Corrosion-resistant and weather-resistant functional filler, preparation method thereof and corrosion-resistant and weather-resistant coating
By coating fly ash with a mesoporous oxide layer and a carbon quantum dot organic carbon layer, combined with weather-resistant oxide additives, the problem of insufficient anti-corrosion and weather resistance of fly ash in anti-corrosion coatings is solved, and the coating is highly efficient. Improved anti-corrosion and weather resistance.
Patent Information
- Application Number
- CN202410918365.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Adding fly ash to existing anti-corrosion coatings is not enough to meet the company's requirements for anti-corrosion and weather resistance. There are microporous defects and interface gap problems in the coating, which affect the performance of the coating.
Fly ash is used as the basic filler, and the anti-corrosion and weather-resistant functional filler is formed by coating the mesoporous oxide layer and the heteroatom-doped carbon quantum dot organic carbon layer, combined with weather-resistant oxide additives and passivation oxide additives. Prepared by one-pot calcination method and hydrothermal reaction technology to enhance the anti-corrosion and weather resistance of the coating.
It significantly improves the anti-corrosion and weather-resistant performance of the coating, reduces the degradation hazard of the weather-resistant filler to the coating, enhances the interface bonding ability between the filler and the resin matrix, and improves the density and corrosion inhibition activity of the coating.
Smart Images

Figure CN118772686A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and in particular relates to an anti-corrosion and weather-resistant functional filler and a preparation method thereof, and an anti-corrosion and weather-resistant coating. Background Art
[0002] In the field of industrial engineering, the corrosion behavior of metals has caused a lot of economic losses and waste of resources, and has brought major safety hazards. Surface coating protection technology is a simple construction and effective metal corrosion prevention measure. Some microporous defects will be formed in the coating preparation process, including gaps between polymer chains, micropores formed during solvent evaporation, and gaps between the interface of pigments and resin matrix, which have a great impact on the performance of the coating. The weather resistance of the coating is an important durability indicator. A large amount of weather-resistant fillers are often added to the weather-resistant coating. The weather-resistant fillers can fill the pores in the coating film, increase the density of the coating film, and improve the corrosion resistance and weather resistance of the coating film.
[0003] Fly ash is a common solid waste in coal-fired power plants. It has stable physical and chemical properties and has great potential in the field of anti-corrosion fillers. It is often used as a weather-resistant filler in anti-corrosion coatings. However, in actual applications, coatings with fly ash added are not enough to meet the requirements of enterprises for the anti-corrosion and weather-resistant properties of coatings, and further improvement is needed.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] The purpose of the present invention is to provide an anti-corrosion and weather-resistant functional filler and a preparation method thereof and an anti-corrosion and weather-resistant coating. The anti-corrosion and weather-resistant functional filler can improve the anti-corrosion and weather-resistant performance of the coating.
[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0007] The anti-corrosion and weather-resistant functional filler comprises fly ash, the fly ash is coated with a mesoporous oxide layer, and the mesoporous oxide layer is coated with a heteroatom-doped carbon quantum dot organic carbon layer;
[0008] The mesoporous oxide layer includes a weather-resistant element and a passivation element. The weather-resistant element is one or both of titanium and zinc, and the passivation element is one or more of cerium and iron.
[0009] In one or more embodiments of the present invention, the raw materials include, by weight: 200-400 parts of fly ash, 20-80 parts of porogen, 100-150 parts of oxide additives, 50-100 parts of carbon-based compounds, 50-100 parts of carbon quantum dot dopants, 20-50 parts of chemical modifiers and 50-150 parts of glacial acetic acid; wherein the oxide additives include weather-resistant oxide additives and passivating oxide additives, and the weather-resistant oxide additives are one or both of tetrabutyl titanate and zinc chloride; the passivating oxide additives are one or more of cerium nitrate hexahydrate, ferric chloride hexahydrate and ferric nitrate nonahydrate.
[0010] In one or more embodiments of the present invention, the porogen is selected from one or more of polyoxyethylene polyoxypropylene ether, polyethylene imine, polyethylene glycol; and / or,
[0011] The carbon-based compound is selected from one or more of 4-aminosalicylic acid, citric acid, tartaric acid, ascorbic acid, mercaptosuccinic acid, and chitosan; and / or,
[0012] The carbon quantum dot dopant is selected from one or more of thiourea, ethylenediamine, p-phenylenediamine, o-phenylenediamine, and oleylamine; and / or,
[0013] The chemical modifier is selected from one or more of γ-aminopropyltriethoxysilane, trichlorovinylsilane, α-ethyl cyanoacrylate, and dopamine hydrochloride.
[0014] In one or more embodiments of the present invention, the weight ratio of the weathering oxide additive to the passivating oxide additive is 1:(0.8-2).
[0015] Another specific embodiment of the present invention provides a technical solution as follows:
[0016] The preparation method of the anticorrosive and weather-resistant functional filler comprises the following steps:
[0017] Using fly ash, water, porogen, oxide additive and glacial acetic acid as raw materials, a mesoporous oxide layer is coated on the fly ash to obtain a mesoporous oxide-fly ash filler; wherein the oxide additive comprises a weather-resistant oxide additive and a passivating oxide additive, the weather-resistant oxide additive makes the mesoporous oxide layer include titanium and / or zinc, and the passivating oxide additive makes the mesoporous oxide layer include cerium and / or iron;
[0018] Using mesoporous oxide-fly ash filler, water, carbon-based compound and carbon quantum dot dopant as raw materials, carbon quantum dots are loaded on the mesoporous oxide-fly ash filler to obtain carbon-based mesoporous oxide-fly ash filler;
[0019] The carbon-based mesoporous oxide-fly ash filler is reacted with a chemical modifier to obtain an anti-corrosion and weather-resistant functional filler.
[0020] In one or more embodiments of the present invention, a one-pot calcination method is used to prepare a mesoporous oxide-fly ash filler, specifically, fly ash, water, a porogen, an oxide additive and glacial acetic acid are mixed, ground to form a sticky mixed material, and then calcined, ultrasonicated, hydrothermally reacted, washed with alcohol, and dried to obtain;
[0021] And / or, when preparing the mesoporous oxide-fly ash filler, the weight ratio of fly ash, water, porogen, oxide additive and glacial acetic acid is (5-15):(0.5-3.5):(2-7):(3-10):(2-8);
[0022] And / or, when preparing carbon-based mesoporous oxide-fly ash filler, the weight ratio of mesoporous oxide-fly ash filler, carbon-based compound, water and carbon quantum dot dopant is (5-10):(2-3.5):(6-18):(1.2-3).
[0023] In one or more embodiments of the present invention, the carbon-based mesoporous oxide-fly ash filler is prepared by hydrothermal reaction, and the hydrothermal reaction temperature is 130-220°C.
[0024] In one or more embodiments of the present invention, the carbon-based mesoporous oxide-fly ash filler and the chemical modifier are dispersed in an ethanol aqueous solution, stirred and mixed at 25-80°C, and then subjected to ultrasound, filtration, and drying to obtain an anti-corrosion and weather-resistant functional filler.
