PBAT / TPS-RC fully biodegradable material with double shape memory performance prepared by closed-loop recovery of caprolactone

By thermally cracking caprolactone monomer to generate polycaprolactone grafted starch, combined with a polar plasticizer, a PBAT/TPS-RC material with dual shape memory properties was prepared, which solved the problem of deformation of PBAT/TPS films during use. , realizing the reusable and fully biodegradable properties of materials, improving resource utilization and reducing carbon emissions.

CN118772610AActive Publication Date: 2024-10-15SOUTH CHINA UNIV OF TECH

Patent Information

Application Number
CN202411018378.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The existing PBAT/TPS biodegradable film is prone to deformation during use, making it difficult to reuse, and its degradation form does not comply with the low-carbon concept. Its high creep defects and complex preparation process were ignored in the study.

Method used

The caprolactone monomer recovered through efficient closed-loop thermal cracking is used to generate polycaprolactone grafted starch copolymer. Combined with polar plasticizer, in-situ ring-opening polymerization and extrusion molding methods are used to prepare dual shape memory properties. TPS-RC material and blended with PBAT to form PBAT/TPS-RC composite material.

Benefits of technology

It achieves the excellent thermal drive and microwave drive shape memory properties of the PBAT/TPS-RC material, extends the service life of the material, reduces the cost, and maintains the fully biodegradable properties. The material can effectively return to its original shape after use, achieving a one-time Reusable plastic bags.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004966423560000011
    Figure HDA0004966423560000011
  • Figure HDA0004966423560000012
    Figure HDA0004966423560000012
  • Figure HDA0004966423560000013
    Figure HDA0004966423560000013
Patent Text Reader

Abstract

The invention belongs to the technical field of fully biodegradable materials, and discloses a PBAT / TPS-RC fully biodegradable material with dual shape memory performance prepared by closed-loop recovery of caprolactone. According to the invention, a caprolactone monomer is recycled in a high-efficiency closed-loop manner through thermal cracking, a polycaprolactone grafted starch copolymer is generated through in-situ ring-opening polymerization, and TPS-RC with excellent shape memory performance is obtained through extrusion molding. When TPS-RC and PBAT are subjected to twin-screw extrusion blending and film blowing, TPS-RC is uniformly dispersed in a PBAT matrix in a micro-nano scale, and PBAT / TPS-RC shows excellent mechanical properties. And interestingness is that due to the existence of the plasticizer with strong microwave absorption, the PBAT / TPS-RC can quickly realize the dual thermal driving and microwave driving shape memory characteristics with the shape recovery rates of 97% and 100% respectively within 10-40s after being heated or heated by microwaves.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of fully biodegradable materials, and in particular relates to a PBAT / TPS-RC fully biodegradable material with dual shape memory properties prepared by closed-loop recycling of caprolactone. Background Art

[0002] At present, the threat of petroleum-based plastics to the environment has attracted extensive research and attention from researchers on fully biodegradable materials. Among them, blending expensive polybutylene terephthalate adipate (PBAT) with cheap thermoplastic starch (TPS) is an effective way to reduce costs, obtain excellent comprehensive properties and replace polyethylene (PE) plastic film.

[0003] Research on PBAT / TPS films at home and abroad mainly focuses on improving their mechanical properties, barrier properties, thermal properties, etc., aiming to prepare PBAT / TPS biodegradable films with excellent performance to expand their application areas. However, researchers have overlooked that amorphous PBAT / TPS films with excellent flexibility still have the defect of high creep, which will make the biodegradable material extremely easy to deform during daily use until it can no longer be reused, and eventually become a direct cause of disposable biodegradable waste. Although PBAT / TPS films have biodegradable properties, the final degradation form is still mainly carbon dioxide, water, etc., which does not conform well to the low-carbon concept.

