Weak acid-polyol-based adhesive as well as preparation method and application thereof

Through the preparation of weak acid-polyol-based adhesives, the problems of traditional adhesives with high curing temperature, long time and sticky glue are solved, achieving efficient gluing and stable storage at low temperatures, meeting the performance requirements of plywood, and avoiding the need for formaldehyde. Released, suitable for use in the plywood industry.

CN118772828AActive Publication Date: 2024-10-15NANJING FORESTRY UNIV

Patent Information

Application Number
CN202410979939.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-15
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

In the preparation of plywood, traditional petroleum-based adhesives have problems such as high curing temperature, long curing time, and high hot pressing temperature, resulting in low bonding strength of the plate and easy to cause brittleness of the board, and prone to glue lumps, which affects the performance and storage stability of the plywood. .

Method used

Weak acid-polyol-based adhesive is used, mainly made of lactic acid or oxalic acid, polyvinyl alcohol or polypropylene glycol, ferric trichloride hexahydrate or tetrabutyl titanate, diphenylmethane diisocyanate or epoxy resin and other raw materials Preparation, by low Using high-speed stirring and high-speed stirring reactions, an adhesive with a solid content of 50% to 60% and moderate viscosity is prepared, which can be hot pressed at 110 to 130°C to ensure the brittleness and bonding strength of the board and improve the glue phenomenon.

Benefits of technology

It achieves rapid curing and high-strength gluing at lower temperatures, avoids formaldehyde release, meets E0 grade standards, and the adhesive can still be used after being left for more than one month, improving the overall performance and application prospects of plywood.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004955744610000051
    Figure BDA0004955744610000051
  • Figure BDA0004955744610000052
    Figure BDA0004955744610000052
  • Figure BDA0004955744610000061
    Figure BDA0004955744610000061
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, in particular to a weak acid-polyol-based adhesive as well as a preparation method and application thereof. The weak acid-polyol-based adhesive provided by the invention is a green, environment-friendly and formaldehyde-free adhesive prepared by taking specific weak acid and polyol as matrixes, ferric trichloride hexahydrate or tetrabutyl titanate as a catalyst and diphenylmethane diisocyanate or epoxy resin as a curing agent. The raw materials of the adhesive are simple and easy to obtain, and the solid content is high. After the adhesive is used for preparing the plywood, the plywood can be pressed under the condition of 110-130 DEG C, and the brittleness of the plywood is not influenced while the bonding strength of the pressing plate is ensured; in addition, the hot pressing efficiency is improved by the adhesive, the adhesive lumping phenomenon is improved, the adhesive can still be used after being placed for more than one month, and the bonding quality is high. Therefore, the plywood with excellent comprehensive performance can be prepared by adopting the adhesive, and preparation and application of the high-quality plywood are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, and in particular to a weak acid-polyol-based adhesive and a preparation method and application thereof. Background Art

[0002] As a renewable natural resource, wood is increasingly widely used in the field of man-made panels. Plywood is one of the three major types of man-made panels. It is a three-layer or multi-layer board material made by peeling wood segments into veneers or planing wood blocks into veneers, and then gluing them with adhesives. Plywood can improve the utilization rate of wood and is the main way to save wood. It is also one of the commonly used materials for furniture. It is also widely used in aircraft, ships, trains, automobiles, construction, packaging boxes and other fields. The popularization and application of plywood in the industry is inseparable from the use of wood adhesives. At the same time, the increase in demand for plywood has further promoted the development of wood adhesives.

[0003] Traditional thermosetting resin adhesives based on petrochemicals are still the most widely used adhesives on the market due to their good economic advantages and performance. However, it cannot be ignored that the formaldehyde release problem caused by traditional petroleum-based adhesives has a huge impact on human health and the environment. Therefore, the development of sustainable and environmentally friendly formaldehyde-free adhesives has become the focus of research in the wood-based panel industry.

[0004] At present, technicians have developed a series of adhesive types made of environmentally friendly materials. However, in the application of plywood preparation, conventional adhesives still have the following problems that need to be solved: 1) High curing temperature and long curing time; 2) High hot pressing temperature, low bonding strength of the pressed board, and easy to affect the brittleness of the board; 3) Easy to have problems of glue clumping and difficult storage.

[0005] Therefore, how to develop a new type of environmentally friendly adhesive to comprehensively solve the above problems plays a key role in promoting the rational application of plywood and improving wood properties. Summary of the invention

[0006] In order to solve the above problems existing in the prior art, the purpose of the present invention is to provide a weak acid-polyol based adhesive, which is environmentally friendly and formaldehyde-free. After being used for plywood, it can be hot-pressed at 110-130°C without affecting the brittleness of the board. It has a fast curing speed and high curing strength, and the prepared plywood has excellent comprehensive performance. At the same time, the adhesive can improve the problem of glue clumping and can still be used after being placed for more than one month, and is suitable for use in the plywood industry.

