Composite fireproof adhesive and preparation method thereof
By using water-based expanded graphite, sodium silicate colloidal solution, aluminum hydroxide and other components in water-based fire-retardant adhesives, the problem of insufficient performance of existing fire-retardant adhesives is solved, and the excellent fire-retardant and flame-retardant properties and economy of the composite fire-retardant adhesive are achieved. Possible preparation methods.
Patent Information
- Application Number
- CN202411117071.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methods of preparing water-based fireproof adhesives using a single expanded graphite have poor performance, and the organic binder reduces the fireproof and flame retardant properties, making it difficult to meet the demand for efficient fireproof and flame retardant.
Water-based expanded graphite is compounded with sodium silicate colloidal solution, combined with aluminum hydroxide and inorganic fillers, and through the interaction of specific proportions of components, a composite fire-retardant adhesive with excellent fire retardant properties is prepared.
On the basis of meeting the basic requirements for use, the product has significantly improved fire and flame retardant properties, and the process is simple, the conditions are mild, the raw materials are easily available and the cost is low, and it has broad application prospects.
Smart Images

Figure BDA0004994699680000101 
Figure BDA0004994699680000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fireproof adhesives, and more specifically to a composite fireproof adhesive and a preparation method thereof. Background Art
[0002] my country is the largest country in terms of natural graphite resources, with 2 / 3 of the world's reserves in my country. Graphite is an inorganic substance with a chemical composition of Q and belongs to the hexagonal crystal system. The crystals are hexagonal plates and flakes, and the aggregates are scaly. It is iron black and has a density of 2.25g / cm 3 , has a slippery feel, can conduct electricity, is chemically inactive, and has corrosion resistance. Expandable graphite is a graphite product obtained by chemical or electrochemical treatment of natural flake graphite. The expandable graphite material made from natural flake graphite not only retains the high temperature resistance and corrosion resistance of graphite, can withstand long-term irradiation of neutron flow, β rays, and γ rays, has a low friction coefficient, good self-lubrication, and is electrically conductive and thermally anisotropic, but also has the characteristics of bendability, compressibility, elasticity, and impermeability that natural graphite does not have. It is loose and porous, does not decompose, deform or age under high temperature, high pressure or radiation conditions, and has stable chemical properties. At the same time, graphite has a layered structure. Alkali metals, halogen metal halides, strong oxidizing oxygen-containing acids, etc. can be embedded in the interlayer to form interlayer compounds. When subjected to high temperatures above 200°C, due to the decomposition of the compounds absorbed in the layered lattice, the compounds between the graphite layers rapidly decompose, gasify, and expand (expanding 150 to 250 times along the interlayer), causing the expandable graphite to begin to expand and reach its maximum volume at 1100°C; the final volume can reach 280 times the initial volume, thereby producing a very low density (0.003 to 0.005 g / cm 3 ) of worm-like graphite. It is a loose, soft and tough material, so it is usually called flexible graphite.
[0003] However, the existing preparation of water-based fireproof adhesive uses a single expanded graphite as a raw material, which has poor fireproof and flame retardant properties and affects the quality of the water-based fireproof adhesive; at the same time, acrylic emulsion or polyurethane emulsion is used as an adhesive, and a large amount of organic adhesive reduces the fireproof and flame retardant properties of the water-based fireproof adhesive. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a composite fireproof adhesive and a preparation method thereof. The composite fireproof adhesive provided by the present invention is compounded by aqueous expanded graphite and an inorganic colloid solution, and has excellent fireproof and flame retardant properties on the basis of meeting basic use requirements.