[0004] Dong Yubing et al. (International Journal of Biological Macromolecules: Structure, Function and Interactions, 2023, 240) prepared a photo-crosslinked PBAT / starch film with good thermally driven shape memory properties by a one-step reaction extrusion method. The film achieved a recovery rate of 93.94% at a PBAT / starch ratio of 1:1, but the tensile strength and elongation at break were only 9.9 MPa and 400%, respectively. Chinese patent CN202310958933.0 prepared a CaCO3 / PBAT film with good shape memory properties and heat shrinkage properties by melt extrusion of CaCO3 powder and PBAT particles, with the assistance of epoxy chain extender ADR and compatibilizer SMA-2005, and a recovery rate of more than 80% can be achieved at 120°C. Research on other bio-based shape memory composites has also gradually attracted attention. Chinese patent CN201510020770.7 uses a mixing method for polylactic acid and different thermoplastic elastomers to prepare a polylactic acid-based shape memory composite material with excellent mechanical properties and shape memory properties. However, most of the thermoplastic elastomers that play an important role are not biodegradable, which affects the overall degradation performance of the material. Chinese patent CN201711348973.4 purifies malic acid by reacting it under negative pressure at 110°C for 45 hours, and then adds propylene glycol to react under negative pressure for 9 hours to prepare a biodegradable material with shape memory properties, with an optimal tensile strength of 10,000 kPa. However, this patent uses a chemical synthesis method, including purification and other processes, and the preparation cycle is long and relatively complicated.

[0005] Therefore, it is of great significance to seek a simple and easy way to enable PBAT / TPS fully biodegradable materials with excellent mechanical properties to fully realize their value and improve their reuse efficiency through multiple shape memory properties. Summary of the invention

[0006] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a TPS-RC material with shape memory properties.

[0007] The present invention utilizes caprolactone monomers recovered by thermal cracking and high-efficiency closed-loop polymerization to generate polycaprolactone grafted starch copolymers by in-situ ring-opening polymerization, and obtains TPS-RC with excellent shape memory properties by extrusion molding.

[0008] Another object of the present invention is to provide a PBAT / TPS-RC composite material with dual shape memory based on the above-mentioned TPS-RC.

[0009] The present invention utilizes TPS-RC with excellent shape memory performance to endow PBAT with excellent thermally driven shape memory performance and microwave driven shape memory performance.

[0010] Another object of the present invention is to provide a method for preparing the above-mentioned PBAT / TPS-RC composite material with dual shape memory.

[0011] Another object of the present invention is to provide application of the above-mentioned PBAT / TPS-RC composite material with dual shape memory in fully biodegradable materials.

[0012] The purpose of the present invention is achieved through the following solutions:

[0013] A TPS-RC material with shape memory properties, comprising 70-85 parts by weight of polycaprolactone grafted starch and 15-30 parts by weight of a polar plasticizer;

[0014] The raw materials of polycaprolactone grafted starch include 70-85 parts by weight of starch, 700-850 parts by weight of water, 10-100% of caprolactone by weight of starch, and 0.1-1 mol% of catalyst by weight of caprolactone monomer.

[0015] The starch is at least one of corn starch, tapioca starch and potato starch.

[0016] The caprolactone is a product of polycaprolactone (PCL) recovered by thermal cracking and high-efficiency closed-loop recovery, comprising 90-100wt% of caprolactone monomer, and the rest of the caprolactone dimer and caprolactone trimer.

[0017] The catalyst is at least one of stannous isooctanoate, cesium hydroxide monohydrate, HND580 solid acid catalyst, magnesium chloride hexahydrate, and stannous chloride.

[0018] The polar plasticizer is at least one of glycerol, ethylene glycol, pentaerythritol, sorbitol, urea and formamide.

[0019] The preparation method of the TPS-RC material with shape memory performance comprises the following steps:

[0020] (1) adding starch into water, gelatinizing, adding caprolactone for premixing, adding a catalyst, and performing an in-situ ring-opening polymerization reaction to obtain polycaprolactone grafted starch;

[0021] (2) The polycaprolactone grafted starch is mixed with a polar plasticizer and blended to obtain a TPS-RC material.

