Rock wool-based multifunctional water-based paint and preparation method thereof
By using rock wool powder and fly ash as fillers, combined with water-based styrene-acrylic emulsion and carboxylated styrene-butadiene emulsion, a multi-functional water-based coating is prepared, which solves the deficiencies in thermal insulation and hydrophobic properties of exterior wall coatings, reduces costs, and achieves Improved low thermal conductivity and hydrophobic properties.
Patent Information
- Application Number
- CN202410965275.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing exterior wall coatings have not yet been able to effectively balance environmental protection, waterproofing and heat insulation in terms of performance, and the problems of low thermal conductivity and high-cost nanofillers of rock wool solid waste have not been effectively solved.
Rock wool powder and fly ash are used as fillers, combined with water-based styrene-acrylic emulsion and carboxyl styrene-butadiene emulsion, and a multi-functional water-based coating is prepared through a high-speed disperser to form a coating with low thermal conductivity and hydrophobic properties. Paraffin microemulsion is used to replace high-cost Nanofillers reduce costs.
It achieves thermal insulation performance with low thermal conductivity of 0.069-0.108W/(m·K) and hydrophobic performance of 139.6-157.2°, reducing coating costs, and the coating has long-term waterproof performance and high adhesion.
Smart Images

Figure CN118772702A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of exterior wall coatings, and in particular to a rock wool-based multifunctional water-based coating and a preparation method thereof. Background Art
[0002] Exterior wall paint was originally used for building decoration, but with the development of science and technology, people's performance requirements for exterior wall paint are not just to beautify the building, but also to take into account environmental protection, waterproof and heat insulation properties.
[0003] In the process of producing exterior wall rock wool insulation boards, basalt rock wool powder waste is generated, which needs to be treated for environmental protection, which is time-consuming and labor-intensive and causes energy waste. In addition, rock wool insulation boards will become waste after a certain number of years, causing environmental pollution and waste of resources, and corresponding methods are needed to recycle the waste. However, there is no suitable treatment method at present. Therefore, it is extremely important to recycle rock wool solid waste.
[0004] A lot of research has been done on fly ash-based coatings (CN 116333519 B), but there are few reports on rock wool-based hydrophobic and heat-insulating exterior wall coatings. Although there are many formulas for exterior wall coatings, the fillers use nanofillers such as silicon-based / titanium-based, and fluorine-containing / fluorine-free silanes as low surface energy substances, which are expensive (CN 111154357B; CN 115895372 B). In addition, the room-temperature film-forming, safety and environmental protection, hydrophobicity, anti-fouling and heat-insulating properties of hydrophobic and heat-insulating exterior wall coatings need to be improved. More importantly, the low thermal conductivity of rock wool solid waste (0.035-0.044W / (m·K)) makes it a good way to use it as a filler for exterior wall coatings. Therefore, it is necessary to use rock wool waste to develop a rock wool-based multifunctional water-based coating. Summary of the invention
[0005] The present application provides a rock wool-based multifunctional water-based paint and a preparation method thereof, so as to solve the rock wool solid waste problem and improve the performance of exterior wall paint, so that the coating has excellent hydrophobic, anti-fouling and thermal insulation properties.
[0006] The present application provides a rock wool-based multifunctional water-based coating, which comprises a component A and a component B, wherein the component A comprises, by weight, 120-150 parts of styrene acrylic emulsion, 20-30 parts of carboxylated styrene butadiene emulsion, 40-55 parts of paraffin microemulsion, 15-25 parts of cellulose thickener, 2-8 parts of defoamer, 20-30 parts of fly ash, 40-60 parts of rock wool powder, and 140-150 parts of deionized water; the component B comprises, by weight, 20-30 parts of styrene acrylic emulsion, 1-3 parts of cross-linking agent, 5-15 parts of paraffin microemulsion, 1-5 parts of defoamer, 5-10 parts of fly ash, 10-20 parts of rock wool powder, and 40-50 parts of deionized water;
[0007] Among them, styrene acrylic emulsion has good adhesion, transparent film, good aging resistance, and can form film at room temperature; carboxylated styrene butadiene emulsion can undergo chemical reactions to improve coating adhesion, water resistance and hardness; paraffin microemulsion is acid-resistant, alkali-resistant, highly water-soluble, and emulsion-stable, and can be diluted with water in any proportion without stratification or demulsification, has a high solid content, and good dispersibility; cellulose thickener increases the viscosity or consistency of the coating, and has the advantages of small dosage, obvious thickening, and easy use; defoaming agent has good heat resistance, good diffusivity, good permeability, stable chemical properties, and strong oxidation resistance; aziridine crosslinker can be cured with carboxylated styrene butadiene emulsion at room temperature.