[0005] The present invention provides a composite fireproof adhesive, which is prepared from raw materials including the following components:
[0006] 10 to 30 parts by weight of water-based adhesive;
[0007] 10 to 30 parts by weight of sodium silicate colloidal solution;
[0008] 10 to 25 parts by weight of expanded graphite;
[0009] 5 to 20 parts by weight of heat-absorbing powder;
[0010] 15 to 25 parts by weight of inorganic filler;
[0011] 0.2 to 0.8 parts by weight of defoamer;
[0012] 0.5 to 1.5 parts by weight of wetting agent;
[0013] 0.5 to 1.5 parts by weight of dispersant;
[0014] 1 to 2 parts by weight of thickener;
[0015] Water: 4 to 8 parts by weight.
[0016] Preferably, the aqueous adhesive is an acrylic emulsion.
[0017] Preferably, the preparation method of the sodium silicate colloidal solution is specifically as follows:
[0018] Liquid caustic soda and quartz sand are mixed in a mass ratio of (2-4):1, reacted at 100-150°C to obtain a sodium silicate reaction liquid, and then the sodium silicate reaction liquid is filtered and concentrated to obtain a sodium silicate colloidal solution.
[0019] Preferably, the fineness of the expanded graphite is 600-800 mesh, and the expansion ratio is 180-250 times.
[0020] Preferably, the endothermic powder is aluminum hydroxide with a fineness of 600-800 mesh.
[0021] Preferably, the inorganic filler is selected from diatomaceous earth and / or heavy calcium carbonate; the fineness of the inorganic filler is 600-800 mesh.
[0022] Preferably, the defoaming agent is selected from one or more of modified siloxane, organosilicon defoaming agent and mineral oil defoaming agent.
[0023] Preferably, the dispersant is a sodium polyacrylate dispersant.
[0024] Preferably, the thickener is selected from polyurethane thickeners and / or acrylic thickeners.
[0025] The present invention also provides a method for preparing the composite fireproof adhesive described in the above technical solution, comprising the following steps:
[0026] a) stirring the expanded graphite, inorganic filler and endothermic powder at 100 r / min to 200 r / min for 20 min to 40 min to obtain a premix;
[0027] b) stirring the aqueous binder, the sodium silicate colloidal solution, the defoamer, the dispersant, the wetting agent, the thickener and water at 300 r / min to 500 r / min for 10 to 20 min to obtain a mixed sol;
[0028] c) adding the premix obtained in step a) to the mixed sol obtained in step b) under stirring at 300 r / min to 500 r / min, and then dispersing at 1300 r / min to 1400 r / min for 40 min to 50 min to obtain slurry; finally, the slurry is sand-milled, paint-mixed and filtered in sequence to obtain a composite fireproof adhesive after discharging.
[0029] The present invention provides a composite fireproof adhesive, which is prepared from raw materials including the following components: 10 to 30 parts by weight of water-based adhesive; 10 to 30 parts by weight of sodium silicate colloidal solution; 10 to 25 parts by weight of expanded graphite; 5 to 20 parts by weight of endothermic powder; 15 to 25 parts by weight of inorganic filler; 0.2 to 0.8 parts by weight of defoamer; 0.5 to 1.5 parts by weight of wetting agent; 0.5 to 1.5 parts by weight of dispersant; 1 to 2 parts by weight of thickener; and 4 to 8 parts by weight of water. Compared with the prior art, the composite fireproof adhesive provided by the present invention adopts specific components in specific contents to achieve better overall interaction, and the product has excellent fireproof and flame-retardant properties on the basis of meeting basic use requirements.
[0030] In addition, the preparation method provided by the present invention has a simple process, mild and easy-to-control conditions, and the raw materials are readily available and low in cost, and has broad application prospects. DETAILED DESCRIPTION
[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The present invention provides a composite fireproof adhesive, which is prepared from raw materials including the following components:
[0033] 10 to 30 parts by weight of water-based adhesive;
[0034] 10 to 30 parts by weight of sodium silicate colloidal solution;
[0035] 10 to 25 parts by weight of expanded graphite;
[0036] 5 to 20 parts by weight of heat-absorbing powder;
[0037] 15 to 25 parts by weight of inorganic filler;
[0038] 0.2 to 0.8 parts by weight of defoamer;
[0039] 0.5 to 1.5 parts by weight of wetting agent;
[0040] 0.5 to 1.5 parts by weight of dispersant;
[0041] 1 to 2 parts by weight of thickener;
[0042] Water: 4 to 8 parts by weight.
