Highly environment-friendly modified epoxy resin adhesive based on earthquake prevention and disaster reduction
By using specific diluents and modifiers in the preparation of modified epoxy resin adhesives, combined with optimized formulas of curing agents and cross-linking agents, the bonding performance and performance of epoxy resin adhesives in earthquake prevention and disaster reduction applications are solved. The problem of improving environmental performance has enabled the preparation of efficient and environmentally friendly adhesives, which is suitable for bonding applications in complex environments.
Patent Information
- Application Number
- CN202410934413.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-15
AI Technical Summary
Existing modified epoxy resin adhesives are difficult to meet the requirements for high environmental performance and easy operation during the preparation process. Especially in earthquake prevention and disaster reduction applications, the bonding performance and environmental performance need to be further improved.
A highly environmentally friendly modified epoxy resin adhesive is prepared using a sequential step method, including using butyl glycidyl ether or 1,6-hexanediol diacrylate as diluent, and ethylenediamine or polyamide resin as modification Agent, acid anhydride and 1,4-butanediol diglycidyl ether are used as curing agent and cross-linking agent, ensuring uniform mixing through heating and stirring, and optimizing the formula to improve bonding performance.
The preparation of modified epoxy resin adhesive that is simple to operate, low in cost and highly environmentally friendly has been realized, which significantly improves the strength and adhesion of the adhesive, adapts to the bonding needs in complex environments, and reduces environmental pollution.
Smart Images

Figure CN118772816A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesive material preparation, and in particular relates to a method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction. Background Art
[0002] As a high-performance functional building material, epoxy resin has many excellent physical and chemical properties, such as high adhesion, small curing shrinkage, stable chemical properties, and excellent electrical insulation. Epoxy resin contains a variety of polar groups and highly active epoxy groups, so it has strong adhesion to a variety of polar materials such as metal, glass, cement, and wood, especially materials with high surface activity. At the same time, the cohesive strength of epoxy cured products is also very large, so its bonding strength is very high. And this adhesive has been widely used in many fields, plays a huge role in daily life, has broad application prospects, and is known as "universal glue" or "strong glue". In construction projects, epoxy resin can be bonded to a variety of materials such as metal, concrete, and wood. It is used to fix steel beams, steel plates, steel bars and other components in buildings, and can also be used to repair damaged building components; at the same time, epoxy resin can also be used as a coating to protect the surface of buildings and increase the service life of buildings. In recent years, with the demand for high-strength, lightweight and green environmentally friendly materials, more and more environmentally friendly epoxy resins have been used in construction projects. For example, in the repair of buildings after an earthquake, epoxy resin can quickly heal damaged parts and improve the earthquake resistance of buildings; in the field of building energy conservation, epoxy resin's low volatility and solvent-free characteristics make it an excellent thermal insulation material. At the same time, epoxy resin has good plasticity and corrosion resistance, making it an ideal choice for structural bonding of buildings such as aquariums and swimming pools.
[0003] The preparation of modified epoxy resin adhesives can be mainly modified by adding different types and proportions of diluents, modifiers, curing agents and other toughening agents to improve the comprehensive properties such as adhesion, toughness, and impact resistance. In the modification process, special attention is paid to the improvement of environmental performance, such as selecting non-toxic and harmless diluents, modifiers and curing agents to reduce the pollution of the adhesive to the environment during production and use. Therefore, exploring a simple and environmentally friendly preparation method for modified epoxy resin adhesives is of great significance to meet the ever-changing industrial needs. Summary of the invention
[0004] In order to solve the above problems, the object of the present invention is to provide a method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction.
[0005] In order to achieve the above-mentioned object, the method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction provided by the present invention comprises the following steps performed in sequence:
[0006] (1) Weigh 5-10 g of epoxy resin as the base resin and place it in a beaker. When the constant temperature heating device is heated to 75-80°C, place the beaker in the beaker and stir it. Measure 0.5-3.0 g of diluent and add it to the beaker. Stir for 2-3 minutes to ensure uniform heating until the epoxy resin is completely diluted. Take out the beaker and wait for 13-15 minutes to let it cool naturally.
[0007] (2) 0.4-1.2 g of a modifier is measured and slowly added dropwise to the diluted epoxy resin prepared in step (1), while continuously stirring to fully improve the properties of the mixed adhesive; and a curing agent and a cross-linking agent are measured in a mass ratio of 0.3-1.0:0.4-1.2, mixed as a bonding phase in a glass container, stirred to mix, and a mixed solution is obtained for use.
[0008] (3) Slowly pour the mixed solution prepared in step (2) into the modified mixed adhesive solution, and place it in a stirrer to mix it thoroughly until a modified epoxy resin adhesive is obtained.
[0009] 2. The method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction according to claim 1, characterized in that: the diluent in step (1) can be butyl glycidyl ether, 1,6-hexanediol diacrylate, etc. wherein the concentration of butyl glycidyl ether is 98-99% and the concentration of 1,6-hexanediol diacrylate is 90-95%.