[0022] The gelatinization temperature in step (1) is 70-100° C. and the gelatinization time is 1-3 hours.

[0023] The premixing temperature in step (1) is 70-100° C. and the premixing time is 5-15 hours.

[0024] The temperature of the in-situ ring-opening polymerization reaction in step (1) is 100-130° C. and the time is 5-15 hours.

[0025] After the reaction in step (1), the obtained product is washed, specifically washed twice with ethanol, dried, crushed by a crusher, washed again three times with dichloromethane, and dried to obtain polycaprolactone grafted starch.

[0026] After the mixing in step (2), the mixture is allowed to stand for 8-16 hours.

[0027] The blending in step (2) is melt blending, including at least one of extrusion, mixing, injection molding, and open mixing.

[0028] The extruder for blending in step (2) is a co-rotating parallel twin-screw extruder (L / D=40:1); the parameters of the extruder are set such that the temperature range from the extruder feed port to the die is 80-160°C, and the screw speed is 80-120r / min.

[0029] A PBAT / TPS-RC composite material with dual shape memory based on the TPS-RC comprises 50-70 parts by weight of PBAT, 30-50 parts by weight of TPS-RC material, and 0.5-3 parts by weight of a coupling agent.

[0030] The coupling agent is at least one of KH550, KH570, DL-411 and LK-201.

[0031] The preparation method of the above-mentioned PBAT / TPS-RC composite material with dual shape memory comprises the following steps: mixing TPS-RC material, PBAT and a coupling agent, and obtaining the PBAT / TPS-RC composite material by melt blending.

[0032] The melt blending is at least one of extrusion, internal mixing, injection molding, open mixing and blow molding.

[0033] The melt blending extruder is a co-rotating parallel twin-screw extruder (L / D=40:1); the extruder parameters are set as follows: the temperature from the feed port to the die of the extruder is 100-180° C., and the screw speed is 50-300 r / min.

[0034] Application of the above-mentioned PBAT / TPS-RC composite material with dual shape memory in fully biodegradable materials.

[0035] The application is specifically to prepare the PBAT / TPS-RC composite material into a film by a blow molding machine.

[0036] The blow molding machine is a single-screw extrusion blow molding machine; the parameters are set as follows: film thickness 0.03-0.05 mm, film inflation ratio 0.5-2.5, extruder screw speed 70-100 rpm, temperature 140-150°C.

[0037] The mechanism of the present invention is:

[0038] The present invention successfully grafts caprolactone monomers recovered by thermal cracking into starch molecular chains. Compared with pure starch, after a series of reactions such as high temperature, stirring, and gelatinization, the molecular weight of polycaprolactone grafted starch is reduced, which is more conducive to the plasticization of starch, improves the fluidity of TPS-RC, and greatly improves its dispersibility in PBAT. In addition, polycaprolactone not only provides a fixing force to ensure the stability of the temporary shape, but also ensures the contraction force to restore the original permanent shape, so that TPS-RC has excellent shape memory properties.

[0039] The present invention uses polycaprolactone as a switch, and raises or lowers the temperature under the stimulation of the external environment to promote or restrict the movement of the surrounding molecular chains. When TPS-RC is blended with PBAT by twin-screw extrusion and blown film, TPS-RC is uniformly dispersed in the PBAT matrix at a micro-nano scale, and good compatibility gives PBAT / TPS-RC excellent mechanical properties. At the same time, by increasing the temperature, PBAT / TPS-RC can be stimulated to obtain excellent thermally driven shape memory properties. It is worth mentioning that since the polar plasticizer in the TPS-RC component can also be used as a strong microwave absorber, it can quickly convert microwave energy into thermal energy, perfectly realizing the excellent microwave-driven shape memory performance of PBAT / TPS-RC. Finally, the PBAT / TPS-RC film material prepared by the present invention can effectively eliminate creep after use, restore the original scale, and achieve the purpose of reusable PBAT / TPS-RC disposable plastic bags.

