Weather-resistant self-cleaning coating as well as preparation method and application thereof
By using a weather-resistant self-cleaning coating with a specific composition, the problem of panel damage and insufficient coating adhesion caused by dust removal on photovoltaic panels has been solved, high adhesion, weather resistance and self-cleaning functions have been achieved, and photovoltaic power generation efficiency and lifespan have been improved.
Patent Information
- Application Number
- CN202410988264.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-15
AI Technical Summary
Existing dust removal methods for photovoltaic panels can damage the panels, and conventional transparent superhydrophobic coatings have insufficient adhesion and weather resistance, making it difficult to meet the needs for long-term self-cleaning and high light transmittance.
A weather-resistant self-cleaning coating composed of hydroxyl-terminated hyperbranched polysiloxane, hydroxyl fluorocarbon resin, non-isocyanate polyurethane polyol and solvent is used to form a coating with high adhesion and low surface energy through stirring, mixing and solidification to achieve hydrophobic and permeable coating. A combination of light and weather-resistant properties.
It achieves high adhesion, weather resistance and self-cleaning functions of photovoltaic panels, reduces power generation efficiency loss, and improves photovoltaic power generation efficiency and service life.
Smart Images

Figure BDA0004958114560000041 
Figure BDA0004958114560000042 
Figure BDA0004958114560000051
Abstract
Description
Technical Field
[0001] The invention relates to a weather-resistant self-cleaning coating and a preparation method and application thereof. Background Art
[0002] With the optimization of the railway energy structure, the "railway + photovoltaic" model has been innovated. The application of photovoltaics in the railway system not only realizes the full utilization of the space along the railway, but also the electricity resources generated by photovoltaics can be used or stored nearby, connected to the overhead line, and distributed to power facilities such as stations, monitoring, and signal lights along the railway, thereby reducing the loss caused by long-distance power transmission. At present, photovoltaics have been applied in railway station buildings, railway slopes, railway passenger car bodies, freight yards and other scenes.
[0003] After long-term use of the photovoltaic system, dust or dirt will accumulate on the surface of the photovoltaic panels. The presence of dust or dirt seriously reduces the transmittance of sunlight, which greatly reduces the power generation efficiency of the panels. The uneven transmittance of sunlight will also affect the surface temperature of the panels, causing the circuits to overheat and thus short-circuit. In addition, dust absorbs pollutants in the air and, after mixing with rainwater, forms acidic and alkaline substances that corrode the photovoltaic panels, forming pits on the surface of the glass cover. The non-smooth photovoltaic glass cover increases the diffuse reflection of its surface, reducing the power generation of the photovoltaic panels.
[0004] The following methods are currently used to remove dust deposited on photovoltaic panels: (1) When installing photovoltaic modules, high-pressure spray equipment is installed at a fixed position to clean the photovoltaic panels. This dust removal method not only wastes a large amount of water resources, but the high-pressure water will also cause certain damage to the panels. (2) Spray the panels with tap water and then wipe them manually. This dust removal method also consumes a lot of tap water. If the manual force is uneven, scratches or cracks are likely to appear on the surface of the panel. It can be seen that although the above dust removal method can clean the dust deposited on the panel, it will also cause damage to the panel during the dust removal process, reducing the service life of the photovoltaic panel. In addition, the high dust removal cost also increases the operation and maintenance cost of the photovoltaic panel.