[0043] In the present invention, the composite fireproof adhesive is prepared from raw materials including aqueous adhesive, sodium silicate colloidal solution, expanded graphite, endothermic powder, inorganic filler, defoamer, wetting agent, dispersant, thickener and water, preferably prepared from aqueous adhesive, sodium silicate colloidal solution, expanded graphite, endothermic powder, inorganic filler, defoamer, wetting agent, dispersant, thickener and water.
[0044] In the present invention, the water-based adhesive is preferably an acrylic emulsion. The present invention has no special restrictions on the source of the water-based adhesive, and commercially available products known to those skilled in the art can be used. In the present invention, the composite fireproof adhesive includes 10 to 30 parts by weight of the water-based adhesive, which can be 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, or 30 parts by weight.
[0045] In the present invention, the sodium silicate colloidal solution is an inorganic colloidal solution, and its preparation method is preferably as follows:
[0046] Mixing liquid caustic soda and quartz sand in a mass ratio of (2-4):1, reacting at 100°C-150°C to obtain a sodium silicate reaction liquid, and then filtering and concentrating the sodium silicate reaction liquid to obtain a sodium silicate colloidal solution;
[0047] More preferably:
[0048] Liquid caustic soda and quartz sand are mixed in a mass ratio of 3:1, reacted at 120°C to 130°C to obtain a sodium silicate reaction liquid, and then the sodium silicate reaction liquid is filtered and concentrated to obtain a sodium silicate colloidal solution. The present invention has no particular restrictions on the sources of the liquid caustic soda and quartz sand, and commercially available products known to those skilled in the art can be used.
[0049] The invention adopts the self-made sodium silicate colloidal solution, which has good thermal stability, is not easy to decompose at high temperature, and has lower thermal conductivity.
[0050] In the present invention, the composite fireproof adhesive comprises 10 to 30 parts by weight of sodium silicate colloidal solution, which may be 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, or 30 parts by weight.
[0051] In the present invention, the fineness of the expanded graphite is preferably 600-800 meshes, and the expansion ratio is preferably 180-250 times. The present invention has no special restrictions on the source of the expanded graphite, and commercially available products known to those skilled in the art can be used. In the present invention, the composite fireproof adhesive includes 10-25 parts by weight of expanded graphite, which can be 10 parts by weight, 15 parts by weight, 20 parts by weight, or 25 parts by weight.
[0052] In the present invention, the endothermic powder is preferably aluminum hydroxide with a fineness of 600-800 mesh; aluminum hydroxide will produce an endothermic reaction at high temperature, which can slow down or inhibit the combustion of objects, and the composite expanded graphite has a better fire retardant effect. The present invention has no special restrictions on the source of the endothermic powder, and commercial products known to those skilled in the art can be used. In the present invention, the composite fireproof adhesive includes 5 to 20 parts by weight of the endothermic powder, which can be 5 parts by weight, 10 parts by weight, 15 parts by weight, and 20 parts by weight.
[0053] In the present invention, the inorganic filler is preferably selected from diatomaceous earth and / or heavy calcium carbonate, more preferably diatomaceous earth; compared with inorganic fillers such as heavy calcium carbonate, mica powder, talcum powder, diatomaceous earth has a lower thermal conductivity; the fineness of the inorganic filler is preferably 600 mesh to 800 mesh. The present invention has no special restrictions on the source of the inorganic filler, and commercially available products known to those skilled in the art can be used. In the present invention, the composite fireproof adhesive includes 15 to 25 parts by weight of inorganic filler, which can be 15 parts by weight, 20 parts by weight, or 25 parts by weight.
