Efficient opening smooth master batch and preparation method thereof
Through the blending and extrusion process of carrier resin and other raw materials, an efficient and smooth opening masterbatch is prepared, which solves the difficulty in opening caused by the large surface friction coefficient of traditional masterbatch, and significantly improves the opening and ease of use of plastic films.
Patent Information
- Application Number
- CN202410978911.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-15
AI Technical Summary
After the traditional masterbatch is made into a plastic film, the surface friction coefficient is relatively large, making it difficult to open and affecting the ease of use.
Using a combination of carrier resin, anti-wear filler, slip agent, dispersant, opening agent, plasticizer, antioxidant and anti-adhesive agent, the mixed raw materials are melted into granular masterbatch through an extruder to reduce the friction coefficient And improve film opening.
It effectively reduces the friction coefficient of the masterbatch, improves the thermal stability and opening properties of the film, and solves the problem of difficulty in opening the traditional masterbatch.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of masterbatch preparation, in particular to a high-efficiency open and smooth masterbatch and a preparation method thereof. Background Art
[0002] Plastic film is a film made of polyvinyl chloride, polyethylene, polypropylene, polystyrene and other resins, used for packaging and as a coating layer. Plastic packaging and plastic packaging products occupy an increasingly large share in the market and have been widely used in food, medicine, chemical and other fields. Food packaging accounts for the largest proportion, such as beverage packaging, frozen food packaging, steamed food packaging, fast food packaging, etc. These products have brought great convenience to people's lives;
[0003] At present, for the production of plastic film, in order to better save costs and process problems, people will choose to use masterbatch, which saves a lot of overall process. However, after the masterbatch in the traditional technology is made into plastic film, its surface friction coefficient is large, which makes it difficult to open during use, affecting the convenience of using the plastic film;
[0004] To this end, the present invention provides a high-efficiency open and smooth masterbatch and a preparation method to solve the above problems. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a high-efficiency open and smooth masterbatch and a preparation method thereof, which solve the above-mentioned problems.
[0006] To achieve the above objectives, the present invention is implemented through the following technical scheme: a high-efficiency open and smooth masterbatch, which is made of the following raw materials, by weight, 50-75 parts of carrier resin, 7-18 parts of anti-wear filler, 3-9 parts of lubricant, 2-5 parts of dispersant, 3-9 parts of opening agent, 2-7 parts of plasticizer, 3-8 parts of antioxidant, and 1-5 parts of anti-adhesive agent.
[0007] Preferably, the carrier resin includes at least one of epoxy resin E0, unsaturated resin D120 and alkyd resin H50.
[0008] Preferably, the anti-wear filler includes at least one of mica, calcium carbonate, silica fume and aluminum hydroxide.
[0009] Preferably, the lubricant includes at least one of polyethylene glycol 400, sodium stearate and magnesium stearate.
[0010] Preferably, the dispersant includes at least one of an organic carboxylate and polyvinyl alcohol.
[0011] Preferably, the opening agent includes at least one of glycerol, polyethylene glycol and glyceryl stearate.
[0012] Preferably, the plasticizer includes at least one of octyl laurate caproate, octyl oleate, butyl trihydroxycaproate and trihexyl phosphate.
[0013] Preferably, the antioxidant comprises at least one of dimethyl sulfoxide and ascorbic acid.
[0014] Preferably, the anti-adhesive agent includes at least one of nano silicon dioxide, nano ferrosoferric oxide, polyvinyl butyl ether and polyphosphate hydrochloride.
[0015] A method for preparing a high-efficiency open and smooth masterbatch, the steps are as follows:
[0016] The first step is raw material preparation, which involves preparing the required ingredients by weight in advance;
[0017] The second step is to crush the raw materials and refine the larger ingredients;
[0018] The third step is raw material mixing, mixing the ingredients with the carrier resin;
[0019] The fourth step is to melt the raw materials, and put the mixed raw materials into the extruder to melt the raw material particles;
[0020] The fifth step is to extrude the masterbatch, and extrude the molten raw material into granules through an extruder to obtain the masterbatch.
[0021] Beneficial Effects
[0022] The present invention provides a high-efficiency open and smooth masterbatch and a preparation method thereof. Compared with the prior art, it has the following beneficial effects:
[0023] The high-efficiency opening and smooth masterbatch and preparation method can effectively reduce the friction coefficient of the masterbatch through the mutual coordination of carrier resin, anti-wear filler, lubricant, dispersant, opening agent, plasticizer, antioxidant and anti-adhesive agent, and have good thermal stability. After being made into a film, the problem of difficulty in opening the film can be significantly improved. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Embodiment 1:
[0026] A high-efficiency open and smooth masterbatch is made of the following raw materials, by weight: 50-75 parts of carrier resin, 7-18 parts of anti-wear filler, 3-9 parts of lubricant, 2-5 parts of dispersant, 3-9 parts of open agent, 2-7 parts of plasticizer, 3-8 parts of antioxidant and 1-5 parts of anti-adhesive agent.