[0005] The transparent super-hydrophobic coating not only has a low surface energy (coating surface energy <25mN / m), but also has a weak bonding force on the surface of the coating for dust, oil stains, etc., making it difficult to adhere to it. Even if it adheres, it can be easily removed by rain washing or other mechanical methods, reflecting the self-cleaning or easy-to-clean effect. Moreover, due to its anti-reflection and anti-transmittance properties, the glass can maintain a high degree of transparency, meet the lighting requirements, and thus improve the power generation efficiency of photovoltaic panels. This combination of anti-transmittance and super-hydrophobic properties has important application value and significance in the photovoltaic field. However, conventional transparent super-hydrophobic coatings have low adhesion to glass substrates, poor weather resistance, and short service life, making it difficult to meet the actual needs of maintaining self-cleaning and high light transmittance for a long time. How to solve the adhesion of the glass substrate while achieving weather resistance, self-cleaning and other functions is a major technical problem to be overcome in the current functional coatings industry. For example, the Chinese invention patent application "A transparent super-hydrophobic film, its preparation method and application" (publication number: CN109338304 A) discloses the preparation of a transparent, super-hydrophobic film with a thickness of 500-600nm, a visible light transmittance greater than 90%, and a water contact angle greater than 165°, but the invention adopts a combination of radio frequency magnetron sputtering and annealing, and the preparation process is complicated and the preparation cost is high; the Chinese invention patent application "A transparent self-cleaning film and its preparation method and application" (publication number: CN101492544) discloses that after the film is formed and dried by a mixed solution of tetraethyl orthosilicate, ethanol, ammonia water and water, it is placed in a silane and ethanol solution to self-assemble into a film, and a water contact angle of more than 150°, a hysteresis angle of less than 20°, and a light transmittance of more than 90% are obtained. The film has high mechanical strength and good self-cleaning performance. However, the weather resistance of the self-cleaning film prepared by this method is poor. Summary of the invention
[0006] In order to overcome the defects of the prior art, the present invention provides a weather-resistant self-cleaning coating and a preparation method thereof. The coating of the present invention has excellent hydrophobicity, light transmittance and adhesion, and has excellent weather resistance. The preparation method of the coating of the present invention is simple to operate, mild in conditions, and easy to realize mass production and application.
[0007] The technical solution adopted by the present invention is as follows:
[0008] On the one hand, the present invention provides a weather-resistant self-cleaning coating, which consists of two components A and B, wherein the component A is made of the following raw materials in parts by weight:
[0009] 5-30 parts of terminal hydroxyl hyperbranched polysiloxane;
[0010] 5-30 parts of hydroxy fluorocarbon resin;
[0011] 5-30 parts of non-isocyanate polyurethane polyol;
[0012] Catalyst 0.01-1 part;
[0013] 10-60 parts of the first solvent;
[0014] The B component is made of the following raw materials by weight:
[0015] 5-30 parts of isocyanate;
[0016] The second solvent is 10-60 parts.
[0017] Preferably, the A component is made of the following raw materials in parts by weight:
[0018] 5-20 parts of terminal hydroxyl hyperbranched polysiloxane;
[0019] 5-20 parts of hydroxy fluorocarbon resin;
[0020] 5-20 parts of non-isocyanate polyurethane polyol;
[0021] Catalyst 0.01-0.5 parts;
[0022] 10-50 parts of the first solvent;
[0023] Further preferably, the component A is made of the following raw materials in parts by weight:
[0024] 10-20 parts of terminal hydroxyl hyperbranched polysiloxane;
[0025] 5-15 parts of hydroxy fluorocarbon resin;
[0026] 10-20 parts of non-isocyanate polyurethane polyol;
[0027] Catalyst 0.03-0.5 parts;
[0028] 20-40 parts of the first solvent.
[0029] Preferably, the B component is made of the following raw materials in parts by weight:
[0030] Isocyanate 5-20 parts;
[0031] 10-50 parts of the second solvent;
[0032] Further preferably, the B component is made of the following raw materials in parts by weight:
[0033] Isocyanate 10-20 parts;
[0034] 20-40 parts of the second solvent.