[0054] In the present invention, the defoamer is preferably selected from one or more of modified siloxane, silicone defoamer and mineral oil defoamer, more preferably a mineral oil defoamer. The present invention has no special restrictions on the source of the defoamer, and commercially available products well known to those skilled in the art can be used. In the present invention, the composite fireproof adhesive includes 0.2 to 0.8 parts by weight of the defoamer, which can be 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, and 0.8 parts by weight.
[0055] The present invention has no special restrictions on the type and source of the wetting agent, and a commercially available wetting agent that can play a wetting role and is well known to those skilled in the art can be used. In the present invention, the composite fireproof adhesive includes 0.5 to 1.5 parts by weight of the wetting agent, which can be 0.5 parts by weight, 1 part by weight, or 1.5 parts by weight.
[0056] In the present invention, the dispersant is preferably a sodium polyacrylate dispersant, which can be a commercially available product known to those skilled in the art. In the present invention, the composite fireproof adhesive includes 0.5 to 1.5 parts by weight of the dispersant, which can be 0.5 parts by weight, 1 part by weight, or 1.5 parts by weight.
[0057] In the present invention, the thickener is preferably selected from polyurethane thickeners and / or acrylic thickeners, and more preferably acrylic thickeners. The present invention has no special restrictions on the source of the thickener, and commercially available products known to those skilled in the art can be used. In the present invention, the composite fireproof adhesive includes 1 to 2 parts by weight of the thickener, which can be 1 part by weight, 1.5 parts by weight, or 2 parts by weight.
[0058] In the present invention, the water is preferably deionized water. In the present invention, the composite fireproof adhesive comprises 4 to 8 parts by weight of water, which may be 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, or 8 parts by weight.
[0059] The composite fireproof adhesive provided by the present invention adopts specific components in specific contents to achieve better overall interaction. For example, the inorganic colloidal solution sodium silicate is used in combination with the acrylic emulsion as a water-based adhesive to improve the fireproof and flame retardant properties of the product. At the same time, the expanded graphite and the endothermic powder aluminum hydroxide are used in combination to greatly improve the fireproof and flame retardant properties of the product. Therefore, the product has excellent fireproof and flame retardant properties on the basis of meeting basic use requirements.
[0060] The present invention also provides a method for preparing the composite fireproof adhesive described in the above technical solution, comprising the following steps:
[0061] a) stirring the expanded graphite, inorganic filler and endothermic powder at 100 r / min to 200 r / min for 20 min to 40 min to obtain a premix;
[0062] b) stirring the aqueous binder, the sodium silicate colloidal solution, the defoamer, the dispersant, the wetting agent, the thickener and water at 300 r / min to 500 r / min for 10 to 20 min to obtain a mixed sol;
[0063] c) adding the premix obtained in step a) to the mixed sol obtained in step b) under stirring at 300 r / min to 500 r / min, and then dispersing at 1300 r / min to 1400 r / min for 40 min to 50 min to obtain slurry; finally, the slurry is sand-milled, paint-mixed and filtered in sequence to obtain a composite fireproof adhesive after discharging.
[0064] The present invention uniformly mixes expanded graphite, inorganic filler and endothermic powder to obtain a premix; uniformly mixes an aqueous adhesive, a sodium silicate colloidal solution (inorganic colloidal solution), a defoamer, a dispersant, a wetting agent, a thickener and water to obtain a mixed sol; then the mixed sol is mixed with the premix, and the aqueous expanded graphite, the inorganic filler and the endothermic powder are fully dispersed in the mixed sol; finally, the fineness and viscosity of the product are adjusted by sand milling, paint mixing and filtering to meet the use requirements, and the prepared composite fireproof adhesive is obtained by discharging the material, and the composite fireproof adhesive is stored in a sealed container. The present invention has no special restrictions on the stirring device, such as a mixer, a disperser, a dispersion kettle, etc. well known to those skilled in the art.
