of the diene vulcanized rubber, thereby helping to interrupt the autocatalytic oxidation process of the vulcanized rubber, and further helping to improve the aging resistance of the tire. Therefore, the vulcanized rubber prepared by using the vulcanized rubber composition of the present application has the advantages of low heat generation, low resistance and aging resistance.
[0024] In order to further improve the low heat generation, low resistance and aging resistance of the vulcanized rubber, in one embodiment of the present application, the vulcanized rubber composition preferably includes 10.0 to 40.0 parts of natural rubber, 10.0 to 60.0 parts of styrene-butadiene rubber, 10.0 to 40.0 parts of butadiene rubber, 10.0 to 25.0 parts of carbon black, 10.0 to 60.0 parts of white carbon black, 2.0 to 6.0 parts of silane coupling agent and 3.0 to 8.0 parts of polyaniline.
[0025] In one embodiment of the present application, the average relative molecular mass of the polyaniline is 3000-9000; and / or the polyaniline is sulfonic acid group-modified polyaniline; and / or the mass content of sulfonic acid groups in the sulfonic acid group-modified polyaniline is 1.5%-4.5%.
[0026] The average relative molecular weight of polyaniline is too low, which is not conducive to improving the electrical conductivity of the vulcanized rubber. The average relative molecular weight of polyaniline is too high, which is not conducive to improving its compatibility with other components, and thus is not conducive to improving its dispersion effect in the vulcanized rubber composition, and thus is not conducive to improving the low heat generation performance of the rubber compound. It is preferred to control the average relative molecular weight of polyaniline within the above range, which helps to take into account the low resistance and low heat generation performance of the vulcanized rubber. The polarity of polyaniline is relatively large, and the use of sulfonic acid groups to modify polyaniline helps to reduce the polarity of polyaniline, thereby helping to improve the compatibility of polyaniline with diene vulcanized rubber, and then helps to improve the low heat generation performance of the vulcanized rubber finally formed. The mass content of sulfonic acid groups in sulfonic acid group-modified polyaniline is too low, which is not conducive to improving the dispersibility of polyaniline and its compatibility with rubber, and thus is not conducive to improving the low heat generation performance of the rubber compound. Too high a mass content of sulfonic acid groups in the sulfonic acid group-modified polyaniline is not conducive to improving the electrical conductivity of the polyaniline. It is preferred to control the mass content of sulfonic acid groups in the sulfonic acid group-modified polyaniline within the above range, which helps to further improve the low heat generation and low resistance properties of the finally formed vulcanized rubber.
[0027] In one embodiment of the present application, the mass ratio of the polyaniline to the carbon black is 0.2-0.54:1.
[0028] If the mass ratio of polyaniline to carbon black is too high, it will be disadvantageous to improve the low heat generation performance of the vulcanized rubber. If the mass ratio of polyaniline to carbon black is too low, the effect of improving the conductive performance is not obvious. It is preferred to control the mass ratio of polyaniline to carbon black within the above range, which will help reduce the conductive percolation threshold of the final vulcanized rubber, thereby helping to improve the conductive performance of the final vulcanized rubber.
[0029] In order to further improve the conductive properties of the final vulcanized rubber, in one embodiment of the present application, the total weight proportion of the polyaniline and carbon black in the vulcanized rubber composition is preferably ≥ 7.8%, and the mass of polyaniline / the mass of carbon black is ≥ 0.2.
[0030] In one embodiment of the present application, the mass ratio of the polyaniline to white carbon black is 0.06-0.16:1.
[0031] If the mass ratio of polyaniline to white carbon black is too high, it is not conducive to improving the low heat generation performance of the vulcanized rubber. If the mass ratio of polyaniline to white carbon black is too low, the effect of improving the low heat generation and low resistance performance is not obvious. It is preferred to control the mass ratio of polyaniline to white carbon black within the above range, which helps to improve the dispersion effect of white carbon black in the vulcanized rubber composition, and further helps to improve the low heat generation and low resistance performance of the finally formed vulcanized rubber.
[0032] In order to further improve the aging resistance of the finally formed vulcanized rubber, in one embodiment of the present application, it is preferred that the mass proportion of the polyaniline in the vulcanized rubber composition is ≥1.6%.
[0033] In one embodiment of the present application, the mass ratio of the natural rubber, styrene-butadiene rubber and butadiene rubber is 1-3:3-4:4-5.