[0035] Preferably, the A component is made of the following raw materials by weight:
[0036] 5-20 parts of terminal hydroxyl hyperbranched polysiloxane;
[0037] 5-20 parts of hydroxy fluorocarbon resin;
[0038] 5-20 parts of non-isocyanate polyurethane polyol;
[0039] Catalyst 0.01-0.5 parts;
[0040] 10-50 parts of the first solvent;
[0041] Preferably, the A component is made of the following raw materials by weight:
[0042] 5-20 parts of terminal hydroxyl hyperbranched polysiloxane;
[0043] 5-20 parts of hydroxy fluorocarbon resin;
[0044] 5-20 parts of non-isocyanate polyurethane polyol;
[0045] Catalyst 0.01-0.5 parts;
[0046] 10-50 parts of the first solvent;
[0047] Further preferably, the component A is made of the following raw materials in parts by weight:
[0048] 10-20 parts of terminal hydroxyl hyperbranched polysiloxane;
[0049] 5-15 parts of hydroxy fluorocarbon resin;
[0050] 10-20 parts of non-isocyanate polyurethane polyol;
[0051] Catalyst 0.03-0.5 parts;
[0052] 20-40 parts of the first solvent;
[0053] The B component is made of the following raw materials by weight:
[0054] Isocyanate 10-20 parts;
[0055] 20-40 parts of the second solvent.
[0056] Preferably, the mass ratio of the component A to the component B is 1 to 3:1, preferably 2:1. Preferably, the repeating unit of the hydroxyl-terminated hyperbranched polysiloxane is as follows:
[0057]
[0058] Preferably, the number average molecular weight of the terminal hydroxyl hyperbranched polysiloxane is 6000-15000, preferably 8000-12000.
[0059] Preferably, the hydroxyl value of the hydroxy fluorocarbon resin is 20KOH / g to 70KOH / g, preferably 30 to 60KOH / g, more preferably 40 to 60KOH / g;
[0060] Preferably, the hydroxyl fluorocarbon resin is selected from FEVE fluorocarbon resins which are copolymerized with fluoroolefins and alkyl vinyl ethers or alkyl vinyl esters and have hydroxyl groups in the molecular side chains;
[0061] Preferably, the chemical formula of the non-isocyanate polyurethane polyol is as follows:
[0062]
[0063] Wherein a=an integer of 3 to 6, b=an integer of 0 to 4, and c=an integer of 0 to 4.
[0064] Preferably, a=an integer of 3-6, b=an integer of 2-4, and c=an integer of 2-4.
[0065] Preferably, the non-isocyanate polyurethane polyol is selected from:
[0066]
[0067] Preferably, the catalyst is selected from one or more of dibutyltin dilaurate, di-n-octyltin dilaurate, dibutyltin didodecylsulfide, stannous octoate, dimethyltin dioctanoate and di-n-butyltin oxide, preferably dibutyltin didodecylsulfide;
[0068] Preferably, the isocyanate is selected from one or more of dimethyl diphenylmethane diisocyanate, p-phenylene diisocyanate, toluene diisocyanate and triphenylmethane triisocyanate, preferably dimethyl diphenylmethane diisocyanate;
[0069] Preferably, the first solvent and the second solvent are independently selected from one or more of butyl acetate, ethyl acetate, dimethyl succinate and dimethyl phthalate, preferably butyl acetate.
[0070] On the other hand, the present invention provides a method for preparing the aforementioned weather-resistant self-cleaning coating, the method comprising: stirring and mixing all raw materials in the A component to obtain the A component; stirring and mixing all raw materials in the B component to obtain the B component, thereby obtaining a two-component self-cleaning coating.
[0071] Preferably, the rotation speed of the stirring and mixing (the stirring and mixing can be the stirring and mixing when preparing component A or the stirring and mixing when preparing component B) is 200 r / min to 1000 r / min, preferably 300 r / min to 600 r / min.
[0072] Preferably, the temperature of the stirring and mixing (the stirring and mixing may be the stirring and mixing during the preparation of component A or the stirring and mixing during the preparation of component B) is 50°C to 100°C, preferably 60°C to 95°C.
[0073] Preferably, the stirring and mixing (the stirring and mixing may be the stirring and mixing during the preparation of component A or the stirring and mixing during the preparation of component B) takes place for 20 to 80 minutes, preferably for 30 to 60 minutes.
[0074] On the other hand, the present invention provides a weather-resistant self-cleaning coating, which is made of the above-mentioned high-transparency weather-resistant self-cleaning coating.
[0075] Preferably, the method for preparing the coating comprises the steps of mixing and curing the component A and the component B to form the coating.