[0025] In one or more embodiments of the present invention, the weight ratio of the carbon-based mesoporous oxide-fly ash filler and the chemical modifier is (1-2):(0.5-1).
[0026] Another specific embodiment of the present invention provides a technical solution as follows:
[0027] The anti-corrosion and weather-resistant coating comprises the above-mentioned anti-corrosion and weather-resistant functional filler.
[0028] Compared with the prior art, the present invention applies solid waste fly ash, mesoporous oxides, carbon-based structures and carbon quantum dots to the coating system, thereby enhancing the anti-corrosion and weather resistance of the coating.
[0029] First, the microscopic morphology and composition of fly ash are optimized, and the microbead form of fly ash with excellent shielding performance is retained, providing basic shielding properties for the coating.
[0030] Then, a mesoporous oxide layer is constructed on the surface of fly ash by one-pot calcination method, which makes the filler have both anti-corrosion and weather resistance. The mesoporous structure is conducive to improving the weather resistance of the material and reducing the degradation hazard of weather-resistant fillers to the coating.
[0031] Then, in a hydrothermal reaction, the carbon-based compound is polymerized on the mesoporous oxide layer to form an organic carbon layer containing carbon quantum dots, and the organic carbon layer is doped with nitrogen and phosphorus atoms, so that the composite filler exhibits excellent corrosion inhibition activity. In the composite process of carbon quantum dots and mesoporous functional fillers, the mesoporous structure exhibits a large specific surface area, which allows it to load a large number of carbon quantum dots, thereby enhancing the corrosion inhibition performance of the coating. A carbon-coated mesoporous structure is constructed on the surface of fly ash, which enhances the interface behavior between the filler and the resin matrix.
[0032] Finally, chemical modifiers are used to modify the surface of the mesoporous anticorrosive and weather-resistant filler, which enhances the interfacial bonding ability between the filler and the resin matrix. Among them, the mesoporous oxide-fly ash filler is treated by double-layer coating, which greatly reduces the degradation effect of the weather-resistant filler on the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 The EIS test results of the coating samples of Example 1, Example 2, Comparative Example 1 and Comparative Example 2 of the present invention at 60 days;
[0035] Figure 2 The variation trend of the water contact angle of the coating samples of Example 1, Comparative Example 1 and Comparative Example 2 of the present invention over time after the xenon lamp weathering test;
[0036] Figure 3 The microscopic morphology of the mesoporous filler samples of Example 2 of the present invention and Comparative Example 2. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0038] Fly ash is a mixture with uncertain composition content and has some loose and porous morphological structures, which is not conducive to the preparation of anti-corrosion coatings with stable performance. Some oxides can provide some new properties for coatings, such as weather resistance, corrosion inhibition, etc. Therefore, the present invention explores the use of oxides to modify fly ash fillers to obtain anti-corrosion functional fillers with stable performance.
[0039] Specifically, fly ash, an industrial solid waste, is ground, classified, and calcined to strengthen its shielding properties. Fly ash with a specific particle size is selected as a basic filler to provide basic anti-corrosion properties for coatings. Since fly ash fillers have a single property, a one-pot calcination method is used to construct an oxide outer layer with specific functions on the outer layer of fly ash to prepare a functional filler precursor with both anti-corrosion and weathering properties.
[0040] However, the outer oxide layer of the anti-corrosion and weather-resistant functional filler precursor mainly exhibits weather resistance, which mainly exhibits weather resistance by absorbing ultraviolet light in the environment. This process is often accompanied by a photocatalytic effect, which will cause the coating film itself to degrade, which is not conducive to the coating film maintaining a stable anti-corrosion and weather-resistant function. Therefore, an organic carbon layer containing carbon quantum dots is constructed on the outer layer of the oxide, and the carbon quantum dots are distributed in the organic carbon layer, which can provide certain corrosion inhibition and passivation properties for the metal substrate, and at the same time can reduce the degradation of the coating film by the photocatalytic effect of the outer layer of the oxide. In addition, doping the carbon layer with heteroatom elements can further enhance the complex passivation effect of carbon quantum dots on the metal substrate.
[0041] At the same time, by introducing a porogen in the process of preparing the oxide outer layer and constructing an outer oxide with a mesoporous morphology, not only the weather-resistant reaction sites are increased, but also the contact area between the filler and the coating film is increased, thereby improving the anti-corrosion and weather resistance of the coating by the carbon layer containing carbon quantum dots, thereby appropriately reducing the degree of degradation of the coating system by the oxide outer layer due to the photocatalytic effect.
[0042] Furthermore, when preparing the oxide outer layer, tetrabutyl titanate and zinc chloride, which are mainly weather-resistant, and cerium nitrate hexahydrate, ferric chloride hexahydrate and ferric nitrate nonahydrate, which have a passivating effect on the metal substrate, are selected to make the oxide outer layer exhibit weather-resistant function while reducing the negative impact of the photocatalytic effect.
[0043] A specific embodiment of the present invention provides an anti-corrosion and weather-resistant functional filler, including fly ash, the fly ash is coated with a mesoporous oxide layer, and the mesoporous oxide layer is coated with a heteroatom-doped carbon quantum dot organic carbon layer; the mesoporous oxide layer includes a weather-resistant element and a passivation element, the weather-resistant element is one or both of titanium and zinc, and the passivation element is one or more of cerium and iron.
[0044] Specifically, fly ash itself has excellent shielding properties, and a mesoporous oxide layer is formed on the surface of fly ash. The oxide layer is prepared by using tetrabutyl titanate and zinc chloride, which are mainly weather-resistant, and cerium nitrate hexahydrate, ferric chloride hexahydrate and ferric nitrate nonahydrate, which are mainly passivation. The oxide layer is in the form of oxide doping or even atomic doping, so that the oxide layer effectively improves the overall weather resistance of the filler. In addition, carbon quantum dots are a kind of carbon-based zero-dimensional material. The surface of carbon quantum dots contains a large number of active groups, such as hydroxyl, carboxyl, amino, etc., which make it have excellent corrosion inhibition. The organic carbon layer containing carbon quantum dots is coated on the oxide layer. On the one hand, the affinity between the organic carbon layer and the coating system can improve the interface bonding performance between the filler and the coating. On the other hand, the coating effect of carbon quantum dots on the oxide layer can appropriately reduce the decomposition effect of the oxide layer on the coating.
[0045] In addition, although the coating of the oxide layer by the organic carbon layer appropriately reduces the photocatalytic effect, the mesoporous morphology of the oxide layer provides a channel for oxygen transmission, so that the filler retains the weathering effect of the oxide layer on the coating. Therefore, through the compound use of the mesoporous oxide layer, the weathering oxide additive and the passivating oxide additive, and the comprehensive effect of the organic carbon layer on the fly ash, the fly ash filler formed can simultaneously improve the weathering resistance and anti-corrosion performance of the coating, and can reduce the negative impact of the photocatalytic effect on the coating.