[0007] At the same time, the present invention also aims to provide a method for preparing the above-mentioned weak acid-polyol-based adhesive.

[0008] At the same time, the present invention also aims to provide the application of the above-mentioned weak acid-polyol-based adhesive.

[0009] At the same time, the present invention also aims to provide a plywood.

[0010] To achieve the above object, the technical solution adopted by the present invention is:

[0011] A weak acid-polyol-based adhesive is mainly prepared from the following raw materials in parts by weight: 25-35 parts of weak acid, 16-24 parts of polyol, 3-5 parts of catalyst, 10-15 parts of curing agent, and 40-50 parts of water;

[0012] Wherein, the weak acid is lactic acid or oxalic acid; the polyol is polyvinyl alcohol or polypropylene glycol; the catalyst is ferric chloride hexahydrate or tetrabutyl titanate; and the curing agent is diphenylmethane diisocyanate or epoxy resin.

[0013] The solid content and viscosity of the adhesive are within a reasonable range, which can ensure that the adhesive can be hot-pressed at a temperature of 110-130°C without affecting the brittleness of the board. As a preferred embodiment of the present invention, the solid content of the weak acid-polyol based adhesive is 50%-60% and the viscosity is 20000-40000 mPa·s.

[0014] As a preferred embodiment of the present invention, the weak acid-polyol-based adhesive is mainly prepared from the following raw materials in parts by weight: 32.7 parts of weak acid, 17.3 parts of polyol, 5 parts of catalyst, 10 parts of curing agent, and 45 parts of water; wherein the weak acid is lactic acid; the polyol is polyvinyl alcohol; the catalyst is ferric chloride hexahydrate; the curing agent is diphenylmethane diisocyanate;

[0015] Alternatively, the weak acid-polyol based adhesive is mainly prepared from the following raw materials in parts by weight: 25.3 parts of weak acid, 21.7 parts of polyol, 3 parts of catalyst, 12.5 parts of curing agent, and 50 parts of water; wherein the weak acid is oxalic acid; the polyol is polypropylene glycol; the catalyst is tetrabutyl titanate; and the curing agent is epoxy resin.

[0016] The present invention has no particular limitation on the type of water used in the adhesive raw material, and any type of water used to prepare adhesives known to those skilled in the art can be used. As a preferred embodiment of the present invention, the water is distilled water.

[0017] As a preferred solution of the present invention, the polyvinyl alcohol is polyvinyl alcohol 1799; the polypropylene glycol is polypropylene glycol 400; and the epoxy resin is epoxy resin T31.

[0018] The preparation method of the above-mentioned weak acid-polyol-based adhesive comprises the following steps:

[0019] Step 1, mixing a weak acid, a polyol and water, and performing a low-speed stirring reaction;

[0020] Step 2, adding a catalyst to the system after the low-speed stirring reaction in step 1, and performing a high-speed stirring reaction;

[0021] Step 3, adding a curing agent to the system after the high-speed stirring reaction in step 2, and stirring until uniform, thereby obtaining the weak acid-polyol-based adhesive.

[0022] As a preferred embodiment of the present invention, the temperature of the low-speed stirring reaction is 80-90°C, the reaction time is 0.5-1h, and the stirring speed is 100-150r / min; the temperature of the high-speed stirring reaction is 90-110°C, the reaction time is 1-2h, and the stirring speed is 300-400r / min.

[0023] The above-mentioned weak acid-polyol based adhesive is used as an adhesive in the preparation of plywood.

[0024] A plywood is prepared by hot pressing the weak acid-polyol-based adhesive and a board; the board comprises a veneer and a core board.

[0025] As a preferred solution of the present invention, the method for preparing the plywood comprises the following steps:

[0026] The weak acid-polyol-based adhesive is evenly coated on one side of two veneers, and then the core board is placed on the glued side of one veneer, and then the glued side of another glued veneer is placed on the core board, keeping the wood grain directions perpendicular to each other to complete the assembly; the assembled boards are hot pressed to obtain the plywood.

[0027] As a preferred embodiment of the present invention, the double-sided sizing amount of the weak acid-polyol-based adhesive is 180-220 g / m 2 The hot pressing temperature is 110-130°C, the pressure is 1-1.5MPa, and the time is 8-12min.