[0040] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0041] (1) In terms of research significance, the present invention is the first to break away from the problem of alleviating environmental pressure by replacing petroleum-based plastics with biodegradable materials. It innovatively proposes to give bio-based materials (such as PBAT / TPS materials with high creep and defects that are difficult to recover from initial size defects after being stressed) certain shape memory properties, thereby solving the problem of materials being discarded due to deformation during use, extending the material life cycle, and achieving the purpose of PBAT / TPS disposable plastic materials being reusable and maximizing their value, which has the advantages of reducing carbon emissions and improving resource utilization.

[0042] (2) The present invention proposes for the first time to utilize caprolactone monomers that are efficiently closed-loop recovered by thermal cracking to generate polycaprolactone grafted starch copolymers by in situ polymerization. The polycaprolactone grafted on the starch chain not only provides a fixing force to ensure the stability of the temporary shape, but also ensures the shrinkage force to restore the original permanent shape, successfully achieving the excellent shape memory properties of TPS-RC.

[0043] (3) While maintaining the fully biodegradable properties of the material, the present invention prepares a PBAT / TPS-RC material that can be repeatedly used and has excellent dual shape memory properties by extruding and blending TPS-RC with good shape memory properties and PBAT with high creep defects. When TPS-RC is blended with PBAT by twin-screw extrusion and film blowing, TPS-RC is dispersed in the PBAT matrix at a micro-nano scale, which not only reduces the cost of PBAT but also does not lose excellent mechanical properties (23.8MPa, 1126%), and is the first time to give PBAT excellent dual shape memory properties. PBAT / TPS-RC has excellent thermally driven shape memory, and the polar plasticizer in the TPS-RC component can also serve as a strong microwave absorber, which is expected to quickly convert microwave energy into thermal energy, thereby increasing the temperature of PBAT / TPS-RC and perfectly realizing the excellent microwave-driven shape memory properties of PBAT / TPS-RC. Among them, under thermal drive for 20-40s, the shape recovery rate of the PBAT / TPS-RC material reaches 97%, and under microwave drive for 10-20s, the shape recovery rate of the PBAT / TPS-RC material reaches 100%. Finally, the PBAT / TPS-RC film material prepared by the present invention can effectively eliminate creep after use, restore the sample to its original size, and achieve the purpose of reusable PBAT / TPS-RC disposable plastic bags. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is a "U"-shaped test result diagram of the TPS obtained in Comparative Example 2 and the TPS-RC obtained in Examples 1-3.

[0045] Figure 2 The infrared spectrum and nuclear magnetic hydrogen spectrum of the corn starch in comparative example 2 and the polycaprolactone grafted starch raw material in example 3 are shown.

[0046] Figure 3 It is a "U"-shaped test result diagram of the products obtained in Comparative Example 2 and Example 3.

[0047] Figure 4 It is a microwave test result diagram of the products obtained from Comparative Examples 1-2, Example 3 and Example 5. DETAILED DESCRIPTION

[0048] The present invention is further described in detail below in conjunction with the examples and drawings, but the embodiments of the present invention are not limited thereto. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0049] Unless otherwise specified, the reagents used in the examples can be purchased from the market.

[0050] Corn starch (food grade) used in the following examples was purchased from Shandong Hengren Industry and Trade Co., Ltd.; glycerol (analytical grade) was purchased from Tianjin Damao Chemical Reagent Factory; polybutylene terephthalate-adipate (extrusion grade) was purchased from Xinjiang Western Water Saving Technology Co., Ltd. PCL was purchased from Hunan Juren Chemical New Materials Technology Co., Ltd., M w 50000 g / mol.

[0051] Preparation of Caprolactone:

[0052] In the reaction system of reduced pressure distillation, PCL was stirred at 120°C for 2h to remove small molecular impurities in the system. Subsequently, 0.25 mol% (percentage PCL) of stannous isooctanoate was added, and the reaction product was collected by condensation at 250°C and 0.08MPa vacuum. After a period of time, the product was stopped and caprolactone was recovered.