[0046] In a specific embodiment, the raw materials include, by weight: 200-400 parts of fly ash, 20-80 parts of porogen, 100-150 parts of oxide additives, 50-100 parts of carbon-based compounds, 50-100 parts of carbon quantum dot dopants, 20-50 parts of chemical modifiers and 50-150 parts of glacial acetic acid; wherein the oxide additives include weather-resistant oxide additives and passivating oxide additives, the weather-resistant oxide additive is one or both of tetrabutyl titanate and zinc chloride; the passivating oxide additive is one or more of cerium nitrate hexahydrate, ferric chloride hexahydrate and ferric nitrate nonahydrate.
[0047] In a specific embodiment, the porogen is selected from one or more of polyoxyethylene polyoxypropylene ether, polyethylene imine, and polyethylene glycol; the carbon-based compound is selected from one or more of 4-aminosalicylic acid, citric acid, tartaric acid, ascorbic acid, mercaptosuccinic acid, and chitosan; the carbon quantum dot dopant is selected from one or more of thiourea, ethylenediamine, p-phenylenediamine, o-phenylenediamine, and oleylamine; the chemical modifier is selected from one or more of γ-aminopropyltriethoxysilane, trichlorovinyl silane, α-ethyl cyanoacrylate, and dopamine hydrochloride.
[0048] Specifically, porogens are used to create pores in the oxide layer, construct a unique mesoporous structure, and increase the reactive sites of the filler. Carbon quantum dot dopants can introduce N and S atoms into the carbon quantum dot layer. N and S atoms have lone pairs of electrons or π bonds, which are easily adsorbed on the metal surface, hindering the contact between corrosive media and metals, thereby enhancing the corrosion inhibition and anti-corrosion effect of the organic carbon layer on the metal substrate. After the chemical modifier modifies the filler, the interface modification of the functional group can enhance the bonding between the filler and the coating system, thereby promoting the dispersion of the filler in the coating, improving the mechanical properties of the coating, and also helping the filler to play a weather-resistant role in the coating.
[0049] In a specific embodiment, the weight ratio of the weather-resistant oxide additive to the passivating oxide additive is 1:(0.8-2).
[0050] Specifically, the weather-resistant oxide additive and the passivating oxide additive are compounded in a specific weight ratio so that the prepared filler has better anti-corrosion and weather-resistant effects.
[0051] Another specific embodiment of the present invention provides a method for preparing an anti-corrosion and weather-resistant functional filler, comprising steps 1-3.
[0052] Step 1, using fly ash, water, porogen, oxide additive and glacial acetic acid as raw materials, coating the fly ash with a mesoporous oxide layer through a one-pot calcination method to obtain a mesoporous oxide-fly ash filler.
[0053] Specifically, in step 1, fly ash filler, water, porogen, oxide additive and glacial acetic acid are mixed uniformly in a container in a weight ratio of (5-15): (0.5-3.5): (2-7): (3-10): (2-8), ground to form a sticky mixed material, and then gradually calcined, ultrasonically treated in ethanol, hydrothermally reacted, washed with alcohol, and dried. Among them, the oxide additive includes a weather-resistant oxide additive and a passivating oxide additive, the weather-resistant oxide additive is selected from one or both of tetrabutyl titanate and zinc chloride, and the passivating oxide additive is one or more of cerium nitrate hexahydrate, ferric chloride hexahydrate and ferric nitrate nonahydrate. A mesoporous oxide layer is formed on the fly ash using a specific proportion of raw materials, so that the mesoporous oxide layer can have better weathering and passivation properties.
[0054] Step 2, using mesoporous oxide-fly ash filler, water, carbon-based compound and carbon quantum dot dopant as raw materials, loading carbon quantum dots on the mesoporous oxide-fly ash filler through hydrothermal reaction to obtain carbon-based mesoporous oxide-fly ash filler.
[0055] Specifically, in step 2, the mesoporous oxide-fly ash filler, the carbon-based compound, the deionized water and the carbon quantum dot dopant are mixed in the ratio of (5-10):(2-3.5):(6-18):(1.2-3), placed in a reactor for hydrothermal reaction at 130-220° C., and filtered and dried to obtain the carbon-based mesoporous oxide-fly ash filler. The organic carbon layer of the carbon quantum dots is loaded and coated on the mesoporous oxide layer using a specific ratio of raw materials, so that the combination effect of the organic carbon layer and the mesoporous oxide layer is better, and the filler has better corrosion resistance and weather resistance.
[0056] Step 3, reacting the carbon-based mesoporous oxide-fly ash filler with a chemical modifier to obtain an anti-corrosion and weather-resistant functional filler.
[0057] Specifically, the reaction of the carbon-based mesoporous oxide-fly ash filler and the chemical modifier is achieved through one or more of chemical grafting, chemical growth, and physical coating. Specifically, the weight ratio of the carbon-based mesoporous oxide-fly ash filler and the chemical modifier is (1-2):(0.5-1), the carbon-based mesoporous oxide-fly ash filler and the chemical modifier are dispersed in an ethanol aqueous solution, stirred and mixed at 25-80°C, and then subjected to ultrasound, filtration, and drying to obtain an anti-corrosion and weather-resistant functional filler.
[0058] Another specific embodiment of the present invention provides an anti-corrosion and weather-resistant coating, including the above-mentioned anti-corrosion and weather-resistant functional filler.
[0059] Specifically, adding anti-corrosion and weather-resistant functional fillers to the coating can simultaneously improve the anti-corrosion performance and weather resistance of the coating.
[0060] The present invention is further described in detail below in conjunction with specific embodiments.
[0061] Example 1
[0062] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0063] 500 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 5-20 μm, and calcined at 500° C. for 6 hours to obtain fly ash filler.
[0064] 200 parts by weight of fly ash filler, 50 parts by weight of glacial acetic acid, 30 parts by weight of water, 20 parts by weight of tetrabutyl titanate, 40 parts by weight of zinc chloride, 40 parts by weight of cerium nitrate hexahydrate, 10 parts by weight of polyethyleneimine, and 10 parts of polyethylene glycol were placed in a mortar and fully ground for 30 minutes to obtain a gelled product, which was placed in a muffle furnace at 300 degrees Celsius and calcined for 6 hours to obtain a mesoporous oxide-fly ash precursor. Subsequently, ultrasonic treatment and hydrothermal reaction operations were gradually performed in a mixed solution of water and ethanol to obtain a mesoporous oxide-fly ash filler.
[0065] 100 parts by weight of mesoporous oxide-fly ash filler are placed in a beaker, and 50 parts by weight of water, 15 parts by weight of 4-aminosalicylic acid, 20 parts by weight of tartaric acid, 5 parts of chitosan, 10 parts of mercaptosuccinic acid, 40 parts by weight of ethylenediamine, and 10 parts by weight of thiourea are added. After mechanical stirring for 20 minutes, the mixture is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 220°C for 12 hours. After filtering and drying, a carbon-based mesoporous oxide-fly ash filler is obtained.