[0010] Preferably, the modifier in step (2) may be ethylenediamine, polyamide resin, etc., the curing agent may be an acid anhydride, and the cross-linking agent may be 1,4-butanediol diglycidyl ether; the above are conventional chemicals and can be directly purchased.
[0011] Preferably, the operation sequence of step (2) is to first add a modifier to the epoxy resin diluted in step (1) to improve its properties, and then add a curing agent and a cross-linking agent to improve the bonding performance of the mixed glue.
[0012] Preferably, in step (2), the concentration of ethylenediamine is 97-99%, the particle size of the polyamide resin is 100-200 mesh, the concentration of the acid anhydride is 97-99%, and the concentration of 1,4-butanediol diglycidyl ether is 60-65%.
[0013] Preferably, the diluent, modifier and curing agent in steps (1) and (2) are all analytically pure, with a purity higher than 90%.
[0014] Preferably, steps (1), (2), and (3) require stirring to ensure that the epoxy resin and the adhesive are fully mixed for later use.
[0015] Preferably, the order of adding the raw materials in steps (1), (2) and (3) is as follows: the epoxy resin and the diluent are first mixed and heated, and stirred together; after cooling for 13-15 minutes, a certain proportion of the modifier is added to the diluted epoxy resin and stirred continuously; then, an appropriate amount of curing agent and cross-linking agent are added to the mixed adhesive solution and stirred continuously to obtain a modified epoxy resin adhesive.
[0016] The preparation method of the highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction provided by the present invention has the following beneficial effects:
[0017] 1. The preparation process is simple to operate, the formula design is optimized and reasonable, which improves production efficiency and shortens the preparation cycle.
[0018] 2. The raw materials are widely available and low in cost, which reduces production costs and enables mass production.
[0019] 3. The preparation process uses environmentally friendly materials and processes to reduce the emission of harmful substances and reduce environmental pollution.
[0020] 4. The prepared modified environmentally friendly epoxy resin adhesive has significantly improved strength and adhesion, and can better adapt to the bonding needs in various complex environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is an infrared test analysis diagram of the modified environmentally friendly epoxy resin adhesive prepared in Example 1. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with specific embodiments.
[0023] Example 1
[0024] The preparation method of the highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction provided in this embodiment includes the following steps performed in sequence:
[0025] (1) Weigh 5 g of epoxy resin as the base resin and place it in a beaker. When the constant temperature heating device is heated to 78°C, place the beaker in the beaker and stir it. Measure 0.5 g of 1,6-hexanediol diacrylate and add it to the beaker. Stir for 2 min to ensure uniform heating until the epoxy resin is completely diluted. Take out the beaker and wait for 14 min to let it cool naturally.
[0026] (2) 0.6 g of ethylenediamine is measured and slowly added dropwise to the diluted epoxy resin prepared in step (1), while continuously stirring to fully improve the properties of the mixed adhesive; and anhydride and 1,4-butanediol diglycidyl ether are measured in a mass ratio of 0.5:0.6, mixed as a binder phase in a glass container, stirred to mix, and a mixed solution is obtained for use.
[0027] (3) Pour the mixed solution prepared in step (2) into the modified mixed adhesive solution, and place it in a stirrer to mix it thoroughly until a modified epoxy resin adhesive is obtained.
[0028] Example 2
[0029] The preparation method of the highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction provided in this embodiment includes the following steps performed in sequence.
[0030] (1) Weigh 10 g of epoxy resin as the base resin and place it in a beaker. When the constant temperature heating device is heated to 80°C, place the beaker in the beaker and stir it. Measure 3.0 g of butyl glycidyl ether and add it to the beaker. Stir for 3 min to ensure uniform heating until the epoxy resin is completely diluted. Take out the beaker and wait for 15 min to let it cool naturally.
[0031] (2) 1.0 g of ethylenediamine is measured and slowly added dropwise to the diluted epoxy resin prepared in step (1), while continuously stirring to fully improve the properties of the mixed adhesive; and anhydride and 1,4-butanediol diglycidyl ether are measured in a mass ratio of 0.6:1.0, mixed as a binder phase in a glass container, stirred to mix, and a mixed solution is obtained for use.
[0032] (3) Slowly pour the mixed solution prepared in step (2) into the modified mixed adhesive solution, and place it in a stirrer to mix it thoroughly until a modified epoxy resin adhesive is obtained.
[0033] Example 3
[0034] The preparation method of the highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction provided in this embodiment includes the following steps performed in sequence:
[0035] (1) Weigh 5 g of epoxy resin as the base resin and place it in a beaker. When the constant temperature heating device is heated to 75°C, place the beaker in the beaker and stir it. Measure 0.5 g of 1,6-hexanediol diacrylate and add it to the beaker. Stir for 2 min to ensure uniform heating until the epoxy resin is completely diluted. Take out the beaker and wait for 13 min to let it cool naturally.
[0036] (2) 0.5 g of ethylenediamine is measured and slowly added dropwise to the diluted epoxy resin prepared in step (1), while continuously stirring to fully improve the properties of the mixed adhesive; and anhydride and 1,4-butanediol diglycidyl ether are measured in a mass ratio of 0.4:0.5, mixed as a binder phase in a glass container, stirred to mix, and a mixed solution is obtained for use.