[0027] Preferably, the carrier resin includes at least one of epoxy resin E0, unsaturated resin D120 and alkyd resin H50;
[0028] In more detail, the molecular structure of epoxy resin E0 contains a large number of double bonds and hydroxyl groups, which has good electrophilicity and affinity, and can effectively adsorb and bind to masterbatch particles;
[0029] The molecules of unsaturated resin D120 contain benzene rings and carbon-carbon double bonds, which have good oxidation resistance and weather resistance, and can improve the antistatic properties of masterbatch;
[0030] The molecules of alkyd resin H50 contain alcohol groups, which have good flexibility and plasticity, and can improve the processability and dispersibility of antistatic masterbatch.
[0031] Preferably, the anti-wear filler includes at least one of mica, calcium carbonate, silica fume and aluminum hydroxide.
[0032] Furthermore, mica has good heat resistance, acid resistance, alkali resistance, etc. It can enhance the wear resistance of the masterbatch and improve its mechanical strength;
[0033] Calcium carbonate has good heat resistance, acid resistance, alkali resistance and other properties, which can enhance the wear resistance of the masterbatch and improve its mechanical strength;
[0034] Silica fume has good properties of high temperature resistance, wear resistance, corrosion resistance, etc.;
[0035] Aluminum hydroxide has good acid resistance, alkali resistance, high temperature resistance and other properties. It can enhance the wear resistance of antistatic masterbatch and improve its mechanical strength.
[0036] Preferably, the lubricant includes at least one of polyethylene glycol 400, sodium stearate and magnesium stearate.
[0037] It can be understood that polyethylene glycol 400 has good solubility, hydrophilicity and thickening properties, and can effectively reduce the friction coefficient of the masterbatch surface;
[0038] Sodium stearate and magnesium stearate have good lubricity, which can effectively reduce the friction coefficient of the film surface and improve the fluidity of the film;
[0039] Preferably, the dispersant includes at least one of an organic carboxylate and polyvinyl alcohol.
[0040] Furthermore, organic carboxylates and polyvinyl alcohol can effectively disperse the antistatic filler evenly in the base resin and ensure that it has good fluidity and dispersion stability;
[0041] Preferably, the opening agent includes at least one of glycerol, polyethylene glycol and glyceryl stearate.
[0042] Furthermore, glycerol, polyethylene glycol and glyceryl stearate have good lubricating properties, which can effectively reduce the surface tension of the film, increase the softness and plasticity of the film, and also improve the heat resistance and oxidation resistance of the film, thus facilitating the smooth opening of the film during the packaging process;
[0043] Preferably, the plasticizer includes at least one of octyl laurate caproate, octyl oleate, butyl trihydroxycaproate and trihexyl phosphate.
[0044] Furthermore, octyl laurate caproate, octyl oleate, butyl trihydroxycaproate and trihexyl phosphate are used to improve the flowability and plasticizing properties of plastics;
[0045] Preferably, the antioxidant comprises at least one of dimethyl sulfoxide and ascorbic acid.
[0046] Preferably, the anti-adhesive agent includes at least one of nano silicon dioxide, nano ferrosoferric oxide, polyvinyl butyl ether and polyphosphate hydrochloride;
[0047] Among them, nano-silicon dioxide has good dispersibility and anti-adhesion properties, and can effectively prevent adhesion and agglomeration between particles;
[0048] Nano-ferroferric oxide is magnetic and can be adsorbed on the surface of particles, thereby reducing the bonding force between particles;
[0049] Polyvinyl butylate can form a protective film on the surface of the particles, thereby reducing the adhesion between the particles.
[0050] Polyphosphate hydrochloride can react with the hydroxyl groups on the particle surface to form a lubricating film, thereby reducing the adhesion between particles.
[0051] Embodiment 2:
[0052] This embodiment provides a technical solution based on the first embodiment: a high-efficiency open-mouth lubricant masterbatch, which is made of the following raw materials by weight: 66 parts of carrier resin, 11 parts of anti-wear filler, 6 parts of lubricant, 2.5 parts of dispersant, 4.5 parts of opening agent, 3 parts of plasticizer, 5 parts of antioxidant, and 2 parts of anti-adhesive agent, as shown in the following table:
[0053] raw material Weight Carrier resin 66 Anti-wear filler 11 Lubricant 6 Dispersants 2.5 Opening agent 4.5 Plasticizer 3 Antioxidants 5 Anti-adhesive 2
[0054] Preferably, the carrier resin is epoxy resin E0;
[0055] Preferably, the anti-wear filler is mica and calcium carbonate, and by weight, the mica is 70 parts and the calcium carbonate is 30 parts.