[0066] Place 50 parts by weight of carbon-based mesoporous oxide-fly ash filler in a beaker, add 100 parts by weight of water, 50 parts by weight of anhydrous ethanol, 10 parts by weight of γ-aminopropyltriethoxysilane, and 10 parts by weight of dopamine hydrochloride, mechanically stir at 50°C for 12 hours, and obtain anti-corrosion and weather-resistant functional filler after filtration.
[0067] Example 2
[0068] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0069] 300 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 0.1-15 μm, and calcined at 1000° C. for 6 hours to obtain fly ash filler.
[0070] 150 parts by weight of fly ash filler, 150 parts by weight of glacial acetic acid, 50 parts by weight of water, 100 parts by weight of cerium nitrate hexahydrate, 30 parts by weight of zinc chloride, 20 parts by weight of tetrabutyl titanate and 80 parts by weight of polyoxyethylene polyoxypropylene ether were placed in a mortar and ground for 60 minutes to obtain a gelled product, which was placed in a muffle furnace at 500°C and calcined for 3 hours to obtain a mesoporous oxide-fly ash precursor. Subsequently, ultrasonic treatment and hydrothermal reaction operations were gradually performed in a mixed solution of water and ethanol to obtain a mesoporous oxide-fly ash filler.
[0071] 150 parts by weight of mesoporous oxide-fly ash filler are placed in a beaker, and 10 parts by weight of water, 40 parts by weight of anhydrous ethanol, 50 parts by weight of citric acid, 50 parts by weight of ascorbic acid, 40 parts by weight of p-phenylenediamine, 10 parts of o-phenylenediamine, and 50 parts by weight of oleylamine are added. After mechanical stirring for 40 minutes, the mixture is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 130 degrees Celsius for 36 hours. After filtering and drying, a carbon-based mesoporous oxide-fly ash filler is obtained.
[0072] 150 parts by weight of carbon-based mesoporous oxide-fly ash filler were placed in a beaker, 300 parts by weight of water, 25 parts by weight of trichlorovinyl silane, and 25 parts by weight of ethyl α-cyanoacrylate were added, mechanically stirred at 80° C. for 12 hours, and the anti-corrosion and weather-resistant functional filler was obtained after filtration.
[0073] Example 3
[0074] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0075] 500 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 5-20 μm, and calcined at 500° C. for 6 hours to obtain fly ash filler.
[0076] 200 parts by weight of fly ash filler, 50 parts by weight of glacial acetic acid, 30 parts by weight of water, 20 parts by weight of tetrabutyl titanate, 20 parts by weight of ferric chloride hexahydrate, 40 parts by weight of zinc chloride, 20 parts by weight of ferric nitrate nonahydrate, 10 parts by weight of polyethyleneimine, and 10 parts of polyethylene glycol were placed in a mortar and fully ground for 30 minutes to obtain a gelled product, which was placed in a muffle furnace at 300 degrees Celsius and calcined for 6 hours to obtain a mesoporous oxide-fly ash precursor. Subsequently, ultrasonic treatment and hydrothermal reaction operations were gradually performed in a mixed solution of water and ethanol to obtain a mesoporous oxide-fly ash filler.
[0077] 100 parts by weight of mesoporous oxide-fly ash filler are placed in a beaker, and 50 parts by weight of water, 15 parts by weight of 4-aminosalicylic acid, 20 parts by weight of tartaric acid, 5 parts of chitosan, 10 parts of mercaptosuccinic acid, 40 parts by weight of ethylenediamine, and 10 parts by weight of thiourea are added. After mechanical stirring for 20 minutes, the mixture is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 220°C for 12 hours. After filtering and drying, a carbon-based mesoporous oxide-fly ash filler is obtained.
[0078] Place 50 parts by weight of carbon-based mesoporous oxide-fly ash filler in a beaker, add 100 parts by weight of water, 50 parts by weight of anhydrous ethanol, 10 parts by weight of γ-aminopropyltriethoxysilane, and 10 parts by weight of dopamine hydrochloride, mechanically stir at 50°C for 12 hours, and obtain anti-corrosion and weather-resistant functional filler after filtration.
[0079] Example 4
[0080] The only difference between this embodiment and embodiment 2 is that the amount of tetrabutyl titanate used is 27 parts by weight, the amount of zinc chloride used is 40 parts by weight, and the amount of cerium nitrate hexahydrate used is 83 parts by weight.
[0081] Example 5
[0082] The only difference between this embodiment and embodiment 2 is that the amount of tetrabutyl titanate used is 35 parts by weight, the amount of zinc chloride used is 40 parts by weight, and the amount of cerium nitrate hexahydrate used is 75 parts by weight.
[0083] Example 6
[0084] The only difference between this embodiment and embodiment 2 is that the amount of tetrabutyl titanate used is 40 parts by weight, the amount of zinc chloride used is 60 parts by weight, and the amount of cerium nitrate hexahydrate used is 50 parts by weight.
[0085] Example 7
[0086] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0087] 300 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 0.1-15 μm, and calcined at 1000° C. for 6 hours to obtain fly ash filler.
[0088] 200 parts by weight of fly ash filler, 80 parts by weight of glacial acetic acid, 20 parts by weight of water, 80 parts by weight of cerium nitrate hexahydrate, 24 parts by weight of zinc chloride, 16 parts of tetrabutyl titanate and 80 parts by weight of polyoxyethylene polyoxypropylene ether were placed in a mortar and ground for 60 minutes to obtain a gelled product, which was placed in a muffle furnace at 500°C and calcined for 3 hours to obtain a mesoporous oxide-fly ash precursor. Subsequently, ultrasonic treatment and hydrothermal reaction operations were gradually performed in a mixed solution of water and ethanol to obtain a mesoporous oxide-fly ash filler.
[0089] 150 parts by weight of mesoporous oxide-fly ash filler are placed in a beaker, and 10 parts by weight of water, 40 parts by weight of anhydrous ethanol, 50 parts by weight of citric acid, 50 parts by weight of ascorbic acid, 40 parts by weight of p-phenylenediamine, 10 parts of o-phenylenediamine, and 50 parts by weight of oleylamine are added. After mechanical stirring for 40 minutes, the mixture is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 130 degrees Celsius for 36 hours. After filtering and drying, a carbon-based mesoporous oxide-fly ash filler is obtained.
[0090] 150 parts by weight of carbon-based mesoporous oxide-fly ash filler were placed in a beaker, 300 parts by weight of water, 25 parts by weight of trichlorovinyl silane, and 25 parts by weight of ethyl α-cyanoacrylate were added, mechanically stirred at 80° C. for 12 hours, and the anti-corrosion and weather-resistant functional filler was obtained after filtration.
[0091] Example 8
[0092] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0093] 300 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 0.1-15 μm, and calcined at 1000° C. for 6 hours to obtain fly ash filler.