[0076] Preferably, the mass ratio of the component A to the component B is 1 to 3:1, preferably 2:1;
[0077] Preferably, the curing temperature is 50-100°C, preferably 60-90°C, and more preferably 85°C.
[0078] Preferably, the curing time is 5 to 20 hours, preferably 10 to 18 hours.
[0079] Compared with the prior art, the present invention has at least the following beneficial technical effects:
[0080] The present invention selects a terminal hydroxyl hyperbranched polysiloxane of a specific type and molecular weight, which has many reactive active points and a high crosslinking density, so that the coating has higher mechanical properties and weather resistance; in addition, the terminal hydroxyl hyperbranched polysiloxane structure of the present invention contains more silicon-oxygen bonds, so that the coating has lower surface energy, high light transmittance and self-cleaning function.
[0081] The non-isocyanate polyurethane polyol selected by the present invention has urethane bonds and multiple active hydroxyl groups, good compatibility with isocyanate, and high crosslinking density, so that the coating has high chemical resistance, high adhesion and other properties; compared with ordinary polyether polyols, it has higher system compatibility and light transmittance.
[0082] The present invention further reduces the surface energy of the coating and improves the hydrophobic property through the synergistic effect of two low surface energy components, the hydroxyl fluorocarbon resin and the terminal hydroxyl hyperbranched polysiloxane.
[0083] In the process of coating curing of the present invention, due to the surface energy difference among the terminal hydroxyl hyperbranched polysiloxane, the hydroxyl fluorocarbon resin and the non-isocyanate polyurethane polyol, the non-isocyanate polyurethane polyol is enriched in the bottom layer and combined with the substrate to provide high adhesion and mechanical properties, the hydroxyl fluorocarbon resin is enriched in the middle layer, and the organosilicon chain segments of the terminal hydroxyl hyperbranched polysiloxane are enriched on the surface to form a self-cleaning coating with microphase separation. DETAILED DESCRIPTION
[0084] The present invention is further described below in conjunction with the embodiments. These embodiments are intended to help illustrate the content of the present invention rather than to limit the scope of the present invention.
[0085] Unless otherwise specified, the sources of the raw materials used in the following examples are as follows:
[0086] The synthesis method of terminal hydroxyl hyperbranched polysiloxane refers to Hu Xianfei et al., "Research on Hyperbranched Polysiloxane Modified Epoxy Resin", Thermosetting Resins, Vol. 37, No. 4, July 2022, pp. 19-30, and its repeating unit is as follows:
[0087]
[0088] Non-isocyanate polyurethane polyol having the following structures 1 to 4
[0089]
[0090]
[0091] Purchased from Guangdong Jinbo Chemical Co., Ltd.;
[0092] Hydroxy fluorocarbon resin, a FEVE-type fluorocarbon resin, was purchased from Shanghai Dongfu Chemical Technology Co., Ltd.;
[0093] Dimethyl diphenylmethane diisocyanate was purchased from Yantai Wanhua Chemical Group Co., Ltd.;
[0094] Hydroxypolydimethylsiloxane was purchased from Guangdong Keton Chemical Co., Ltd.;
[0095] Other reagents and instruments can be purchased from the market.
[0096] Example 1
[0097] 150g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 10000), 100g of non-isocyanate polyurethane polyol having the structure shown in Formula 1, 150g of hydroxyl fluorocarbon resin (hydroxyl value 50KOH / g), 1g of di(dodecylsulfide) dibutyltin, and 250g of butyl acetate were heated to 65°C, stirred and mixed at a speed of 500r / min for 40min to obtain component A of the self-cleaning coating.
[0098] 250 g of dimethyl diphenylmethane diisocyanate and 220 g of butyl acetate were heated to 95° C. and stirred and mixed at a speed of 400 r / min for 40 minutes to obtain component B of the self-cleaning coating.
[0099] Example 2
[0100] 100 g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 10,000), 150 g of non-isocyanate polyurethane polyol having the structure shown in Formula 2, 100 g of hydroxyl fluorocarbon resin (hydroxyl value 50 KOH / g), 2 g of di-n-octyltin dilaurate, and 300 g of butyl acetate were heated to 50° C. and stirred and mixed at a speed of 300 r / min for 60 min to obtain component A of the self-cleaning coating.