[0056] Preferably, the lubricant is polyethylene glycol 400 and sodium stearate, and in parts by weight, the polyethylene glycol 400 is 55 parts and the sodium stearate is 45 parts.
[0057] Preferably, the dispersant is an organic carboxylate.
[0058] Preferably, the opening agent is glycerol and polyethylene glycol, and by weight, glycerol is 32 parts and polyethylene glycol is 68 parts.
[0059] Preferably, the plasticizer is octyl laurate caproate, octyl oleate and trihexyl phosphate, and in parts by weight, octyl laurate caproate is 21 parts, octyl oleate is 43 parts, and trihexyl phosphate is 36 parts.
[0060] Preferably, the antioxidant is dimethyl sulfoxide.
[0061] Preferably, the anti-adhesive agent is nano-silicon dioxide and polyvinyl butyl ether, and in parts by weight, the nano-silicon dioxide is 68 parts and the polyvinyl butyl ether is 32 parts.
[0062] In summary, through testing the above masterbatch, some test data are shown in the following table:
[0063]
[0064] It can be seen from the above table that in this embodiment, the masterbatch data is:
[0065] The dynamic friction coefficient is: 0.054;
[0066] Mohs hardness is: 1;
[0067] Static friction coefficient: 0.063;
[0068] Melt flow rate: 0.65 / 10min;
[0069] Moisture content: 0.2%.
[0070] Embodiment three:
[0071] This embodiment provides a technical solution based on the first embodiment: a high-efficiency open-mouth lubricant masterbatch, which is made of the following raw materials by weight: 64 parts of carrier resin, 9 parts of anti-wear filler, 7 parts of lubricant, 4 parts of dispersant, 6 parts of open-mouth agent, 4.3 parts of plasticizer, 3.3 parts of antioxidant, and 2.4 parts of anti-adhesive agent, as shown in the following table:
[0072] raw material Weight Carrier resin 64 Anti-wear filler 9 Lubricant 7 Dispersants 4 Opening agent 6 Plasticizer 4.3 Antioxidants 3.3 Anti-adhesive 2.4
[0073] Preferably, the carrier resin is epoxy resin E0 and unsaturated resin D120, and by weight, the epoxy resin E0 is 65 parts and the unsaturated resin D120 is 35 parts;
[0074] Preferably, the anti-wear filler is mica, silica fume and aluminum hydroxide, and by weight, the mica is 23 parts, the silica fume is 44 parts, and the aluminum hydroxide is 33 parts.
[0075] Preferably, the lubricant is polyethylene glycol 400 and magnesium stearate, and in parts by weight, the polyethylene glycol 400 is 43.7 parts and the magnesium stearate is 66.3 parts.
[0076] Preferably, the dispersant is polyvinyl alcohol.
[0077] Preferably, the opening agent is polyethylene glycol and glyceryl stearate, and by weight, the polyethylene glycol is 27.5 parts and the glyceryl stearate is 72.5 parts.
[0078] Preferably, the plasticizer is octyl laurate caproate, butyl trihydroxycaproate and trihexyl phosphate, and in parts by weight, octyl laurate caproate is 36 parts, butyl trihydroxycaproate is 43 parts, and trihexyl phosphate is 21 parts.
[0079] Preferably, the antioxidant is ascorbic acid.
[0080] Preferably, the anti-adhesive agent is nano-silicon dioxide and polyphosphate hydrochloride, and in parts by weight, the nano-silicon dioxide is 50 parts and the polyphosphate hydrochloride is 50 parts.
[0081] In summary, through testing the above masterbatch, some test data are shown in the following table:
[0082]
[0083] It can be seen from the above table that in this embodiment, the masterbatch data is:
[0084] The dynamic friction coefficient is: 0.059;
[0085] Mohs hardness is: 1;
[0086] Static friction coefficient: 0.066;
[0087] Melt flow rate: 0.68 / 10min;
[0088] Moisture content: 0.2%.
[0089] Embodiment 4:
[0090] This embodiment provides a technical solution based on the first embodiment: a high-efficiency open-mouth lubricant masterbatch, which is made of the following raw materials by weight: 63 parts of carrier resin, 7 parts of anti-wear filler, 4 parts of lubricant, 5 parts of dispersant, 8 parts of opening agent, 6 parts of plasticizer, 4 parts of antioxidant, and 3 parts of anti-adhesive agent, as shown in the following table:
[0091] raw material Weight Carrier resin 63 Anti-wear filler 7 Lubricant 4 Dispersants 5 Opening agent 8 Plasticizer 6 Antioxidants 4 Anti-adhesive 3
[0092] Preferably, the carrier resin is unsaturated resin D120;
[0093] Preferably, the anti-wear filler is mica, calcium carbonate and aluminum hydroxide, and in parts by weight, mica is 42 parts, calcium carbonate is 26 parts, and aluminum hydroxide is 32 parts.