[0034] The presence of natural rubber and butadiene rubber helps to promote the processing and molding of the vulcanized rubber composition, thereby helping to improve the control of the production process of the vulcanized rubber and help to improve the high strength and high wear resistance of the tire. The presence of styrene-butadiene rubber helps to improve the compatibility between the vulcanized rubber system and white carbon black, thereby helping to improve the low heat generation performance of the vulcanized rubber finally formed. It is preferred to control the mass ratio of natural rubber, styrene-butadiene rubber and butadiene rubber within the above range, which helps to reduce the low heat generation performance of the vulcanized rubber while improving the production efficiency of the vulcanized rubber.
[0035] In one embodiment of the present application, the above-mentioned styrene-butadiene rubber is a solution-polymerized styrene-butadiene rubber; preferably, the model of the solution-polymerized styrene-butadiene rubber is SOL5251H; and / or, the content of cis-butadiene in the butadiene rubber is ≥96.0%; preferably, the butadiene rubber is BR9000; and / or, the model of carbon black is selected from any one or more of N115, N134, N110, N234 and N220; and / or, the model of white carbon black is selected from any one or more of Z1165MP, Z1115MP and Z200MP; and / or, the silane coupling agent is selected from any one or more of Si75, Si69 and Si747.
[0036] Preferably, the type of styrene-butadiene rubber is controlled within the above range, which helps to further reduce the low heat generation performance of the vulcanized rubber finally formed. Preferably, the cis-butadiene content in cis-butadiene rubber is controlled within the above range, which helps to improve the wear resistance of the vulcanized rubber finally formed. Preferably, the types of carbon black, white carbon black and silane coupling agent are controlled within the above range, which helps to enrich the selectivity of material types and reduce the production cost of the vulcanized rubber composition.
[0037] In order to further improve the comprehensive performance of the vulcanized rubber finally formed, in one embodiment of the present application, the activator is preferably stearic acid and zinc oxide, the weight proportion of stearic acid is 1.0 to 3.0 parts, and the weight proportion of zinc oxide is 1.5 to 5.0 parts; and / or, the vulcanized rubber composition further comprises 0.8 to 2.0 parts of protective wax, 1.6 to 5 parts of chemical antioxidant, 0.8 to 3.5 parts of accelerator and 0.1 to 0.2 parts of scorch retarder. In addition, the vulcanized rubber composition further comprises 0.5 to 1.5 parts of diphenyl guanidine, preferably the chemical antioxidants are antioxidant RD and antioxidant 4020, the weight portion of antioxidant RD is 0.8 to 2.0 parts; the weight portion of antioxidant 4020 is 0.8 to 3.0 parts, preferably 0.8 to 2.5 parts; the accelerators are accelerator NS and accelerator DPG, the weight portion of accelerator NS is 0.5 to 2.0 parts, preferably 0.5 to 1.8 parts; the weight portion of accelerator DPG is 0.3 to 1.5 parts; the anti-scorch agent is anti-scorch agent CTP.
[0038] In another typical embodiment of the present application, a vulcanized rubber is provided. The vulcanized rubber is prepared from the aforementioned vulcanized rubber composition.
[0039] Since the vulcanized rubber is prepared from the vulcanized rubber composition of the present application, the vulcanized rubber has the advantages of low heat generation, low resistance and aging resistance.
[0040] In another typical embodiment of the present application, a method for preparing vulcanized rubber is provided: one-stage mixing rubber: using a GE320 internal mixer, setting the speed to 48 rpm, adding natural rubber, styrene-butadiene rubber, butadiene rubber, carbon black, white carbon black, activator, anti-aging wax and antioxidant, pressing the top bolt and mixing for 45 seconds, raising the top bolt to its place, adding silane coupling agent and polyaniline, pressing the top bolt, adjusting the speed to automatic adjustment, mixing at a constant temperature for 60 seconds, raising the top bolt, pressing the top bolt and mixing at a constant temperature for 60 seconds, raising the top bolt, pressing the top bolt and mixing at a constant temperature for 60 seconds, then opening the unloading door, discharging the rubber, controlling the rubber temperature at 150°C to 155°C, opening the mixer to unload the sheet, and cooling and collecting the rubber; two-stage mixing rubber: using a GE320 internal mixer, setting the speed to 45 rpm, adding a first stage Master rubber, press the top bolt, mix for 50 seconds, lift the top bolt to put it in place, press the top bolt and mix for 50 seconds, lift the top bolt, press the top bolt and mix for 50 seconds, open the unloading door to discharge the rubber, and the discharge temperature is controlled at 140℃~150℃; open the mixing mill to unload the sheet, cool and collect the rubber; final mixing: use GK255 internal mixer, set the speed to 34 rpm, add the second stage master rubber, sulfur, accelerator and anti-scorch agent, press the top bolt, mix for 40 seconds, lift the top bolt, press the top bolt and mix for 40 seconds, lift the top bolt, press the top bolt and mix for 40 seconds, open the unloading door to discharge the rubber, and the discharge temperature is controlled at 100~110℃, open the mixing mill to unload the sheet, cool and collect the rubber, and obtain the final mixing rubber, which is placed on a flat vulcanizer for vulcanization at a vulcanization temperature of 150℃ and a vulcanization time of 30min to obtain vulcanized rubber.