[0101] 250 g of dimethyl diphenylmethane diisocyanate and 250 g of butyl acetate were heated to 95° C. and stirred and mixed at a speed of 400 r / min for 40 minutes to obtain component B of the self-cleaning coating.
[0102] Example 3
[0103] 120g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 10000), 200g of non-isocyanate polyurethane polyol having the structure shown in Formula 3, 80g of hydroxyl fluorocarbon resin (hydroxyl value 30KOH / g), 1g of di(dodecylsulfide) dibutyltin, 120g of butyl acetate and 130g of dimethyl phthalate were heated to 65°C, stirred and mixed at a speed of 500r / min for 45min to obtain component A of the self-cleaning coating.
[0104] 210 g of p-phenylene diisocyanate and 200 g of dimethyl phthalate were heated to 80° C. and stirred and mixed at a speed of 500 r / min for 50 min to obtain component B of the self-cleaning coating.
[0105] Example 4
[0106] 100 g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 10,000), 110 g of non-isocyanate polyurethane polyol having the structure shown in Formula 4, 100 g of hydroxyl fluorocarbon resin (hydroxyl value 55 KOH / g), 2.5 g of dibutyltin(dodecylsulfide), and 270 g of butyl acetate were heated to 80° C. and stirred and mixed at a speed of 500 r / min for 40 min to obtain component A of the self-cleaning coating.
[0107] 100 g of dimethyl diphenylmethane diisocyanate, 80 g of toluene diisocyanate and 200 g of butyl acetate were heated to 60° C. and stirred and mixed at a speed of 400 r / min for 50 min to obtain component B of the self-cleaning coating.
[0108] Example 5
[0109] 150g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 10000), 100g of non-isocyanate polyurethane polyol having the structure shown in Formula 1, 50g of hydroxyl fluorocarbon resin (hydroxyl value 60KOH / g), 1g of stannous octoate, and 250g of dimethyl phthalate were heated to 65°C, stirred and mixed at a speed of 500r / min for 40min to obtain component A of the self-cleaning coating.
[0110] 200 g of toluene diisocyanate and 220 g of dimethyl phthalate were heated to 80° C., and stirred and mixed at a speed of 400 r / min for 40 minutes to obtain component B of the self-cleaning coating.
[0111] Example 6
[0112] 150g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 10000), 200g of non-isocyanate polyurethane polyol having the structure shown in Formula 1, 150g of hydroxyl fluorocarbon resin (hydroxyl value 50KOH / g), 1g of dibutyltin dilaurate, and 250g of butyl acetate were heated to 65°C, stirred and mixed at a speed of 500r / min for 40min to obtain component A of the self-cleaning coating.
[0113] 270 g of dimethyl diphenylmethane diisocyanate and 250 g of butyl acetate were heated to 70° C. and stirred and mixed at a speed of 550 r / min for 60 min to obtain component B of the self-cleaning coating.
[0114] Comparative Example 1
[0115] 150g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 3000), 100g of non-isocyanate polyurethane polyol having the structure shown in Formula 1, 150g of hydroxyl fluorocarbon resin (hydroxyl value 50KOH / g), 1g of di(dodecylsulfide) dibutyltin, and 250g of butyl acetate were heated to 65°C, stirred and mixed at a speed of 500r / min for 40min to obtain component A of the self-cleaning coating.
[0116] 250 g of dimethyl diphenylmethane diisocyanate and 220 g of butyl acetate were heated to 95° C. and stirred and mixed at a speed of 400 r / min for 40 minutes to obtain component B of the self-cleaning coating.
[0117] Comparative Example 2
[0118] 150g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 25000), 100g of non-isocyanate polyurethane polyol having the structure shown in Formula 1, 150g of hydroxyl fluorocarbon resin (hydroxyl value 50KOH / g), 1g of di(dodecylsulfide) dibutyltin, and 250g of butyl acetate were heated to 65°C, stirred and mixed at a speed of 500r / min for 40min to obtain component A of the self-cleaning coating.