[0094] 150 parts by weight of fly ash filler, 150 parts by weight of glacial acetic acid, 50 parts by weight of water, 100 parts by weight of cerium nitrate hexahydrate, 30 parts by weight of zinc chloride, 20 parts by weight of tetrabutyl titanate and 80 parts by weight of polyoxyethylene polyoxypropylene ether were placed in a mortar and ground for 60 minutes to obtain a gelled product, which was placed in a muffle furnace at 500°C and calcined for 3 hours to obtain a mesoporous oxide-fly ash precursor. Subsequently, ultrasonic treatment and hydrothermal reaction operations were gradually performed in a mixed solution of water and ethanol to obtain a mesoporous oxide-fly ash filler.
[0095] 250 parts by weight of the mesoporous oxide-fly ash filler prepared by the above method is placed in a beaker, and 300 parts by weight of water, 40 parts by weight of anhydrous ethanol, 50 parts by weight of citric acid, 50 parts by weight of ascorbic acid, 24 parts by weight of p-phenylenediamine, 6 parts of o-phenylenediamine, and 30 parts by weight of oleylamine are added. After mechanical stirring for 40 minutes, it is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 130 degrees Celsius for 36 hours. After filtering and drying, a carbon-based mesoporous oxide-fly ash filler is obtained.
[0096] 150 parts by weight of carbon-based mesoporous oxide-fly ash filler were placed in a beaker, 300 parts by weight of water, 25 parts by weight of trichlorovinyl silane, and 25 parts by weight of ethyl α-cyanoacrylate were added, mechanically stirred at 80° C. for 12 hours, and the anti-corrosion and weather-resistant functional filler was obtained after filtration.
[0097] Example 9
[0098] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0099] 300 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 0.1-15 μm, and calcined at 1000° C. for 6 hours to obtain fly ash filler.
[0100] 150 parts by weight of fly ash filler, 150 parts by weight of glacial acetic acid, 50 parts by weight of water, 100 parts by weight of cerium nitrate hexahydrate, 30 parts by weight of zinc chloride, 20 parts by weight of tetrabutyl titanate and 80 parts by weight of polyoxyethylene polyoxypropylene ether were placed in a mortar and ground for 60 minutes to obtain a gelled product, which was placed in a muffle furnace at 500°C and calcined for 3 hours to obtain a mesoporous oxide-fly ash precursor. Subsequently, ultrasonic treatment and hydrothermal reaction operations were gradually performed in a mixed solution of water and ethanol to obtain a mesoporous oxide-fly ash filler.
[0101] 250 parts by weight of the mesoporous oxide-fly ash filler prepared by the above method is placed in a beaker, and 10 parts by weight of water, 40 parts by weight of anhydrous ethanol, 25 parts by weight of citric acid, 25 parts by weight of ascorbic acid, 37.5 parts by weight of p-phenylenediamine, 7.5 parts of o-phenylenediamine, and 30 parts by weight of oleylamine are added. After mechanical stirring for 40 minutes, it is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 130 degrees Celsius for 36 hours. After filtering and drying, a carbon-based mesoporous oxide-fly ash filler is obtained.
[0102] 150 parts by weight of carbon-based mesoporous oxide-fly ash filler were placed in a beaker, 300 parts by weight of water, 25 parts by weight of trichlorovinyl silane, and 25 parts by weight of ethyl α-cyanoacrylate were added, mechanically stirred at 80° C. for 12 hours, and the anti-corrosion and weather-resistant functional filler was obtained after filtration.
[0103] Example 10
[0104] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0105] 300 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 0.1-15 μm, and calcined at 1000° C. for 6 hours to obtain fly ash filler.
[0106] 150 parts by weight of fly ash filler, 150 parts by weight of glacial acetic acid, 50 parts by weight of water, 100 parts by weight of cerium nitrate hexahydrate, 50 parts by weight of tetrabutyl titanate and 80 parts by weight of polyoxyethylene polyoxypropylene ether were placed in a mortar and ground for 60 minutes to obtain a gelled product, which was placed in a muffle furnace at 500°C and calcined for 3 hours to obtain a mesoporous oxide-fly ash precursor. Subsequently, ultrasonic treatment and hydrothermal reaction operations were gradually performed in a mixed solution of water and ethanol to obtain a mesoporous oxide-fly ash filler.
[0107] 150 parts by weight of mesoporous oxide-fly ash filler are placed in a beaker, and 10 parts by weight of water, 40 parts by weight of anhydrous ethanol, 50 parts by weight of citric acid, 50 parts by weight of ascorbic acid, 40 parts by weight of p-phenylenediamine, 10 parts of o-phenylenediamine, and 50 parts by weight of oleylamine are added. After mechanical stirring for 40 minutes, the mixture is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 130 degrees Celsius for 36 hours. After filtering and drying, a carbon-based mesoporous oxide-fly ash filler is obtained.
[0108] 150 parts by weight of carbon-based mesoporous oxide-fly ash filler were placed in a beaker, 300 parts by weight of water, 25 parts by weight of trichlorovinyl silane, and 25 parts by weight of ethyl α-cyanoacrylate were added, mechanically stirred at 80° C. for 12 hours, and the anti-corrosion and weather-resistant functional filler was obtained after filtration.
[0109] Embodiment 11
[0110] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0111] 500 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 5-20 μm, and calcined at 500° C. for 6 hours to obtain fly ash filler.
[0112] 200 parts by weight of fly ash filler, 50 parts by weight of glacial acetic acid, 30 parts by weight of water, 20 parts by weight of tetrabutyl titanate, 40 parts by weight of zinc chloride, 40 parts by weight of cerium nitrate hexahydrate, 10 parts by weight of polyethyleneimine, and 10 parts of polyethylene glycol were placed in a mortar and fully ground for 30 minutes to obtain a gelled product, which was placed in a muffle furnace at 300 degrees Celsius and calcined for 6 hours to obtain a mesoporous oxide-fly ash precursor. Subsequently, ultrasonic treatment and hydrothermal reaction operations were gradually performed in a mixed solution of water and ethanol to obtain a mesoporous oxide-fly ash filler.
[0113] 100 parts by weight of mesoporous oxide-fly ash filler are placed in a beaker, and 50 parts by weight of water, 15 parts by weight of 4-aminosalicylic acid, 20 parts by weight of tartaric acid, 5 parts of chitosan, and 10 parts of mercaptosuccinic acid are added. After mechanical stirring for 20 minutes, the mixture is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 220°C for 12 hours. After filtering and drying, a carbon-based mesoporous oxide-fly ash filler precursor is obtained.
[0114] 100 parts by weight of carbon-based mesoporous oxide-fly ash filler precursor, 40 parts by weight of ethylenediamine, and 10 parts by weight of thiourea are placed in a beaker, 50 parts by weight of water are added, and after mechanical stirring for 30 minutes, the mixture is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 220°C for 6 hours. After filtering and drying, a carbon-based mesoporous oxide-fly ash filler is obtained.
[0115] Place 50 parts by weight of carbon-based mesoporous oxide-fly ash filler in a beaker, add 100 parts by weight of water, 50 parts by weight of anhydrous ethanol, 10 parts by weight of γ-aminopropyltriethoxysilane, and 10 parts by weight of dopamine hydrochloride, mechanically stir at 50°C for 12 hours, and obtain anti-corrosion and weather-resistant functional filler after filtration.