[0041] In another typical embodiment of the present application, a tire is provided, wherein the tire contains the aforementioned vulcanized rubber.
[0042] Since the tire contains the vulcanized rubber prepared from the vulcanized rubber composition of the present application, the tire has the advantages of low heat generation, low resistance and aging resistance.
[0043] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.
[0044] Example 1
[0045] The composition of the vulcanized rubber composition is shown in Table 1 in parts by weight, wherein the average relative molecular mass of the sulfonic acid group-modified polyaniline is 6000, and the mass content of the sulfonic acid group in the sulfonic acid group-modified polyaniline is 3.0%. The vulcanized rubber composition is used for the preparation of the final rubber mix: a first-stage mixing rubber: a GE320 internal mixer is used, the speed is set to 48 rpm, natural rubber, styrene-butadiene rubber, butadiene rubber, carbon black, white carbon black, activator, anti-aging wax and antioxidant are added, the top bolt is pressed and mixed for 45 seconds, the top bolt is raised and put in place, silane coupling agent and polyaniline are added, the top bolt is pressed, the speed is adjusted to automatic adjustment, and the mixture is mixed at a constant temperature for 60 seconds, the temperature of the rubber material is controlled at 155°C, the top bolt is raised, the top bolt is pressed and mixed at a constant temperature for 60 seconds, the top bolt is raised, the top bolt is pressed and mixed at a constant temperature for 60 seconds, and then Then open the unloading door, discharge the rubber, open the mixer and unload the rubber, cool and collect the rubber; second-stage mixing rubber: use GE320 internal mixer, set the speed to 45 rpm, add the first-stage masterbatch, press the top bolt, mix for 50 seconds, lift the top bolt to put it in place, press the top bolt and mix for 50 seconds, lift the top bolt, press the top bolt and mix for 50 seconds, open the unloading door to discharge the rubber, and the discharge temperature is controlled at 140℃; open the mixer and unload the rubber, cool and collect the rubber; final mixing rubber: use GK255 internal mixer, set the speed to 34 rpm, add the second-stage masterbatch, sulfur, accelerator and anti-scorch agent, press the top bolt, mix for 40 seconds, lift the top bolt, press the top bolt and mix for 40 seconds, lift the top bolt, press the top bolt and mix for 40 seconds, open the unloading door to discharge the rubber, and the discharge temperature is controlled at 110℃, open the mixer and unload the rubber, cool and collect the rubber to obtain the final mixing rubber.
[0046] Table 1
[0047]
[0048]
[0049] Example 7
[0050] The difference from Example 2 is that the weight portion of the sulfonic acid group-modified polyaniline is 2 parts, and the final rubber mixture is finally obtained.
[0051] Example 8
[0052] The difference from Example 2 is that the average relative molecular mass of the sulfonic acid group-modified polyaniline is 3000, and the final rubber mixture is finally obtained.
[0053] Example 9
[0054] The difference from Example 2 is that the average relative molecular mass of the sulfonic acid group-modified polyaniline is 9000, and the final rubber mixture is finally obtained.
[0055] Example 10
[0056] The difference from Example 2 is that the average relative molecular mass of the sulfonic acid group-modified polyaniline is 15,000, and the final rubber mixture is finally obtained.
[0057] Embodiment 11
[0058] The difference from Example 2 is that the mass content of sulfonic acid groups in the sulfonic acid group-modified polyaniline is 1.5%, and the final rubber mixture is finally obtained.
[0059] Example 12
[0060] The difference from Example 2 is that the mass content of sulfonic acid groups in the sulfonic acid group-modified polyaniline is 4.5%, and the final rubber mixture is finally obtained.
[0061] Example 13
[0062] The difference from Example 2 is that the mass content of sulfonic acid groups in the sulfonic acid group-modified polyaniline is 5.5%, and the final rubber mixture is finally obtained.