[0053] GC test showed that the recovered product contained 91.1 wt % of caprolactone monomer, and the rest were caprolactone dimer and caprolactone trimer.

[0054] In the following examples and comparative examples, 1 part by weight means 1 gram.

[0055] Example 1

[0056] Step 1: Disperse 300 parts by weight of dried corn starch in a reactor containing 3000 parts by weight of deionized water, gelatinize at 80°C for 2 hours by mechanical stirring, introduce 60 parts by weight of caprolactone for premixing for 10 hours, finally heat to 110°C, add 0.5 mol% (percentage of caprolactone monomer) of stannous isooctanoate for catalytic reaction for 10 hours.

[0057] Step 2: The product of step 1 is washed with a large amount of ethanol and repeatedly precipitated twice, the precipitate is completely dried and powdered, and then washed with dichloromethane three times and dried for later use, thereby obtaining a polycaprolactone grafted starch raw material.

[0058] Step 3: Take 290 parts by weight of the raw materials in step 2 and 110 parts by weight of glycerol, mix them evenly, and let them stand for 12 hours.

[0059] Step 4: extrude the mixture after standing in step 3 through a co-rotating twin-screw extruder, set the temperature range from the feed port to the die of the extruder to 90-160° C., and the screw speed to 100 r / min. After cooling and granulation, TPS-3RC particles are obtained.

[0060] Step 5, 300 parts by weight of TPS-3RC particles, 700 parts by weight of PBAT and 20 parts by weight of KH570 in step 4 are premixed and evenly extruded through a co-rotating twin-screw extruder, and the temperature range from the feed port of the extruder to the die is set to 110-170 ° C, the screw speed is 100 r / min, and PBAT / TPS-3RC blend particles are obtained after cooling and granulation.

[0061] Example 2

[0062] The difference from Example 1 is that: in step 1, 150 parts by weight of caprolactone is introduced; in step 4, the product obtained is TPS-10RC; and in step 5, the product obtained is PBAT / TPS-10RC.

[0063] Example 3

[0064] The difference from Example 1 is that: in step 1, 300 parts by weight of caprolactone is introduced; in step 4, the product obtained is TPS-17RC; and in step 5, the product obtained is PBAT / TPS-17RC.

[0065] Example 4

[0066] The difference from Example 3 is that: in step 3, 310 parts by weight of the raw material in step 2 is mixed evenly with 90 parts by weight of glycerol; in step 4, the product obtained is TPS-17RC'; and in step 5, the product obtained is PBAT / TPS-17RC'.

[0067] Example 5

[0068] The difference from Example 3 is that: in step 3, 330 parts by weight of the raw material in step 2 is mixed evenly with 70 parts by weight of glycerol; in step 4, the product obtained is TPS-17RC"; and in step 5, the product obtained is PBAT / TPS-17RC".

[0069] Comparative Example 1

[0070] The difference from Example 1 is that steps 1 to 4 are not performed, and in step 5, 1000 parts by weight of PBAT particles and 83 parts by weight of glycerol are premixed uniformly, and the obtained product is PBAT.

[0071] Comparative Example 2

[0072] The difference from Example 1 is that: Steps 1 and 2 are not performed, 275 parts by weight of glycerol and 725 parts by weight of corn starch are evenly mixed in Step 3; the product obtained in Step 4 is TPS; and the product obtained in Step 5 is PBAT / TPS.

[0073] Test Example:

[0074] 1. Structural characterization and grafting rate:

[0075] Figure 2 The infrared spectra and nuclear magnetic hydrogen spectra of the corn starch in comparative example 2 and the polycaprolactone grafted starch in example 3 are shown in FIG. 1730 cm -1 There is an obvious ester peak at 2800-2950cm -1 The methylene peak was enhanced, and PCL showed obvious signal peaks at 1.3-2.3ppm and 3.99ppm in the H-NMR spectrum, indicating that polycaprolactone was successfully grafted into the starch molecular chain.