[0116] Comparative Example 1
[0117] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0118] 500 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 5-20 μm, and calcined at 500° C. for 6 hours to obtain fly ash filler.
[0119] 100 parts by weight of fly ash filler are placed in a beaker, and 50 parts by weight of water, 15 parts by weight of 4-aminosalicylic acid, 20 parts by weight of tartaric acid, 5 parts of chitosan, 10 parts of mercaptosuccinic acid, 40 parts by weight of ethylenediamine, and 10 parts by weight of thiourea are added. After mechanical stirring for 20 minutes, the mixture is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 220°C for 12 hours. After filtering and drying, a carbon-based fly ash filler is obtained.
[0120] Place 50 parts by weight of carbon-based fly ash filler in a beaker, add 100 parts by weight of water, 50 parts by weight of anhydrous ethanol, 10 parts by weight of γ-aminopropyltriethoxysilane, and 10 parts by weight of dopamine hydrochloride, mechanically stir at 50°C for 12 hours, and obtain anti-corrosion and weather-resistant functional filler after filtration.
[0121] Comparative Example 2
[0122] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0123] 500 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 5-20 μm, and calcined at 500° C. for 6 hours to obtain fly ash filler.
[0124] 200 parts by weight of fly ash filler, 50 parts by weight of glacial acetic acid, 30 parts by weight of water, 20 parts by weight of tetrabutyl titanate, 40 parts by weight of zinc chloride, 40 parts by weight of cerium nitrate hexahydrate, 10 parts by weight of polyethyleneimine, and 10 parts of polyethylene glycol were placed in a mortar and fully ground for 30 minutes to obtain a gelled product, which was placed in a muffle furnace at 300 degrees Celsius and calcined for 6 hours to obtain a mesoporous oxide-fly ash precursor. Subsequently, ultrasonic treatment and hydrothermal reaction operations were gradually performed in a mixed solution of water and ethanol to obtain a mesoporous oxide-fly ash filler.
[0125] Place 50 parts by weight of mesoporous oxide-fly ash filler in a beaker, add 100 parts by weight of water, 50 parts by weight of anhydrous ethanol, 10 parts by weight of γ-aminopropyltriethoxysilane, and 10 parts by weight of dopamine hydrochloride, mechanically stir at 50°C for 12 hours, and obtain anti-corrosion and weather-resistant functional filler after filtration.
[0126] Comparative Example 3
[0127] An anti-corrosion and weather-resistant functional filler is prepared by the following scheme:
[0128] 300 parts by weight of solid waste fly ash were placed in a ball mill and ground for 12 hours, then placed in a cyclone separator to screen fly ash with a particle size of 0.1-15 μm, and calcined at 1000° C. for 6 hours to obtain fly ash filler.
[0129] 150 parts by weight of fly ash filler, 150 parts by weight of glacial acetic acid, 50 parts by weight of water, 100 parts by weight of cerium nitrate hexahydrate, 30 parts by weight of zinc chloride and 20 parts of tetrabutyl titanate were placed in a mortar and fully ground for 60 minutes to obtain a mixture, which was placed in a muffle furnace at 500°C and calcined for up to 3 hours to obtain an oxide-fly ash precursor. Subsequently, ultrasonic treatment and hydrothermal reaction operations were gradually performed in a mixed solution of water and ethanol to obtain an oxide-fly ash filler.
[0130] 150 parts by weight of oxide-fly ash filler are placed in a beaker, and 10 parts by weight of water, 40 parts by weight of anhydrous ethanol, 50 parts by weight of citric acid, 50 parts by weight of ascorbic acid, 40 parts by weight of p-phenylenediamine, 10 parts of o-phenylenediamine, and 50 parts by weight of oleylamine are added. After mechanical stirring for 40 minutes, the mixture is placed in a hydrothermal reactor and subjected to a hydrothermal reaction at 130 degrees Celsius for 36 hours. After filtering and drying, a carbon-based oxide-fly ash filler is obtained.
[0131] 150 parts by weight of carbon-based oxide-fly ash filler are placed in a beaker, 300 parts by weight of water, 25 parts by weight of trichlorovinyl silane, and 25 parts by weight of ethyl α-cyanoacrylate are added, mechanically stirred at 80° C. for 12 hours, and the anti-corrosion and weather-resistant functional filler is obtained after filtration.
[0132] Comparative Example 4
[0133] The only difference between this comparative example and Example 10 is that tetrabutyl titanate is replaced by an equal amount of cerium nitrate hexahydrate.
[0134] Comparative Example 5
[0135] The difference between this comparative example and Example 10 is that the cerium nitrate hexahydrate is replaced by an equal amount of tetrabutyl titanate.
[0136] The anti-corrosion and weather-resistant functional fillers in the above-mentioned embodiments and comparative examples are prepared by the following scheme when preparing anti-corrosion and weather-resistant coatings: 50 parts by weight of epoxy resin, 30 parts by weight of polyamide, 15 parts by weight of xylene, and 15 parts by weight of acetone are mixed evenly using a high-speed disperser, 20 parts by weight of anti-corrosion and weather-resistant functional fillers are added thereto, stirred evenly, and the coating is sprayed on the surface of the metal substrate by an air pump spraying method, and a coating is formed after curing.
[0137] Performance Test:
[0138] (1) Anticorrosion Test: The coating samples formed in each embodiment and each comparative example were placed in a 3.5% NaCl solution for electrochemical impedance spectroscopy (EIS) test. The coating was tested by electrochemical impedance spectroscopy using a three-electrode system. The test frequency range was 100 kHz to 0.01 Hz. A 20 mV sinusoidal perturbation signal was applied to the sample. The test area of the sample was 7.069 cm 2 The main test data are shown in Table 1. The EIS test results after immersion in 3.5% NaCl solution for 60 days are shown in Figure 1 shown.
[0139] Table 1 EIS test data
[0140]
[0141] (2) Conventional performance test: The adhesion of the samples was tested by the pull-off method and the cross-cut test; the samples were subjected to weathering test using a xenon lamp test chamber, where the relative humidity in the chamber was maintained at 50% and the ultraviolet range of the xenon lamp was set to 340nm. The conventional performance test data are shown in Table 2. The changes in the water contact angle of the samples after the xenon lamp weathering test are shown in Table 2. Figure 2 shown.
[0142] Table 2 Conventional performance test data
[0143]
[0144] Referring to Table 1 and Table 2, we can draw the following conclusions:
[0145] (1) The samples of Example 1 and Example 2 exhibited higher impedance moduli at low frequencies, with values of 3.32×10 11 Ω·cm 2 and 3.55×10 11 Ω·cm 2 The higher impedance modulus indicates that the anti-corrosion coating has excellent shielding performance against corrosive media, and the functional composite filler with a specific structure effectively blocks the corrosive media.