[0063] Performance Testing
[0064] The final rubber mix was vulcanized at 150°C for 30 minutes to obtain the vulcanized rubber. The final rubber mix was tested for Mooney viscosity ML (1+4) 125°C according to GB / T 1232.1-2016 Determination of Unvulcanized Rubber by Disc Shear Viscometer Part 1: Determination of Mooney Viscosity; the tensile properties of the vulcanized rubber were tested according to GB / T 528-2009 Determination of Tensile Stress-Strain Properties of Vulcanized Rubber or Thermoplastic Rubber; the hardness was tested according to GB / T 2411-2008 Determination of Shore Hardness of Plastics and Ebonite; the volume resistivity was tested according to GB 2439 Determination of Resistivity (Coefficient) of Conductive and Antistatic Rubber;
[0065] DMA test conditions: set the tensile mode, dynamic strain: 0.25%, static strain: 7%, frequency 10 Hz, test temperature range: 30-80 °C, heating rate 2 °C / min.
[0066] The final rubber mixes prepared in Examples 1 to 6 and Comparative Examples 1 and 2 were subjected to Mooney viscosity, tensile hardness / Shore A test, volume resistivity and DMA test, and the vulcanized rubber was subjected to a tensile property test after being subjected to thermal oxidative aging at 100°C*48h. The test results are shown in Table 2. The final rubber mixes prepared in Examples 7 to 15 were subjected to Mooney viscosity, tensile hardness / Shore A, volume resistivity and DMA test, and the vulcanized rubber was subjected to a tensile property test after being subjected to thermal oxidative aging at 100°C*48h. The test results are shown in Table 3.
[0067] Table 2
[0068]
[0069]
[0070] Table 3
[0071]
[0072] It can be seen from Table 2 that the volume resistivity of Example 1 is 4.50E+08. At this time, the amount of π electrons in the carbon black benzene ring structure and the free electrons in the sulfonic acid group-modified polyaniline is sufficient to connect with each other to form a conductive path in the vulcanized rubber network, so the volume resistivity is significantly reduced, which can meet the low resistance requirement. The -N= structure forms a hydrogen bond with the -OH on the surface of the white carbon black, which helps to improve the dispersion performance of the white carbon black, thereby reducing the heat generation of the vulcanized rubber; the synergistic effect of polyaniline and carbon black in Examples 2 to 5 is achieved, and the resistivity of the vulcanized rubber is low enough to meet the use requirements; the -NH- structure contained in the sulfonic acid group-modified polyaniline structure can timely eliminate the peroxides formed during the thermal oxidative aging of the diene vulcanized rubber, thereby interrupting the autocatalytic oxidation process of the diene vulcanized rubber, improving the aging resistance of the vulcanized rubber, and making the thermal oxidative aging resistance of the vulcanized rubber better; the -N= structure in the polyaniline structure forms a hydrogen bond with the -OH of the white carbon black, the synergistic effect is better, the dispersion of the white carbon black is better improved, and the heat generation of the vulcanized rubber is lower. The resistance of the vulcanized rubber of Comparative Example 1 is relatively high and cannot meet the low resistance requirement. The amount of π electrons in the carbon black benzene ring structure and the electrons in the polyaniline modified with alkanesulfonic acid in the vulcanized rubber of Comparative Example 2 is not enough to connect with each other to form a conductive path in the vulcanized rubber network, so the resistivity is still relatively high at this time.
[0073] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0074] The sp occupied by the lone pair electrons of the nitrogen atom in the polyaniline in the vulcanized rubber composition of the present application 3 Hybrid orbitals are larger than the sp occupied by the lone pair of electrons of the nitrogen atom in ammonia 3The hybrid orbital has more p orbital components, which can overlap with the π electron orbital of the benzene ring in polyaniline to some extent, forming a conjugated delocalized molecular orbital including nitrogen atoms and benzene rings. Electrons can move freely in the conjugated delocalized molecular orbital. At the same time, the nitrogen atom contains lone pairs of electrons. The lone pairs of electrons and the π electrons of the benzene ring can move in the conjugated delocalized molecular orbital, and have the free electrons necessary for conductivity. Therefore, polyaniline contains the electrons and moving orbits required for conductivity. At the same time, the molecular orbital of polyaniline and the molecular orbital of the aromatic ring of carbon black cooperate with each other. The electrons of polyaniline and the π electrons of the aromatic ring in the carbon black structure cooperate with each other, which helps to reduce the conductive percolation threshold of the vulcanized rubber, thereby helping to reduce the resistance of the rubber, and then helping to improve the conductive properties of the rubber. In addition, the -N= structure contained in polyaniline can form hydrogen bonds with the -OH on the surface of silica, which helps to reduce the polarity of the silica surface, thereby helping to improve the dispersion effect of silica in the rubber, and then helping to reduce the heat generation of the rubber. The -NH- structure contained in polyaniline has a synergistic effect with the diene vulcanized rubber, and can timely eliminate the peroxides formed by the reaction with oxygen during the thermal oxidation aging process of the diene vulcanized rubber, thereby helping to interrupt the autocatalytic oxidation process of the vulcanized rubber, and further helping to improve the aging resistance of the tire. Therefore, the vulcanized rubber prepared by using the vulcanized rubber composition of the present application has the advantages of low heat generation, low resistance and aging resistance.