[0008] Preferably, in the component A, the concentration of styrene acrylic emulsion is 45-50wt%, the concentration of carboxylated styrene butadiene emulsion is 35-40wt%, and the concentration of paraffin microemulsion is 30±1wt%.
[0009] Preferably, the concentration of styrene acrylic emulsion in component B is 45-50wt%, and the concentration of paraffin microemulsion is 30±1wt%.
[0010] Preferably, the pH values of the styrene acrylic emulsion, carboxylated styrene butadiene emulsion and paraffin microemulsion in the component A are 7-8; the rock wool powder is in a fiber shape; and the fly ash is spherical, and the particle size is 8-40 μm.
[0011] Preferably, the crosslinking agent in the component B is a tetrafunctional aziridine crosslinking agent or a trifunctional aziridine crosslinking agent, and the concentration is 99±0.2 wt %.
[0012] Preferably, the preparation method comprises the following steps:
[0013] (1) Preparation of component A:
[0014] a. First, disperse deionized water, fly ash and rock wool powder through a high-speed disperser for 10-20 minutes to obtain a filler suspension of component A, and then adjust the speed of the high-speed disperser;
[0015] b. Slowly add styrene acrylic emulsion into the filler suspension of component A and disperse for 30-40 minutes to obtain a preliminary suspension of component A;
[0016] c. Next, disperse the cellulose thickener and the preliminary suspension of component A for 15-20 minutes, and then add the paraffin microemulsion and disperse it in a high-speed disperser for 10-30 minutes;
[0017] d. Finally, add carboxylated styrene butadiene emulsion to disperse in the suspension obtained in the above step, and slowly add defoamer during the dispersion process, disperse for 20-30 minutes, and finally filter impurities through a filter to obtain component A;
[0018] (2) Preparation of component B:
[0019] a. First, disperse deionized water, fly ash and rock wool powder through a high-speed disperser for 10-20 minutes to obtain a filler suspension of component B, and then adjust the speed of the high-speed disperser;
[0020] b. Slowly add styrene acrylic emulsion into the filler suspension of component B and disperse for 25-30 minutes to obtain a preliminary suspension of component B;
[0021] c. Next, disperse the curing agent and the preliminary suspension of component B for 15-20 minutes, then add the paraffin microemulsion and disperse it through a high-speed disperser. Slowly add the defoamer during the dispersion process and disperse for 20-30 minutes. Finally, filter the impurities through a filter to obtain component B.
[0022] (3) Coating suspension and coating preparation:
[0023] The high-speed disperser is used to stir component A while slowly adding component B at a speed of 50-100 rpm, and disperses for 20-30 minutes to obtain a coating suspension, which is then sprayed on the cement board at a curing temperature of 15-35°C and dried in the shade for 48 hours to obtain a self-cleaning and heat-insulating coating.
[0024] Preferably, in step (1), dispersion is first performed at 200-300 rpm, and then the speed of the high-speed disperser is adjusted to 90-100 rpm.
[0025] Preferably, in step (2), dispersion is first performed at 200-300 rpm, and then the speed of the high-speed disperser is adjusted to 90-100 rpm.
[0026] Beneficial effects:
[0027] (1) The present invention adopts fly ash and rock wool powder to replace high-priced nano fillers such as nano silicon dioxide and titanium dioxide as paint fillers, thereby solving the solid waste problem of fly ash and rock wool powder and making high value-added utilization of fly ash and rock wool powder; paraffin microemulsion replaces fluorine-containing / fluorine-free silane as a low surface energy material, reducing the cost of hydrophobic architectural coatings, having the advantages of environmental protection and low cost, and being conducive to the market promotion of this technology.