[0146] The samples of Comparative Example 1 and Comparative Example 2 exhibit relatively low impedance moduli at low frequencies, and their values are 2.76×10 10 Ω·cm 2 and 2.04×10 11 Ω·cm 2 In comparison, the low-frequency impedance modulus of the sample in Comparative Example 1 is smaller, which indicates that the mesoporous structure in Examples 1 and 2 contributes to the uniform distribution of the carbon structure, which is beneficial to improving the anti-corrosion performance of the coating. For Comparative Example 2, although the sample exhibits a higher impedance modulus, there is an obvious upward trend in the high-frequency region of the Bode angle diagram ( Figure 1 (d)), that is, the sample exhibits two time constants, which indicates that stratification behavior occurs inside the sample, which is very unfavorable for corrosion protection.
[0147] In the EIS test results, the Nyquist plots of different samples also have certain differences, among which the capacitive reactance arc radius of comparative example 1 is the smallest ( Figure 1 (b)), which indicates that the coating has a certain amount of water absorption, which is very unfavorable for corrosion. This behavior also shows that the internal dispersion of the material is poor, indicating that the organic carbon layer can appropriately improve the bonding between the filler and the coating interface.
[0148] As can be seen from Table 2, the adhesion of Comparative Examples 1 and 2 to the substrate is poor, which is caused by the uneven distribution of fillers inside the coating. In Comparative Example 1, there is no mesoporous structure in the functional filler, which reduces the dispersion of the filler, which leads to a decrease in the shielding performance of the coating, and a decrease in the neutral salt spray resistance time and the xenon lamp resistance test time. In Comparative Example 2, there is no organic carbon layer containing carbon quantum dots in the filler, which reduces the interfacial behavior between the filler and the resin matrix. The compatibility of the mesoporous filler and the resin matrix is poor, resulting in a significant decrease in the adhesion of the sample. In the pull-off adhesion strength test, the adhesion is only 5.17MPa, and in the cross-grid test adhesion test, the adhesion grade of the sample is level 3. However, the xenon lamp resistance test time performance of the sample in Comparative Example 2 is not bad, and it can withstand 500 hours of xenon lamp resistance test, which also shows that the mesoporous oxide layer gives the coating certain weather resistance.
[0149] (2) The coating samples of Example 1, Comparative Example 1 and Comparative Example 2 were subjected to a xenon lamp aging resistance test, and then the contact angle of the coating surface was tested to analyze the degree of damage to the coating caused by the xenon lamp.
[0150] The initial water contact angle of the sample in Example 1 after xenon lamp testing was 84.68° ( Figure 2 (a)), as the standing time increases to 100 seconds, the water contact angle decreases to 76.56°, and the water contact angle decreases by 8.12° within 100 seconds. The initial water contact angle and water absorption rate of the sample are moderate.
[0151] The initial water contact angle of the sample in Comparative Example 1 after xenon lamp test was 63.24° ( Figure 2 (b)), the initial water contact angle is low, and as the standing time is extended to 100 seconds, the water contact angle decreases to 54.93°, and the water contact angle decreases by 8.31° within 100 seconds. The degree of decrease in the water contact angle of the sample in Comparative Example 1 is close to that of the sample in Example 1, which shows that the water absorption rate of the coating is similar. The low initial angle may be caused by the damage of the xenon lamp to the coating. The sample in Comparative Example 1 does not have a mesoporous oxide layer and has no obvious resistance to the xenon lamp aging test.
[0152] The initial water contact angle of the sample in Comparative Example 2 after the xenon lamp test was 109.79°, which was significantly higher than that of other samples. This may be caused by the photocatalytic reaction of the mesoporous oxide component during the xenon lamp test. As the standing time was extended to 100 seconds, the water contact angle of the sample decreased to 76.56°, and the water contact angle decreased by 33.23° within 100 seconds, indicating that the coating absorbed water seriously and there were obvious defects on the coating surface. The filler in Comparative Example 2 did not contain an organic carbon layer containing carbon quantum dots. The reason for the poor performance may be the poor interfacial cross-linking performance between the filler and the resin.
[0153] (3) The mesoporous structure of the oxide layer is the key factor affecting the coating performance. Figure 3 The microstructure of the mesoporous oxide in Example 2 and Comparative Example 2 is shown. With the help of the carbon layer, the mesoporous morphology of the sample is more obvious, which is conducive to the coating exhibiting better properties.
[0154] The oxide provides excellent weather resistance or anti-corrosion performance, and the mesoporous structure can give the filler excellent transmission channels and active sites. The low-frequency impedance modulus of the EIS test of the sample in comparative example 3 is only 2.48×10 7 Ω·cm 2 , which is 4 orders of magnitude lower than the value of the sample in Example 1, indicating that the pore defects inside the coating are serious, which destroys the anti-corrosion performance of the coating sample. In addition, the xenon lamp resistance time of the sample in Comparative Example 3 is also 600 hours lower than that of the sample in Example 1, which indicates that the mesoporous morphology of the oxide layer is conducive to the filler to exert the corresponding functionality. The photocatalytic effect on the surface of the weather-resistant filler can easily cause the decomposition of the coating resin matrix and reduce the anti-corrosion performance of the coating. Therefore, it is difficult to improve the weather resistance and anti-corrosion performance at the same time in the system. The present invention cleverly utilizes the coating effect of the mesoporous structure and the organic carbon layer containing carbon quantum dots to enhance the effect of the weather-resistant filler and reduce the destructive behavior of the weather-resistant filler on the coating.
[0155] (4) The mesoporous oxide layer structure does not contain only one oxide, nor is it a combination of multiple single oxides. Instead, it is a heterogeneous structure with a doped morphology, which has excellent oxygen transport function. The oxygen transport performance can enhance the role of the weathering unit in the mesoporous structure, quickly transport the oxygen on the surface of the sample to the mesoporous structure, and enhance the weathering performance of the filler. The difference in this property can be seen from Example 10, Comparative Example 4 and Comparative Example 5. Comparative Example 4 is a carbon-based mesoporous CeO2-fly ash filler, which has not been doped with Ti atoms. Although the mesoporous CeO2 structure has a larger pore structure, it has no oxygen transport function, which reduces the anti-corrosion passivation performance of the Ce element on the metal substrate. From the results, the low-frequency impedance modulus in the EIS test of Comparative Example 4 is one order of magnitude lower than the low-frequency impedance modulus of the sample in Example 10.
[0156] It can be seen from the xenon lamp resistance time of Example 10 and Comparative Example 5 that the xenon lamp resistance time of the carbon-based mesoporous TiO2-fly ash coating without Ce atom doping is only 350 hours, which indicates that the lack of doping promotes the photocatalytic process on the filler surface and has an adverse effect on the coating.
[0157] (5) The organic carbon layer coating is very beneficial to the interfacial bonding performance between the mesoporous oxide-fly ash filler and the resin matrix. The carbon layer prepared on the mesoporous oxide layer is enriched in carbon quantum dots in the form of N-atom doping, which has a strong affinity for the interface of the resin matrix. In addition, it is also very beneficial to the passivation behavior of the metal substrate.