[0119] 250 g of dimethyl diphenylmethane diisocyanate and 220 g of butyl acetate were heated to 95° C. and stirred and mixed at a speed of 400 r / min for 40 minutes to obtain component B of the self-cleaning coating.
[0120] Comparative Example 3
[0121] 150g of hydroxy polydimethylsiloxane, 100g of non-isocyanate polyurethane polyol having the structure shown in Formula 1, 150g of hydroxy fluorocarbon resin (hydroxyl value 50KOH / g), 1g of di(dodecylsulfide) dibutyltin, and 250g of butyl acetate are heated to 65°C, stirred and mixed at a speed of 500r / min for 40min to obtain component A of the self-cleaning coating.
[0122] 250 g of dimethyl diphenylmethane diisocyanate and 220 g of butyl acetate were heated to 95° C. and stirred and mixed at a speed of 400 r / min for 40 minutes to obtain component B of the self-cleaning coating.
[0123] Comparative Example 4
[0124] 150g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 10000), 100g of non-isocyanate polyurethane polyol having the structure shown in Formula 5, 150g of hydroxyl fluorocarbon resin (hydroxyl value 50KOH / g), 1g of di(dodecylsulfide) dibutyltin, and 250g of butyl acetate were heated to 65°C, stirred and mixed at a speed of 500r / min for 40min to obtain component A of the self-cleaning coating.
[0125]
[0126] 250 g of dimethyl diphenylmethane diisocyanate and 220 g of butyl acetate were heated to 95° C. and stirred and mixed at a speed of 400 r / min for 40 minutes to obtain component B of the self-cleaning coating.
[0127] Comparative Example 5
[0128] 150g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 10000), 100g of polyether 330N polyol, 150g of hydroxyl fluorocarbon resin (hydroxyl value 50KOH / g), 1g of di(dodecylsulfide) dibutyltin, and 250g of butyl acetate were heated to 65°C, stirred and mixed at a speed of 500r / min for 40min to obtain component A of the self-cleaning coating.
[0129] 250 g of dimethyl diphenylmethane diisocyanate and 220 g of butyl acetate were heated to 95° C. and stirred and mixed at a speed of 400 r / min for 40 minutes to obtain component B of the self-cleaning coating.
[0130] Comparative Example 6
[0131] 150 g of terminal hydroxyl hyperbranched polysiloxane (molecular weight 10,000), 100 g of non-isocyanate polyurethane polyol having the structure shown in Formula 1, 1 g of dibutyltin didodecylsulfide, and 250 g of butyl acetate were heated to 65° C. and stirred and mixed at a speed of 500 r / min for 40 min to obtain component A of the self-cleaning coating.
[0132] 200 g of dimethyl diphenylmethane diisocyanate and 220 g of butyl acetate were heated to 95° C. and stirred and mixed at a speed of 400 r / min for 40 min to obtain component B of the self-cleaning coating.
[0133] Experimental Example 1
[0134] The components A and B of the above-mentioned embodiments 1 to 6 and comparative examples 1 to 6 were mixed in a mass ratio of 2:1, sprayed onto ordinary ultra-white glass within 2 hours, cured at 85°C for 10 hours, and the performance of the paint film was tested after cooling to room temperature. The results are shown in Table 1-2.
[0135] The test method for improving power generation efficiency is the standard comparison method, which is: 2 The photovoltaic panels were cleaned and dried, and a self-cleaning coating with a dry film thickness of 25-30μm was sprayed on the photovoltaic panels as a photovoltaic power generation system test group. 2 The photovoltaic panels were cleaned at the same time and used as the blank group of the photovoltaic power generation system to compare the total power generation of the two photovoltaic power generation systems for 6 months. Power generation efficiency improvement rate = (total power generation of the test group - total power generation of the blank group) / total power generation of the blank group × 100%.