[0076] In addition, it was calculated that the grafting rates of the polycaprolactone grafted starch raw materials of Examples 1-3 were 3.2%, 9.8% and 16.6%, respectively, and thus were represented by TPS-3RC, TPS-10RC and TPS-17RC, respectively.

[0077] 2. Tensile performance test:

[0078] The products obtained in the above Examples 1-3 and Comparative Examples 1-2 were blown into films and subjected to tensile performance tests (according to GB / T1040-2006, the tensile rate was set to 500 mm / min). The test results are shown in Table 1;

[0079] Blown film forming method:

[0080] The products obtained in Examples 1-3 and Comparative Examples 1-2 were blown into films with a thickness of 0.03-0.05 mm by a single screw extrusion film blowing machine, the film blowing ratio was 1.5, the extruder screw speed was 80 rpm, and the temperature was 140-150°C.

[0081] Table 1 Tensile properties

[0082]

[0083] 3. "U" shape test:

[0084] The TPS-RC obtained in the above Examples 1-3, the TPS obtained in Comparative Example 2, and the PBAT / TPS-RC obtained in Example 3 and the PBAT / TPS blend particles obtained in Comparative Example 2 were hot pressed into sheets, and a "U" shape test was performed. The specimens were placed in a 100°C silicone oil bath to soften, and then bent into a "U" shape and quickly placed in 0°C silicone oil to set for 40 seconds. Finally, the "U" shape sample was placed in 100°C silicone oil, and the recovery was observed and recorded. The test results are shown in FIG. Figure 1 , 3 As shown in Tables 2 and 3. Figure 1 As shown in Table 2, compared with Comparative Example 2, Examples 1-3 have a higher recovery rate, indicating that the polycaprolactone finally grafted on the starch chain not only provides a fixing force to ensure the stability of the temporary shape, but also ensures the contraction force to restore the original permanent shape, successfully achieving the excellent shape memory properties of TPS-RC. Figure 3 As shown in Table 3, pure PBAT does not show any shape memory properties. Due to the introduction of TPS-RC, the strong hydrogen bond network of TPS-RC itself gives weaker shape memory properties, and the recovery rate reaches 83%. Polycaprolactone acts as a switch, raising or lowering the temperature under the stimulation of the external environment to promote or restrict the movement of the surrounding molecular chains. By raising the temperature to stimulate PBAT / TPS-RC, excellent thermally driven shape memory properties are obtained. Under thermal actuation for 20-40s, the shape recovery rate of PBAT / TPS-RC material reaches 97%.

[0085] Table 2 TPS and TPS-RC "U" test

[0086]

[0087] Table 3 “U” test of PBAT / TPS and PBAT / TPS-RC

[0088]

[0089] 4. Microwave recovery test:

[0090] The products obtained in Examples 3, 5 and Comparative Examples 1, 2 were hot pressed into sheets and cut into 50×5×1 mm 3 The spline is drawn and a 30mm long section (l0) is drawn at the center. The spline is loaded with a 300g weight and hung in a high humidity (90% HR) environment. Take it out after 2 hours and measure the length of the center part, which is recorded as l1. Finally, the deformed spline is placed in a 700W microwave oven, set to medium and high temperature, observe and record the recovery, and record the final length as l2. The recovery rate R is calculated as follows:

[0091] R=(l1-l2) / (l1-l0)×100%The microwave recovery test results are as follows Figure 4As shown in Table 4, it can be seen from Comparative Example 1 that after microwave heating, the deformed pure PBAT cannot be restored. However, since the polar plasticizer glycerol in TPS-RC can absorb microwave energy to quickly heat up PBAT / TPS-RC, it perfectly realizes the excellent microwave-driven shape memory performance of PBAT / TPS-RC. Therefore, Comparative Example 2 and Examples 3 and 5 all show different degrees of recovery. Example 5 achieves a complete recovery rate of 100% within 20s.