[0158] In Example 1, the organic carbon layer and the carbon quantum dots doped with N atoms are synthesized in one step into the mesoporous oxide-fly ash filler, and the carbon quantum dots are mainly enriched in the outer layer of the filler, which can effectively enhance the bonding behavior of the carbon layer and the resin matrix, and also greatly reduce the decomposition effect of the weather-resistant filler on the interface. In Example 11, the organic carbon layer and the carbon quantum dots are gradually prepared in the functional filler, and the carbon quantum dots are doped in large quantities in the mesoporous structure, which hinders the release of the carbon quantum dots themselves to the metal substrate, and also reduces the role of the weather-resistant filler. From the results, the EIS test and the neutral salt spray resistance test performance of Example 1 are good, which also proves this effect. In addition, the adhesion strength of the pull-off method of Example 1 and Example 2 is higher than the adhesion strength of the sample of Example 11 (the adhesion of the sample of Comparative Example 6 is 7.15MPa), which also illustrates the difference in the interfacial bonding performance of the components inside the coating. Therefore, considering comprehensively, the one-step preparation of the carbon-based mesoporous oxide-fly ash filler by hydrothermal reaction in Example 1 is more conducive to the anti-corrosion and weathering effect of the filler.
[0159] (6) The compounding ratio of the weather-resistant oxide additive and the passivating oxide additive will affect the effect of the filler. In combination with Example 2 and Examples 4-6, it can be seen that compounding the weather-resistant oxide additive and the passivating oxide additive in the weight ratio of 1: (0.8-2) disclosed in the present invention helps the filler to enhance the anti-corrosion and weathering effect of the coating while reducing the adverse effects caused by the photocatalytic effect.
[0160] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0161] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. Anti-corrosion and weather-resistant functional filler, characterized in that: It comprises fly ash, the fly ash is coated with a mesoporous oxide layer, and the mesoporous oxide layer is coated with a heteroatom-doped carbon quantum dot organic carbon layer; The mesoporous oxide layer includes a weather-resistant element and a passivation element. The weather-resistant element is one or both of titanium and zinc, and the passivation element is one or more of cerium and iron.
2. The anticorrosion and weather-resistant functional filler according to claim 1, characterized in that: The raw materials include, by weight: 200-400 parts of fly ash, 20-80 parts of porogen, 100-150 parts of oxide additive, 50-100 parts of carbon-based compound, 50-100 parts of carbon quantum dopant, 20-50 parts of chemical modifier and 50-150 parts of glacial acetic acid; Among them, the oxide additives include weather-resistant oxide additives and passivating oxide additives, the weather-resistant oxide additives are one or two of tetrabutyl titanate and zinc chloride; the passivating oxide additives are one or more of cerium nitrate hexahydrate, ferric chloride hexahydrate and ferric nitrate nonahydrate.
3. The anticorrosion and weather-resistant functional filler according to claim 2, characterized in that: The porogen is selected from one or more of polyoxyethylene polyoxypropylene ether, polyethylene imine, and polyethylene glycol; And / or, the carbon-based compound is selected from one or more of 4-aminosalicylic acid, citric acid, tartaric acid, ascorbic acid, mercaptosuccinic acid, and chitosan; And / or, the carbon quantum dot dopant is selected from one or more of thiourea, ethylenediamine, p-phenylenediamine, o-phenylenediamine, and oleylamine; And / or, the chemical modifier is selected from one or more of γ-aminopropyltriethoxysilane, trichlorovinylsilane, α-ethyl cyanoacrylate, and dopamine hydrochloride.
4. The anticorrosion and weather-resistant functional filler according to claim 2, characterized in that: The weight ratio of the weather-resistant oxide additive to the passivating oxide additive is 1:(0.8-2).
5. The method for preparing the anticorrosive and weather-resistant functional filler according to any one of claims 1 to 4, characterized in that: The following steps are involved: Using fly ash, water, porogen, oxide additive and glacial acetic acid as raw materials, a mesoporous oxide layer is coated on the fly ash to obtain a mesoporous oxide-fly ash filler; wherein the oxide additive comprises a weather-resistant oxide additive and a passivating oxide additive, the weather-resistant oxide additive makes the mesoporous oxide layer include titanium and / or zinc, and the passivating oxide additive makes the mesoporous oxide layer include cerium and / or iron; Using mesoporous oxide-fly ash filler, water, carbon-based compound and carbon quantum dot dopant as raw materials, carbon quantum dots are loaded on the mesoporous oxide-fly ash filler to obtain carbon-based mesoporous oxide-fly ash filler; The carbon-based mesoporous oxide-fly ash filler is reacted with a chemical modifier to obtain an anti-corrosion and weather-resistant functional filler.
6. The method for preparing the anticorrosive and weather-resistant functional filler according to claim 5, characterized in that: The mesoporous oxide-fly ash filler is prepared by a one-pot calcination method, specifically, fly ash, water, porogen, oxide additive and glacial acetic acid are mixed, ground to form a sticky mixed material, and then calcined, ultrasonicated, hydrothermally reacted, washed with alcohol, and dried to obtain; And / or, when preparing the mesoporous oxide-fly ash filler, the weight ratio of fly ash, water, porogen, oxide additive and glacial acetic acid is (5-15):(0.5-3.5):(2-7):(3-10):(2-8); And / or, when preparing carbon-based mesoporous oxide-fly ash filler, the weight ratio of mesoporous oxide-fly ash filler, carbon-based compound, water and carbon quantum dot dopant is (5-10):(2-3.5):(6-18):(1.2-3).
7. The method for preparing the anticorrosive and weather-resistant functional filler according to claim 5, characterized in that: The carbon-based mesoporous oxide-fly ash filler is prepared by hydrothermal reaction, and the hydrothermal reaction temperature is 130-220°C.
8. The method for preparing the anticorrosive and weather-resistant functional filler according to claim 5, characterized in that: The carbon-based mesoporous oxide-fly ash filler and the chemical modifier are dispersed in an ethanol aqueous solution, stirred and mixed at 25-80° C., and then subjected to ultrasonic treatment, suction filtration and drying to obtain an anti-corrosion and weather-resistant functional filler.
9. The method for preparing the anticorrosive and weather-resistant functional filler according to claim 5, characterized in that: The weight ratio of the carbon-based mesoporous oxide-fly ash filler to the chemical modifier is (1-2):(0.5-1). 10.Anti-corrosion and weather-resistant coating, characterized in that: It comprises the anti-corrosion and weather-resistant functional filler as described in any one of claims 1 to 4.
Citation Information
Patent Citations
Double-coated hollow glass microbead heat-insulated coating and preparation method thereof
CN102391754A
Interior wall heat insulation coating
CN103013260A
Seawater resistant graphene modified anticorrosive paint and preparation method thereof
CN108531038A
Wear-resistant corrosion-inhibition powder functional filler, powder coating and preparation method thereof
CN116042014A
Method for coating article and feedstock for thermal spray process
US20180112303A1
Cited By
Multi-effect corrosion-inhibition functional anticorrosive filler, preparation method and multi-effect corrosion-inhibition anticorrosive coating
CN119552529A