[0136] Table 1 Test results of coating properties of Examples 1-6
[0137]
[0138]
[0139] Table 2 Comparative Examples 1-6 Coating Performance Test Results
[0140]
[0141] Compared with Examples 1-6 of the present invention, Comparative Examples 1 and 2 use terminal hydroxyl hyperbranched polysiloxane with a molecular weight of 3000 and terminal hydroxyl hyperbranched polysiloxane with a molecular weight of 25000, and the contact angles are lower than those of Examples 1-6. Comparative Example 1 uses a small molecular weight terminal hydroxyl polysiloxane, with few active groups, poor synergy between organosilicon and organofluorine, and its light transmittance, adhesion, and power generation efficiency improvement rate are all reduced. Comparative Example 3 uses conventional silanol polydimethylsiloxane to replace terminal hydroxyl hyperbranched polysiloxane. Since the reactivity of silanol is lower than that of carbon hydroxyl, it is difficult to fully react with other components, and its weather resistance such as resistance to liquid media and stain resistance is poor, resulting in a decrease in the power generation efficiency improvement rate. Comparative Example 4 uses a long-chain non-isocyanate polyurethane polyol, and its compatibility, reactivity, etc. in the system are all reduced, resulting in an increase in surface energy, a decrease in light transmittance and weather resistance, and thus affecting the photovoltaic power generation efficiency. Comparative Example 5 uses polyether 330N polyol instead of non-isocyanate polyurethane polyol. Since the hydroxyl equivalent of polyether 330N polyol is low, the structural difference between it and non-isocyanate polyurethane polyol is large, resulting in low crosslinking density of the paint film, obvious macroscopic phase separation of the paint film, and a significant decrease in various properties of the paint film. Comparative Example 6 does not use hydroxyl fluorocarbon resin, but only a single low surface energy component, terminal hydroxyl hyperbranched polysiloxane, which loses the synergistic effect of organosilicon and organofluorine, resulting in a lower contact angle to water, and a decrease in hydrophobicity and stain resistance.
[0142] In summary, the coatings prepared in Examples 1 to 6 of the present invention using components such as terminal hydroxyl hyperbranched polysiloxane, non-isocyanate polyurethane polyol, hydroxyl fluorocarbon resin, catalyst, solvent, etc. have high mechanical properties, high light transmittance, high adhesion, high weather resistance, and resistance to chemical solvents.
Claims
1. A weather-resistant self-cleaning coating, the coating is composed of two components A and B, wherein: The A component is made of the following raw materials by weight: 5-30 parts of terminal hydroxyl hyperbranched polysiloxane; 5-30 parts of hydroxy fluorocarbon resin; 5-30 parts of non-isocyanate polyurethane polyol; Catalyst 0.01-1 part; 10-60 parts of the first solvent; The B component is made of the following raw materials by weight: 5-30 parts of isocyanate; The second solvent is 10-60 parts.
2. The weather-resistant self-cleaning coating according to claim 1, characterized in that: The A component is made of the following raw materials by weight: 5-20 parts of terminal hydroxyl hyperbranched polysiloxane; 5-20 parts of hydroxy fluorocarbon resin; 5-20 parts of non-isocyanate polyurethane polyol; Catalyst 0.01-0.5 parts; 10-50 parts of the first solvent; Preferably, the A component is made of the following raw materials in parts by weight: 10-20 parts of terminal hydroxyl hyperbranched polysiloxane; 5-15 parts of hydroxy fluorocarbon resin; 10-20 parts of non-isocyanate polyurethane polyol; Catalyst 0.03-0.5 parts; 20-40 parts of the first solvent; Preferably, the B component is made of the following raw materials in parts by weight: Isocyanate 5-20 parts; 10-50 parts of the second solvent; Preferably, the B component is made of the following raw materials in parts by weight: Isocyanate 10-20 parts; 20-40 parts of the second solvent; Preferably, the mass ratio of the component A to the component B is 1 to 3:1, preferably 2:
1.