[0028] (2) The present invention proposes a rock wool-based multifunctional water-based paint and a preparation method thereof, which comprehensively considers the characteristics of thermal insulation, hydrophobicity, workability, environmental protection and low cost of building exterior wall paint. After the paint is applied and cured, two birds with one stone are achieved: the fluffy rock wool powder with low thermal conductivity and fly ash can construct a porous structure inside the coating to play a role in thermal insulation, with a thermal conductivity of 0.069-0.108W / (m·K); a micro / nano structure can be constructed on the surface of the coating, making the coating hydrophobic with a contact angle of 139.6-157.2°.
[0029] (3) The present invention adopts an aqueous styrene-acrylic emulsion as a film-forming material and an aqueous carboxylated styrene-butadiene emulsion as an adhesion and hardness enhancing phase of the coating film. The carboxyl groups of the aqueous carboxylated styrene-butadiene emulsion and the residual carboxyl groups of the aqueous styrene-acrylic emulsion are cross-linked with a curing agent. After the coating is applied and cured, the hydrophilic carboxyl groups after film formation are reduced, thereby giving the coating a long-term waterproof property and high adhesion to the wall.
[0030] The above description is only an overview of the technical solution of the embodiment of the present application. In order to more clearly understand the technical means of the embodiment of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the embodiment of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, a brief introduction will be given below to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 This is the scanning electron microscope morphology of the multifunctional coating;
[0033] Figure 2 The contact angles of the multifunctional coating to water, sodium hydroxide solution (pH=14) and hydrochloric acid solution (pH=1);
[0034] Figure 3 This is the adhesion test result of the multifunctional coating;
[0035] Figure 4 The self-cleaning test results of the multifunctional coating. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used in the specification of the application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0038] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase "embodiments" in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0039] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application is clearly and completely described below.
[0040] Example 1
[0041] The present application provides a rock wool-based multifunctional water-based coating, which includes a component A and a component B. The component A includes 150 parts of styrene acrylic emulsion, 30 parts of carboxylated styrene butadiene emulsion, 55 parts of paraffin microemulsion, 25 parts of cellulose thickener, 8 parts of defoamer, 30 parts of fly ash, 60 parts of rock wool powder, and 150 parts of deionized water by weight; the component B includes 30 parts of styrene acrylic emulsion, 3 parts of cross-linking agent, 15 parts of paraffin microemulsion, 5 parts of defoamer, 10 parts of fly ash, 20 parts of rock wool powder, and 50 parts of deionized water by weight;
[0042] Among them, styrene acrylic emulsion has good adhesion, transparent film, good aging resistance, and can form film at room temperature; carboxylated styrene butadiene emulsion can undergo chemical reactions to improve coating adhesion, water resistance and hardness; paraffin microemulsion is acid-resistant, alkali-resistant, highly water-soluble, and emulsion-stable, and can be diluted with water in any proportion without stratification or demulsification, has a high solid content, and good dispersibility; cellulose thickener increases the viscosity or consistency of the coating, and has the advantages of small dosage, obvious thickening, and easy use; defoaming agent has good heat resistance, good diffusivity, good permeability, stable chemical properties, and strong oxidation resistance; aziridine crosslinker can be cured with carboxylated styrene butadiene emulsion at room temperature.
[0043] In this embodiment, in component A, the concentration of styrene acrylic emulsion is 45-50wt%, the concentration of carboxylated styrene butadiene emulsion is 35-40wt%, and the concentration of paraffin microemulsion is 30±1wt%.
[0044] In this embodiment, the concentration of styrene acrylic emulsion in component B is 45-50wt%, and the concentration of paraffin microemulsion is 30±1wt%.
[0045] In this embodiment, the pH values of the styrene acrylic emulsion, carboxylated styrene butadiene emulsion and paraffin microemulsion in component A are 7-8; the rock wool powder is in the shape of fibers; and the fly ash is spherical, and the particle size is 8-40 μm.
[0046] In this embodiment, the crosslinking agent in component B is a tetrafunctional aziridine crosslinking agent with a concentration of 99±0.2 wt %.