[0094] Preferably, the lubricant is sodium stearate and magnesium stearate, and by weight, the sodium stearate is 56.7 parts and the magnesium stearate is 43.3 parts.
[0095] Preferably, the dispersant is carboxylate and polyvinyl alcohol, and by weight, the carboxylate is 48.4 parts and the magnesium stearate is 51.6 parts.
[0096] Preferably, the opening agent is glycerol and glyceryl stearate, and by weight, glycerol is 50 parts and glyceryl stearate is 50 parts.
[0097] Preferably, the plasticizer is butyl trihydroxycaproate, trihexyl phosphate and trihexyl phosphate, and in parts by weight, butyl trihydroxycaproate is 64 parts, trihexyl phosphate is 21 parts, and trihexyl phosphate is 15 parts.
[0098] Preferably, the antioxidant is dimethyl sulfoxide and ascorbic acid, and by weight, the dimethyl sulfoxide is 63 parts and the ascorbic acid is 37 parts.
[0099] Preferably, the anti-adhesive agent is nano-silicon dioxide and polyphosphate hydrochloride, and in parts by weight, the nano-silicon dioxide is 50 parts and the polyphosphate hydrochloride is 50 parts.
[0100] In summary, through testing the above masterbatch, some test data are shown in the following table:
[0101]
[0102] It can be seen from the above table that in this embodiment, the masterbatch data is:
[0103] The dynamic friction coefficient is: 0.055;
[0104] Mohs hardness is: 1;
[0105] Static friction coefficient: 0.061;
[0106] Melt flow rate: 0.66 / 10min;
[0107] Moisture content: 0.2%.
[0108] Embodiment five:
[0109] This embodiment provides a method for preparing a high-efficiency open and smooth masterbatch based on the first embodiment, and the steps are as follows:
[0110] The first step is raw material preparation, which involves preparing the required ingredients by weight in advance;
[0111] The second step is to crush the raw materials and refine the larger ingredients;
[0112] The third step is raw material mixing, mixing the ingredients with the carrier resin;
[0113] The fourth step is to melt the raw materials, and put the mixed raw materials into the extruder to melt the raw material particles;
[0114] The fifth step is to extrude the masterbatch, and extrude the molten raw material into granules through an extruder to obtain the masterbatch.
[0115] In summary, by comparing the masterbatch data of Examples 2-4, it can be seen that Example 3 is the best example of the present invention.
[0116] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.
[0117] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0118] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A highly efficient and smooth masterbatch. Features: The invention is made of the following raw materials by weight: 50-75 parts of carrier resin, 7-18 parts of anti-wear filler, 3-9 parts of lubricant, 2-5 parts of dispersant, 3-9 parts of opening agent, 2-7 parts of plasticizer, 3-8 parts of antioxidant and 1-5 parts of anti-adhesive agent.
2. A high-efficiency open and smooth masterbatch according to claim 1, Features: The carrier resin includes at least one of epoxy resin E0, unsaturated resin D120 and alkyd resin H50.
3. A high-efficiency open and smooth masterbatch according to claim 1, Features: The anti-wear filler includes at least one of mica, calcium carbonate, silica fume and aluminum hydroxide.
4. A high-efficiency open and smooth masterbatch according to claim 1, Features: The lubricant includes at least one of polyethylene glycol 400, sodium stearate and magnesium stearate.
5. The high-efficiency open-mouthed and smooth masterbatch according to claim 1, Features: The dispersant includes at least one of an organic carboxylate and polyvinyl alcohol.
6. A high-efficiency open and smooth masterbatch according to claim 1, Features: The opening agent includes at least one of glycerol, polyethylene glycol and glyceryl stearate.
7. The high-efficiency open and smooth masterbatch according to claim 1, Features: The plasticizer includes at least one of octyl laurate caproate, octyl oleate, butyl trihydroxycaproate and trihexyl phosphate.
8. The high-efficiency open and smooth masterbatch according to claim 1, Features: The antioxidant includes at least one of dimethyl sulfoxide and ascorbic acid.
9. The high-efficiency open and smooth masterbatch according to claim 1, Features: The anti-adhesive agent comprises at least one of nano silicon dioxide, nano ferrosoferric oxide, polyvinyl butyl ether and polyphosphate hydrochloride.
10. A method for preparing a highly efficient open and smooth masterbatch, Features: Here are the steps: The first step is raw material preparation, which involves preparing the required ingredients by weight in advance; The second step is to crush the raw materials and refine the larger ingredients; The third step is raw material mixing, mixing the ingredients with the carrier resin; The fourth step is to melt the raw materials, and put the mixed raw materials into the extruder to melt the raw material particles; The fifth step is to extrude the masterbatch, and extrude the molten raw material into granules through an extruder to obtain the masterbatch.