[0092] Table 4 Microwave recovery test of the products obtained in the comparative examples and embodiments

[0093]

[0094] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A TPS-RC material with shape memory properties, characterized in that: The invention comprises 70-85 parts by weight of polycaprolactone grafted starch and 15-30 parts by weight of a polar plasticizer; The raw materials of polycaprolactone grafted starch include 70-85 parts by weight of starch, 700-850 parts by weight of water, 10-100% of caprolactone by weight of starch, and 0.1-1 mol% of catalyst by weight of caprolactone monomer.

2. The TPS-RC material with shape memory properties according to claim 1, characterized in that: The starch is at least one of corn starch, tapioca starch and potato starch; The caprolactone is a product of polycaprolactone recovered through thermal cracking and high-efficiency closed-loop recovery, comprising 90-100 wt % of caprolactone monomer, and the rest of the caprolactone dimer and caprolactone trimer.

3. The TPS-RC material with shape memory properties according to claim 1, characterized in that: The catalyst is at least one of stannous isooctanoate, cesium hydroxide monohydrate, HND580 solid acid catalyst, magnesium chloride hexahydrate, and stannous chloride; The polar plasticizer is at least one of glycerol, ethylene glycol, pentaerythritol, sorbitol, urea and formamide.

4. The method for preparing the TPS-RC material with shape memory properties according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) adding starch into water, gelatinizing, adding caprolactone for premixing, adding a catalyst, and performing an in-situ ring-opening polymerization reaction to obtain polycaprolactone grafted starch; (2) The polycaprolactone grafted starch is mixed with a polar plasticizer and blended to obtain a TPS-RC material.

5. The method for preparing the TPS-RC material with shape memory properties according to claim 4, characterized in that: The gelatinization temperature in step (1) is 70-100° C. and the time is 1-3 hours; The premixing temperature in step (1) is 70-100° C. and the premixing time is 5-15 hours; The temperature of the in-situ ring-opening polymerization reaction in step (1) is 100-130° C. and the time is 5-15 hours.

6. The method for preparing the TPS-RC material with shape memory properties according to claim 4, characterized in that: After the mixing in step (2), the mixture is allowed to stand for 8-16 hours; The blending in step (2) is melt blending, including at least one of extrusion, mixing, injection molding, and open mixing; The extruder for blending in step (2) is a co-rotating parallel twin-screw extruder; the parameters of the extruder are set as follows: the temperature range from the extruder feed port to the die is 80-160° C., and the screw speed is 80-120 r / min.

7. A PBAT / TPS-RC composite material with dual shape memory based on the TPS-RC material according to any one of claims 1 to 3, characterized in that: The invention comprises 50-70 parts by weight of PBAT, 30-50 parts by weight of TPS-RC material and 0.5-3 parts by weight of coupling agent.

8. The PBAT / TPS-RC composite material with dual shape memory according to claim 7, characterized in that: The coupling agent is at least one of KH550, KH570, DL-411 and LK-201.

9. Use of the PBAT / TPS-RC composite material with dual shape memory as claimed in claim 7 in fully biodegradable materials.

10. The use of the PBAT / TPS-RC composite material with dual shape memory in fully biodegradable materials according to claim 9, characterized in that: The application is specifically to prepare the PBAT / TPS-RC composite material into a film by a blow molding machine; The blow molding machine is a single-screw extrusion blow molding machine; the parameters are set as follows: film thickness 0.03-0.05 mm, film inflation ratio 0.5-2.5, extruder screw speed 70-100 rpm, temperature 140-150°C.

Citation Information

Patent Citations

  • Biodegradable polylactic acid based shape memory composite material and preparation method thereof

    CN105838049A

  • High-performance shape memory biodegradable material

    CN108003330A

  • Blending modified CaCO3 / PBAT composite film as well as preparation method and application thereof

    CN117186457A

  • Biodegradable TPS / PBAT composite material and preparation method thereof

    CN103881145A

  • Triple shape memory polymer and preparation method thereof

    CN112759737A

Cited By

  • Two-way shape memory fiber with phase change energy storage and reprogramming functions and preparation method of two-way shape memory fiber

    CN122610238A