[0047] The preparation method of this embodiment comprises the following steps:
[0048] (1) Preparation of component A:
[0049] a. First, disperse deionized water, fly ash and rock wool powder through a high-speed disperser for 20 minutes to obtain a filler suspension of component A, and then adjust the speed of the high-speed disperser;
[0050] b. Slowly add styrene acrylic emulsion into the filler suspension of component A and disperse for 30 minutes to obtain a preliminary suspension of component A;
[0051] c. Next, the cellulose thickener and the preliminary suspension of component A are dispersed for 20 minutes, and then the paraffin microemulsion is added and dispersed by a high-speed disperser for 30 minutes;
[0052] d. Finally, add carboxylated styrene butadiene emulsion to disperse in the suspension obtained in the above step, and slowly add defoamer during the dispersion process, disperse for 20 minutes, and finally filter impurities through a filter to obtain component A;
[0053] (2) Preparation of component B:
[0054] a. First, disperse deionized water, fly ash and rock wool powder through a high-speed disperser for 20 minutes to obtain a filler suspension of component B, and then adjust the speed of the high-speed disperser;
[0055] b. Slowly add styrene acrylic emulsion into the filler suspension of component B and disperse for 25-30 minutes to obtain a preliminary suspension of component B;
[0056] c. Next, the curing agent and the preliminary suspension of component B are dispersed for 20 minutes, and then the paraffin microemulsion is added and dispersed by a high-speed disperser. During the dispersion process, the defoaming agent is slowly added and dispersed for 30 minutes. Finally, impurities are filtered through a filter to obtain component B;
[0057] (3) Coating suspension and coating preparation:
[0058] The high-speed disperser was used to stir component A at a speed of 50 rpm while slowly adding component B. The mixture was dispersed for 20 minutes to obtain a coating suspension, which was then sprayed on the cement board at a curing temperature of 15-35°C. The mixture was dried in the shade for 48 hours to obtain a self-cleaning and heat-insulating coating.
[0059] Preferably, in step (1), dispersion is first performed at 300 rpm, and then the speed of the high-speed disperser is adjusted to 100 rpm.
[0060] Preferably, in step (2), the dispersion is first performed at 200 rpm, and then the speed of the high-speed disperser is adjusted to 90 rpm.
[0061] like Figure 1 As shown in Figure 2, the rock wool-based multifunctional water-based building exterior wall coating has good hydrophobic properties, which is due to the micro / nano structure of the coating surface and the low surface energy modification of the paraffin microemulsion. Figure 2 As shown, the contact angle of the coating to water is 154.4±0.5°, the contact angle to sodium hydroxide solution (pH=14) is 150.7±0.3°, and the contact angle to hydrochloric acid solution (pH=1) is 150.1±0.6°, showing excellent corrosion resistance.
[0062] Example 2-20
[0063] The preparation method of the rock wool-based multifunctional water-based coating is consistent with that in Example 1 and will not be described in detail here, but the proportions of component A and component B are changed as follows.
[0064] Among them, the proportion of component A: 22 parts of cellulose thickener, 6 parts of defoamer, 28 parts of fly ash, 60 parts of rock wool powder, and 150 parts of deionized water, the amount of which does not change; the amount of styrene acrylic emulsion (45-50wt%), carboxylated butadiene styrene emulsion (35-40wt%) and paraffin microemulsion (30±1wt%) is changed.
[0065] Among them, the proportion of component B: 4 parts of defoaming agent, 9 parts of fly ash, 18 parts of rock wool powder, and 50 parts of deionized water, the amount of which does not change; the amount of styrene acrylic emulsion (45-50wt%), trifunctional aziridine crosslinker (99±0.2wt%) and paraffin microemulsion (30±1wt%) is changed.
[0066] Adhesion test was carried out according to GB / T 9286 (cross-cut test for paints and varnishes), with adhesion grades ranging from 0 to 5, with a total of 6 grades, with grade 0 being the highest. Figure 3 shown.
[0067] The hardness test is carried out according to GB / T 6739 (Determination of film hardness of paints and varnishes by pencil method). The hardness grade is 9B-9H, with a total of 20 grades, and 9H is the highest.