[0065] The preparation method provided by the invention has simple process, mild and easy-to-control conditions, and readily available raw materials with low cost, and has broad application prospects.
[0066] The present invention provides a composite fireproof adhesive, which is prepared from raw materials including the following components: 10 to 30 parts by weight of water-based adhesive; 10 to 30 parts by weight of sodium silicate colloidal solution; 10 to 25 parts by weight of expanded graphite; 5 to 20 parts by weight of endothermic powder; 15 to 25 parts by weight of inorganic filler; 0.2 to 0.8 parts by weight of defoamer; 0.5 to 1.5 parts by weight of wetting agent; 0.5 to 1.5 parts by weight of dispersant; 1 to 2 parts by weight of thickener; and 4 to 8 parts by weight of water. Compared with the prior art, the composite fireproof adhesive provided by the present invention adopts specific components in specific contents to achieve better overall interaction, and the product has excellent fireproof and flame-retardant properties on the basis of meeting basic use requirements.
[0067] In addition, the preparation method provided by the present invention has a simple process, mild and easy-to-control conditions, and the raw materials are readily available and low in cost, and has broad application prospects.
[0068] In order to further illustrate the present invention, the following examples are used for detailed description. The raw materials used in the following examples of the present invention are all commercially available; among them, the acrylic emulsion is provided by Dow Chemical, model: AV1220, which is a water-based acrylic emulsion, the expanded graphite is provided by Qingdao Tianheda Graphite Co., Ltd., model: KP80250, which is a water-based expanded graphite, and its particle size distribution is uniform, the fineness is between 600 mesh and 800 mesh, and the expansion ratio is 180 to 250 times, the fineness of aluminum hydroxide is 600 mesh to 800 mesh, the fineness of diatomaceous earth is 600 mesh to 800 mesh, the defoamer is NXZ, provided by Japan Nopco, the wetting agent is X-405, provided by Dow Chemical, the dispersant is a polyacrylic acid ammonium salt dispersant, provided by Dow Chemical, and the thickener is TT935, provided by Dow Chemical;
[0069] The sodium silicate colloidal solution is prepared by self-production from commercially available raw materials. The specific preparation method is as follows:
[0070] Liquid caustic soda and quartz sand are mixed in a mass ratio of 3:1, reacted at 125°C to generate a sodium silicate liquid product, and then the liquid after the reaction is filtered to remove impurities, and finally concentrated to obtain a finished sodium silicate colloidal solution with a concentration of 40-42%.
[0071] Example 1
[0072] It is prepared from the following raw materials by weight:
[0073] 30 parts of acrylic emulsion;
[0074] 10 parts of sodium silicate colloidal solution;
[0075] Expanded graphite 25 parts;
[0076] 5 parts of aluminum hydroxide;
[0077] 20 parts of diatomaceous earth;
[0078] 0.5 parts of defoaming agent;
[0079] 1 part wetting agent;
[0080] 1 part of dispersant;
[0081] 1.5 parts of thickener;
[0082] 6 parts of deionized water.
[0083] Example 2
[0084] The preparation method is prepared from the following raw materials in parts by weight: 25 parts of acrylic emulsion;
[0085] 15 parts of sodium silicate colloidal solution;
[0086] Expanded graphite 25 parts;
[0087] 5 parts of aluminum hydroxide;
[0088] 20 parts of diatomaceous earth;
[0089] 0.5 parts of defoaming agent;
[0090] 1 part wetting agent;
[0091] 1 part of dispersant;
[0092] 1.5 parts of thickener;
[0093] 6 parts of deionized water.
[0094] Example 3
[0095] The preparation method is prepared from the following raw materials in parts by weight: 20 parts of acrylic emulsion;
[0096] 20 parts of sodium silicate colloidal solution;
[0097] Expanded graphite 25 parts;
[0098] 5 parts of aluminum hydroxide;
[0099] 20 parts of diatomaceous earth;
[0100] 0.5 parts of defoaming agent;
[0101] 1 part wetting agent;
[0102] 1 part of dispersant;
[0103] 1.5 parts of thickener;
[0104] 6 parts of deionized water.