[0037] (3) Slowly pour the mixed solution prepared in step (2) into the modified mixed adhesive solution, and place it in a stirrer to mix it thoroughly until a modified epoxy resin adhesive is obtained.
[0038] The highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction provided by the present invention uses epoxy resin as a base resin, butyl glycidyl ether and 1,6-hexanediol diacrylate as diluents, ethylenediamine and polyamide resin as modifiers, acid anhydride as a curing agent, and 1,4-butanediol diglycidyl ether as a cross-linking agent. By designing an orthogonal experimental table with four factors and three levels, the bonding effects of different formulas on rubber and steel at different curing temperatures are investigated, including bonding strength, peel strength testing and infrared spectrum analysis.
[0039] In order to verify the effect of the preparation method of the highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction provided in the above embodiment, the inventors conducted the following experiments:
[0040] (1) Prepare a modified environmentally friendly epoxy resin adhesive according to the method of Example 1.
[0041] (2) Preparation of bonded parts: The prepared epoxy resin adhesive was used to bond the steel plate and the rubber to prepare tensile shear test pieces and peel strength test pieces, and then cured at 200°C for 1 h.
[0042] (3) Bond strength and peel strength test: The shear test piece and the peel strength test piece were tested by using a microcomputer-controlled electronic universal testing machine with a servo motor driving the moving crossbeam up and down. After the test, the bond strength and peel strength of the adhesive after curing at 200°C were measured to be 27.19 MPa and 11.13 N / cm, respectively, which were both higher than the technical indicators, indicating that this preparation method can prepare modified epoxy resin adhesives with excellent performance.
[0043] (4) Infrared test: The adhesive cured at 200°C was ground into powder, and then the bonding composition was analyzed using a WQF-530 Fourier transform infrared analyzer, such as Figure 1 shown.
[0044] Depend on Figure 1 It can be seen that the greater the intensity of the epoxy group absorption peak, the higher the degree of crosslinking, which further indicates that the heat resistance, bonding strength and other properties of the prepared modified epoxy resin adhesive are better.
Claims
1. A method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction, characterized in that: The preparation method comprises the following steps performed in sequence: (1) Weigh 5-10 g of epoxy resin as the base resin and place it in a beaker. When the constant temperature heating device is heated to 75-80°C, place the beaker in the beaker and stir it. Measure 0.5-3.0 g of diluent and add it to the beaker. Stir for 2-3 minutes to ensure uniform heating until the epoxy resin is completely diluted. Take out the beaker and wait for 13-15 minutes to let it cool naturally. (2) 0.4-1.2 g of a modifier is measured and slowly added dropwise to the diluted epoxy resin prepared in step (1), while continuously stirring to fully improve the properties of the mixed adhesive; and a curing agent and a cross-linking agent are measured in a mass ratio of 0.3-1.0:0.4-1.2, mixed as a bonding phase in a glass container, stirred to mix, and a mixed solution is obtained for use. (3) Slowly pour the mixed solution prepared in step (2) into the modified mixed adhesive solution, and place it in a stirrer to mix it thoroughly until a modified epoxy resin adhesive is obtained.
2. The method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction according to claim 1, characterized in that: The diluent in step (1) can be butyl glycidyl ether, 1,6-hexanediol diacrylate, etc. wherein the concentration of butyl glycidyl ether is 98-99%, and the concentration of 1,6-hexanediol diacrylate is 90-95%.
3. The method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction according to claim 1, characterized in that: The modifier in step (2) can be ethylenediamine, polyamide resin, etc., the curing agent can be anhydride, and the cross-linking agent can be 1,4-butanediol diglycidyl ether; the above are conventional chemicals and can be directly purchased.
4. The method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction according to claim 1, characterized in that: The operation sequence of step (2) is to first add a modifier to the epoxy resin diluted in step (1) to improve its properties, and then add a curing agent and a cross-linking agent to improve the bonding performance of the mixed glue.
5. The method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction according to claim 1, characterized in that: In step (2), the concentration of ethylenediamine is 97-99%, the particle size of the polyamide resin is 100-200 meshes, the concentration of the acid anhydride is 97-99%, and the concentration of 1,4-butanediol diglycidyl ether is 60-65%.
6. The method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction according to claim 1, characterized in that: The diluent, modifier and curing agent in steps (1) and (2) are all analytically pure, with a purity higher than 90%.
7. The method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction according to claim 1, characterized in that: Steps (1), (2), and (3) require stirring to ensure that the epoxy resin and the adhesive are fully mixed for later use.
8. The method for preparing a highly environmentally friendly modified epoxy resin adhesive for earthquake prevention and disaster reduction according to claim 1, characterized in that: The order of adding the raw materials in steps (1), (2) and (3) is to first mix and heat the epoxy resin and the diluent, and stir them together; after cooling for 13-15 minutes, add a certain proportion of the modifier to the diluted epoxy resin and continue stirring; then add an appropriate amount of curing agent and cross-linking agent to the mixed adhesive solution and continue stirring to obtain a modified epoxy resin adhesive.