[0068] The impact resistance test was carried out according to GB / T 1732 (Determination of impact resistance of paint film), with an impact height of 50 cm, and divided into two states: normal and cracked.
[0069] Table 1 Contact angle, adhesion, hardness and impact resistance test results of the multifunctional coatings prepared in Examples 2-20.
[0070]
[0071]
[0072]
[0073] Examples 21-32
[0074] The preparation method of the multifunctional rock wool-based water-based coating is consistent with that in Example 1 and will not be described in detail here, but the proportions of component A and component B are changed as follows.
[0075] Among them, the proportion of component A is: 150 parts of styrene acrylic emulsion (45-50wt%), 23 parts of carboxylated butadiene styrene emulsion (35-40wt%), 18 parts of cellulose thickener, 5 parts of defoaming agent, 148 parts of deionized water and 44 parts of paraffin microemulsion (30±1wt%), and the amount does not change; the amount of fly ash and rock wool powder is changed.
[0076] Among them, the proportion of component B: 30 parts of styrene acrylic emulsion (45-50wt%), 2 parts of tetrafunctional aziridine crosslinker (99±0.2wt%), 3 parts of defoaming agent, 47 parts of deionized water and 13 parts of paraffin microemulsion (30±1wt%), the amount of which does not change; the amount of fly ash and rock wool powder changes.
[0077] The self-cleaning test is to place a mixture of mud and sand on the surface of the coating sample and then drip deionized water to simulate a rainy day. The raindrops remove pollutants and the results are divided into adhesion and non-adhesion. Example 28 Self-cleaning test Figure 4 shown.
[0078] Table 2 Contact angle, adhesion, hardness, impact resistance, self-cleaning and thermal conductivity test results of the multifunctional coatings prepared in Examples 21-32.
[0079]
[0080]
[0081] It can be seen from the preparation of multifunctional coatings in the above Examples 1-32 that fly ash and rock wool powder can be used as fillers to improve the thermal insulation performance of the coating without affecting the contact angle, adhesion, hardness, impact resistance and self-cleaning performance; paraffin microemulsion replaces fluorinated / non-fluorinated silane as a low surface energy substance, and the coating still exhibits excellent self-cleaning performance and a high contact angle.
[0082] The present invention adopts fly ash and rock wool powder to replace high-priced nano fillers such as nano silicon dioxide and titanium dioxide as paint fillers, thereby solving the solid waste problem of fly ash and rock wool powder and making high value-added utilization of fly ash and rock wool powder; paraffin microemulsion replaces fluorine-containing / fluorine-free silane as a low surface energy material, reducing the cost of hydrophobic architectural coatings, having the advantages of environmental protection and low cost, and being conducive to the market promotion of this technology.
[0083] The present invention adopts water-based styrene-acrylic emulsion as a film-forming material and water-based carboxyl styrene-butadiene emulsion as a coating film adhesion and hardness enhancing phase. The carboxyl group of the water-based carboxyl styrene-butadiene emulsion and the residual carboxyl group of the water-based styrene-acrylic emulsion are cross-linked with a curing agent. After the coating is coated and cured, the hydrophilic carboxyl group after film formation is reduced, thereby giving the coating a long-term waterproof performance and high adhesion to the wall surface.
[0084] In summary, the present invention proposes a rock wool-based multifunctional water-based paint and a preparation method thereof, which comprehensively considers the characteristics of thermal insulation, hydrophobicity, workability, environmental protection and low cost of building exterior wall paint. After the paint is applied and cured, two birds with one stone are achieved: the fluffy rock wool powder with low thermal conductivity and fly ash can construct a porous structure inside the coating to play a role in thermal insulation, with a thermal conductivity of 0.069-0.108W / (m·K); a micro / nano structure can be constructed on the surface of the coating, making the coating hydrophobic with a contact angle of 139.6-157.2°.
[0085] As described above, the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.