[0075] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A vulcanized rubber composition, characterized in that: In parts by weight, the vulcanized rubber composition comprises: 10.0-50.0 parts of natural rubber; 10.0-70.0 parts of styrene-butadiene rubber; 10.0-50.0 parts of butadiene rubber; 10.0 to 30.0 parts of carbon black; 10.0-70.0 parts of white carbon black; 2.0 to 8.0 parts of silane coupling agent; 2.0 to 10.0 parts of polyaniline; 2.5 to 8.0 parts of an activator; and 0.8 to 2.0 parts of sulfur.
2. The vulcanized rubber composition according to claim 1, characterized in that The vulcanized rubber composition comprises: 10.0 to 40.0 parts of the natural rubber; 10.0 to 60.0 parts of the styrene-butadiene rubber; 10.0 to 40.0 parts of the butadiene rubber; 10.0 to 25.0 parts of the carbon black; 10.0 to 60.0 parts of the white carbon black; 2.0 to 6.0 parts of the silane coupling agent; and 3.0 to 8.0 parts of the polyaniline.
3. The vulcanized rubber composition according to claim 1 or 2, characterized in that: The average relative molecular mass of the polyaniline is 3000-9000; and / or the polyaniline is sulfonic acid group-modified polyaniline; and / or the mass content of sulfonic acid groups in the sulfonic acid group-modified polyaniline is 1.5%-4.5%.
4. The vulcanized rubber composition according to any one of claims 1 to 3, characterized in that The mass ratio of the polyaniline to the carbon black is 0.2-0.54:
1.
5. The vulcanized rubber composition according to any one of claims 1 to 4, characterized in that The mass ratio of the polyaniline to the white carbon black is 0.06-0.16:
1.
6. The vulcanized rubber composition according to any one of claims 1 to 5, characterized in that The mass ratio of the natural rubber, the styrene-butadiene rubber and the butadiene rubber is 1-3:3-4:4-5.
7. The vulcanized rubber composition according to any one of claims 1 to 6, characterized in that The styrene butadiene rubber is a solution polymerized styrene butadiene rubber; preferably, the model of the solution polymerized styrene butadiene rubber is SOL5251H; And / or, the content of cis-butadiene in the butadiene rubber is ≥96.0%; preferably, the butadiene rubber is BR9000; And / or, the model of the carbon black is selected from any one or more of N115, N134, N110, N234 and N220; And / or, the model of the white carbon black is selected from any one or more of Z1165MP, Z1115MP and Z200MP; And / or, the model of the silane coupling agent is selected from any one or more of Si75, Si69 and Si747.
8. The vulcanized rubber composition according to any one of claims 1 to 7, characterized in that The activator is stearic acid and zinc oxide, the weight portion of the stearic acid is 1.0 to 3.0 parts, and the weight portion of the zinc oxide is 1.5 to 5.0 parts; And / or, the vulcanized rubber composition further comprises 0.8 to 2.0 parts of protective wax, 1.6 to 5 parts of chemical antioxidant, 0.8 to 3.5 parts of accelerator and 0.1 to 0.2 parts of scorch retarder.
9. A vulcanized rubber, characterized in that: The vulcanized rubber is prepared from the vulcanized rubber composition according to any one of claims 1 to 8.
10. A tire, characterized in that: The tire contains the vulcanized rubber according to claim 9.
Citation Information
Patent Citations
Conductive coating composition
CN102132358A
Silicon rubber composition for integrated circuit and preparation process
CN109627779A
A rubber composition with high mechanical properties, high electrical conductivity, and lightweight, and its preparation method thereof.
CN110591174B
Improved conductive rubber composition and its preparation method
CN112409657B
Cited By