3. The weather-resistant self-cleaning coating according to claim 1 or 2, characterized in that: The repeating unit of the hydroxy-terminated hyperbranched polysiloxane is as follows: Preferably, the number average molecular weight of the terminal hydroxyl hyperbranched polysiloxane is 6000-15000, preferably 8000-12000.
4. The weather-resistant self-cleaning coating according to any one of claims 1 to 3, characterized in that: The hydroxyl fluorocarbon resin has a hydroxyl value of 20KOH / g to 70KOH / g, preferably 30 to 50KOH / g, and more preferably 30 to 40KOH / g; Preferably, the hydroxy fluorocarbon resin is selected from FEVE fluorocarbon resins containing hydroxyl groups in the molecular side chains and formed by copolymerization of fluoroolefins and alkyl vinyl ethers or alkyl vinyl esters.
5. The weather-resistant self-cleaning coating according to any one of claims 1 to 4, characterized in that: The chemical formula of the non-isocyanate polyurethane polyol is as follows: Wherein a=an integer from 3 to 6, b=an integer from 0 to 4, and c=an integer from 0 to 4; Preferably, a=an integer of 3 to 6, b=an integer of 2 to 4, and c=an integer of 2 to 4; Preferably, the non-isocyanate polyurethane polyol is selected from:
6. The weather-resistant self-cleaning coating according to any one of claims 1 to 5, characterized in that: The catalyst is selected from one or more of dibutyltin dilaurate, di-n-octyltin dilaurate, dibutyltin didodecylsulfide, stannous octoate, dimethyltin dioctanoate and di-n-butyltin oxide, preferably dibutyltin didodecylsulfide.
7. The weather-resistant self-cleaning coating according to any one of claims 1 to 6, characterized in that: The isocyanate is selected from one or more of dimethyl diphenyl methane diisocyanate, p-phenylene diisocyanate, toluene diisocyanate and triphenylmethane triisocyanate, preferably dimethyl diphenyl methane diisocyanate.
8. The weather-resistant self-cleaning coating according to any one of claims 1 to 7, characterized in that: The first solvent and the second solvent are independently selected from one or more of butyl acetate, ethyl acetate, dimethyl succinate and dimethyl phthalate, preferably butyl acetate.
9. A method for preparing the weather-resistant self-cleaning coating according to any one of claims 1 to 8, the method comprising: Stirring and mixing all the raw materials in the A component to obtain the A component; Stirring and mixing all the raw materials in the B component to obtain the B component, thereby obtaining a two-component self-cleaning coating; Preferably, the stirring and mixing speed is 200r / min to 1000r / min, preferably 300r / min to 600r / min; Preferably, the stirring and mixing temperature is 50°C to 100°C, preferably 60°C to 95°C; Preferably, the stirring and mixing time is 20 to 80 minutes, preferably 30 to 60 minutes.
10. A weather-resistant self-cleaning coating, the coating being made of the highly transparent weather-resistant self-cleaning coating according to any one of claims 1 to 8; Preferably, the method for preparing the coating comprises the steps of mixing and curing the component A and the component B to form the coating; Preferably, the mass ratio of the component A to the component B is 1 to 3:1, preferably 2:1; Preferably, the curing temperature is 50 to 100°C, preferably 60 to 90°C, and more preferably 85°C; Preferably, the curing time is 5 to 20 hours, preferably 10 to 18 hours.
Citation Information
Patent Citations
Hyperbranched non-ionic waterborne polyurethane leather finishing agent and preparation method thereof
CN104193941A
Preparation method and application of low-viscosity polyether hyperbranched epoxy resin
CN111944120A
Weather-resistant self-cleaning self-layering coating as well as preparation method and application thereof
CN112795307A
Self-cleaning coating as well as preparation method and application thereof
CN114163907A
Ultra-smooth self-cleaning coating and preparation method thereof
CN115340822A
Cited By
Self-repairing and self-cleaning coating as well as preparation method and application thereof
CN119931480A
Self-repairing self-cleaning coating and preparation method and use thereof
CN119931480B
High-solid-content silicon-containing multi-arm star-shaped hydroxyl polyester for antifouling automobile coating and preparation method thereof
CN122302244A