Claims
1. A rock wool based multifunctional water-based coating, It is characterized in that The water-based paint comprises a component A and a component B. The component A comprises, by weight, 120-150 parts of styrene-acrylic emulsion, 20-30 parts of carboxylated styrene-butadiene emulsion, 40-55 parts of paraffin microemulsion, 15-25 parts of cellulose thickener, 2-8 parts of defoamer, 20-30 parts of fly ash, 40-60 parts of rock wool powder and 140-150 parts of deionized water; the component B comprises, by weight, 20-30 parts of styrene-acrylic emulsion, 1-3 parts of cross-linking agent, 5-15 parts of paraffin microemulsion, 1-5 parts of defoamer, 5-10 parts of fly ash, 10-20 parts of rock wool powder and 40-50 parts of deionized water.
2. A rock wool-based multifunctional water-based paint according to claim 1, It is characterized in that In the component A, the concentration of styrene acrylic emulsion is 45-50wt%, the concentration of carboxylated styrene butadiene emulsion is 35-40wt%, and the concentration of paraffin microemulsion is 30±1wt%.
3. A rock wool-based multifunctional water-based paint according to claim 1, It is characterized in that The concentration of styrene acrylic emulsion in the component B is 45-50wt%, and the concentration of paraffin microemulsion is 30±1wt%.
4. A rock wool-based multifunctional water-based paint according to claim 1, It is characterized in that The pH values of the styrene acrylic emulsion, carboxyl styrene butadiene emulsion and paraffin microemulsion in the component A are 7-8; the rock wool powder is in a fiber shape; the fly ash is spherical, and the particle size is 8-40 μm.
5. A rock wool-based multifunctional water-based paint according to claim 1, It is characterized in that The crosslinking agent in the component B is a tetrafunctional aziridine crosslinking agent or a trifunctional aziridine crosslinking agent, and the concentration is 99±0.2wt%.
6. A method for preparing a rock wool-based multifunctional water-based coating as claimed in claim 1, It is characterized in that The preparation method comprises the following steps: (1) Preparation of component A: a. First, disperse deionized water, fly ash and rock wool powder through a high-speed disperser for 10-20 minutes to obtain a filler suspension of component A, and then adjust the speed of the high-speed disperser; b. Slowly add styrene acrylic emulsion into the filler suspension of component A and disperse for 30-40 minutes to obtain a preliminary suspension of component A; c. Next, disperse the cellulose thickener and the preliminary suspension of component A for 15-20 minutes, and then add the paraffin microemulsion and disperse it in a high-speed disperser for 10-30 minutes; d. Finally, add carboxylated styrene butadiene emulsion to disperse in the suspension obtained in the above step, and slowly add defoamer during the dispersion process, disperse for 20-30 minutes, and finally filter impurities through a filter to obtain component A; (2) Preparation of component B: a. First, disperse deionized water, fly ash and rock wool powder through a high-speed disperser for 10-20 minutes to obtain a filler suspension of component B, and then adjust the speed of the high-speed disperser; b. Slowly add styrene acrylic emulsion into the filler suspension of component B and disperse for 25-30 minutes to obtain a preliminary suspension of component B; c. Next, disperse the curing agent and the preliminary suspension of component B for 15-20 minutes, then add the paraffin microemulsion and disperse it through a high-speed disperser. Slowly add the defoamer during the dispersion process and disperse for 20-30 minutes. Finally, filter the impurities through a filter to obtain component B. (3) Coating suspension and coating preparation: The high-speed disperser is used to stir component A while slowly adding component B at a speed of 50-100 rpm, and disperses for 20-30 minutes to obtain a coating suspension, which is then sprayed on the cement board at a curing temperature of 15-35°C and dried in the shade for 48 hours to obtain a self-cleaning and heat-insulating coating.
7. A method for preparing a rock wool-based multifunctional water-based coating according to claim 6, It is characterized in that In the step (1), the dispersion is first performed at 200-300 rpm, and then the speed of the high-speed disperser is adjusted to 90-100 rpm.
8. A method for preparing a rock wool-based multifunctional water-based coating according to claim 6, It is characterized in that In the step (2), the dispersion is first performed at 200-300 rpm, and then the speed of the high-speed disperser is adjusted to 90-100 rpm.
Citation Information
Patent Citations
Water-based interior wall paint and preparation method thereof
CN106189581A
Wall heat insulation coating
CN106810954A
Multifunctional sealing and hardening prime coat, and preparation method and application thereof
CN108587354A
Reinforced heat insulating coating material
JP2020139029A