[0105] Example 4
[0106] The preparation method is prepared from the following raw materials in parts by weight: 10 parts of acrylic emulsion;
[0107] 30 parts of sodium silicate colloidal solution;
[0108] Expanded graphite 25 parts;
[0109] 5 parts of aluminum hydroxide;
[0110] 20 parts of diatomaceous earth;
[0111] 0.5 parts of defoaming agent;
[0112] 1 part wetting agent;
[0113] 1 part of dispersant;
[0114] 1.5 parts of thickener;
[0115] 6 parts of deionized water.
[0116] Example 5
[0117] The preparation method is prepared from the following raw materials in parts by weight: 20 parts of acrylic emulsion;
[0118] 20 parts of sodium silicate colloidal solution;
[0119] 20 parts of expanded graphite;
[0120] 10 parts of aluminum hydroxide;
[0121] 20 parts of diatomaceous earth;
[0122] 0.5 parts of defoaming agent;
[0123] 1 part wetting agent;
[0124] 1 part of dispersant;
[0125] 1.5 parts of thickener;
[0126] 6 parts of deionized water.
[0127] Example 6
[0128] The preparation method is prepared from the following raw materials in parts by weight: 20 parts of acrylic emulsion;
[0129] 20 parts of sodium silicate colloidal solution;
[0130] Expanded graphite 15 parts;
[0131] 15 parts of aluminum hydroxide;
[0132] 20 parts of diatomaceous earth;
[0133] 0.5 parts of defoaming agent;
[0134] 1 part wetting agent;
[0135] 1 part of dispersant;
[0136] 1.5 parts of thickener;
[0137] 6 parts of deionized water.
[0138] Example 7
[0139] It is prepared from the following raw materials by weight:
[0140] Acrylic emulsion 10 parts;
[0141] 20 parts of sodium silicate colloidal solution;
[0142] Expanded graphite 10 parts;
[0143] 20 parts of aluminum hydroxide;
[0144] 20 parts of diatomaceous earth;
[0145] 0.5 parts of defoaming agent;
[0146] 1 part wetting agent;
[0147] 1 part of dispersant;
[0148] 1.5 parts of thickener;
[0149] 6 parts of deionized water.
[0150] The preparation methods of the above-mentioned embodiments 1 to 7 are as follows:
[0151] Mix the raw material components evenly according to the formula to obtain the composite fireproof adhesive; the specific steps are as follows:
[0152] Pour expanded graphite, diatomaceous earth and aluminum hydroxide into a mixer in sequence and mix and stir for 30 minutes (150 r / min) to obtain a premix;
[0153] The acrylic emulsion, sodium silicate colloidal solution, defoamer, dispersant and wetting agent were sequentially added into the dispersion kettle and stirred at a low speed for 15 min (400 r / min) to obtain a mixed sol;
[0154] The premix is slowly added to the mixed sol under low-speed stirring, and then adjusted to high-speed dispersion for 45 minutes (1350r / min) to obtain a slurry; the slurry is then transported to a grinder through a conveying pipeline for sand grinding, and the slurry is sand ground to a suitable fineness of 50 to 70μm, and then the sand-ground slurry is adjusted to a suitable viscosity, with a rotational viscosity of 80000 to 120000MPa.s, and finally filtered, discharged and packaged to obtain a finished composite fireproof adhesive.
[0155] Various performance tests were performed on the composite fireproof adhesives provided in Examples 1 to 7, wherein the fire retardancy was measured according to the combustion characteristics of automobile interior materials in GB8410-2006. The results are shown in Table 1 below.
[0156] Table 1 Performance data of the composite fireproof adhesive provided in Examples 1 to 7
[0157]
[0158]
[0159] The test results show that: (1) When part of the sodium silicate colloidal solution is used to replace the acrylic emulsion in the formula, the fire retardant properties of the product become better as the proportion of the sodium silicate colloidal solution increases, but excessive addition of the sodium silicate colloidal solution will make the dried coating hard and brittle and crack, affecting the application of the product. The results show that the ratio of acrylic emulsion and sodium silicate colloidal solution in Example 3 has good fire retardant properties and other good comprehensive properties. (2) On the basis of Example 3, the fire retardant properties of the product are further improved by adjusting the ratio of expanded graphite and aluminum hydroxide. The results show that Example 6 has the best fire retardant effect.
[0160] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A composite fireproof adhesive, It is characterized in that It is prepared from raw materials including the following components: 10 to 30 parts by weight of water-based adhesive; 10 to 30 parts by weight of sodium silicate colloidal solution; 10 to 25 parts by weight of expanded graphite; 5 to 20 parts by weight of heat-absorbing powder; 15 to 25 parts by weight of inorganic filler; 0.2 to 0.8 parts by weight of defoamer; 0.5 to 1.5 parts by weight of wetting agent; 0.5 to 1.5 parts by weight of dispersant; 1 to 2 parts by weight of thickener; Water: 4 to 8 parts by weight.
2. The composite fireproof adhesive according to claim 1, It is characterized in that The water-based adhesive is acrylic emulsion.
3. The composite fireproof adhesive according to claim 1, It is characterized in that The preparation method of the sodium silicate colloidal solution is specifically as follows: Liquid caustic soda and quartz sand are mixed in a mass ratio of (2-4):1, reacted at 100-150°C to obtain a sodium silicate reaction liquid, and then the sodium silicate reaction liquid is filtered and concentrated to obtain a sodium silicate colloidal solution.
4. The composite fireproof adhesive according to claim 1, It is characterized in that The fineness of the expanded graphite is 600-800 meshes, and the expansion ratio is 180-250 times.
5. The composite fireproof adhesive according to claim 1, It is characterized in that The endothermic powder is aluminum hydroxide with a fineness of 600-800 meshes.
6. The composite fireproof adhesive according to claim 1, It is characterized in that The inorganic filler is selected from diatomaceous earth and / or heavy calcium carbonate; the fineness of the inorganic filler is 600-800 meshes.
7. The composite fireproof adhesive according to claim 1, It is characterized in that The defoamer is selected from one or more of modified siloxane, organosilicon defoamer and mineral oil defoamer.
8. The composite fireproof adhesive according to claim 1, It is characterized in that The dispersant is a sodium polyacrylate dispersant.
9. The composite fireproof adhesive according to claim 1, It is characterized in that The thickener is selected from polyurethane thickeners and / or acrylic thickeners.
10. A method for preparing the composite fireproof adhesive according to any one of claims 1 to 9, It is characterized in that The following steps are involved: a) stirring the expanded graphite, inorganic filler and endothermic powder at 100 r / min to 200 r / min for 20 min to 40 min to obtain a premix; b) stirring the aqueous binder, the sodium silicate colloidal solution, the defoamer, the dispersant, the wetting agent, the thickener and water at 300 r / min to 500 r / min for 10 to 20 min to obtain a mixed sol; c) adding the premix obtained in step a) to the mixed sol obtained in step b) under stirring at 300 r / min to 500 r / min, and then dispersing at 1300 r / min to 1400 r / min for 40 min to 50 min to obtain slurry; finally, the slurry is sand-milled, paint-mixed and filtered in sequence to obtain a composite fireproof adhesive after discharging.
Citation Information
Patent Citations
Water-based fireproof sealant and preparation method thereof
CN109735268A
Fireproof glue and preparation method thereof
CN112358818A
Elastic expansion heat absorption type fireproof coating, preparation method thereof, alumina-based fiber fireproof blanket and preparation method thereof
CN112647307A
Cited By
Fireproof silicone sealant with low smoke amount and preparation method thereof
CN119552630A