[0028] Compared with the prior art, the beneficial effects of the present invention are:

[0029] The weak acid-polyol-based adhesive provided by the present invention is a green, environmentally friendly, formaldehyde-free adhesive suitable for the existing plywood industry, which is prepared with weak acid and polyol as a matrix, ferric chloride hexahydrate or tetrabutyl titanate as a catalyst, and diphenylmethane diisocyanate or epoxy resin as a curing agent. It can effectively avoid the problem of formaldehyde release. In addition, the raw materials of the adhesive are simple and easy to obtain, with a high solid content, and can be pressed at 110-130°C, while ensuring the bonding strength of the pressed plate without affecting the brittleness of the plate; in addition, the adhesive improves the hot pressing efficiency, improves the glue clumping phenomenon, and the adhesive can still be used after being placed for more than one month. The plywood prepared by the adhesive has excellent comprehensive performance, and solves the shortcomings of conventional plywood adhesives such as high curing temperature and long curing time, improves the gluing speed and gluing quality, and has good application prospects in the field of plywood.

[0030] The preparation method of the weak acid-polyol-based adhesive provided by the present invention uses a specific weak acid and a polyol to construct an adhesive matrix, uses tetrabutyl titanate or ferric chloride hexahydrate as a catalyst to catalyze the esterification reaction of the weak acid and the polyol during the synthesis process, and further uses epoxy resin or diphenylmethane diisocyanate to improve the curing rate and curing strength during the curing process, so as to prepare a new type of weak acid-polyol-based green adhesive. The viscosity of the adhesive is moderate, and the solid content can reach 50% to 60%. The prepared adhesive can be hot-pressed at a relatively low temperature (110 to 130° C.) and will not affect the brittleness of the sheet. In addition, the above method of the present invention uses simple and easy-to-obtain raw materials, a simple operation process, and no formaldehyde is generated during the reaction of the raw materials, which is green and environmentally friendly.

[0031] The plywood prepared by the adhesive of the present invention has a formaldehyde emission of ≤0.4 mg / L, which meets the requirements of the E0 grade of plywood in the group standard T / CNFPIA 1001-2019 "Limits of Formaldehyde Emission from Artificial Boards". In addition, the bonding strength is greater than 0.7 MPa, which meets the requirements of Class II plywood in the national standard GB / T 9846-2015 "Ordinary Plywood". Therefore, the adhesive of the present invention is very suitable for use in the plywood industry. DETAILED DESCRIPTION

[0032] The technical scheme and technical effects of the present invention will be clearly and completely described below in conjunction with specific embodiments and test examples. However, it should be understood by those skilled in the art that the embodiments are only used to illustrate the technical scheme of the present invention and should not be regarded as limiting the scope of protection of the present invention. The test methods used in the following examples are conventional methods unless otherwise specified; the raw materials used are all commonly used in the art, available to the public or commercially available, unless otherwise specified.

[0033] In the present invention, there is no special limitation on the types of polyvinyl alcohol, polypropylene glycol and epoxy resin, which only need to ensure the performance of the adhesive. Preferably, in the following embodiments, the polyvinyl alcohol is polyvinyl alcohol 1799; the polypropylene glycol is polypropylene glycol 400; and the epoxy resin is epoxy resin T31.

[0034] The present invention has no particular limitation on the type of water used in the adhesive raw material, and any type of water used to prepare adhesives known to those skilled in the art can be used. Preferably, in the following embodiments, the water is distilled water.

[0035] Example 1

[0036] This embodiment provides a weak acid-polyol-based adhesive, which is mainly prepared from the following raw materials in parts by weight: 32.7 parts of lactic acid, 17.3 parts of polyvinyl alcohol, 5 parts of ferric chloride hexahydrate, 10 parts of diphenylmethane diisocyanate, and 45 parts of water. The weak acid-polyol-based adhesive has a solid content of 55% and a viscosity of 38344 mPa·s after testing.

[0037] This embodiment also provides a method for preparing the above-mentioned weak acid-polyol-based adhesive, comprising the following steps:

[0038] Step 1, lactic acid, polyvinyl alcohol and water are mixed, and reacted at 90° C. with low-speed stirring (150 r / min) for 1 hour;

[0039] Step 2, adding ferric chloride hexahydrate to the system after the reaction in step 1, and reacting at 100° C. with high-speed stirring (400 r / min) for 1 hour;

[0040] Step three, adding diphenylmethane diisocyanate to the system after the reaction in step two, stirring until uniform, to obtain the weak acid-polyol based adhesive of this embodiment.

[0041] This embodiment also provides the use of the above-mentioned weak acid-polyol-based adhesive in the preparation of plywood.

[0042] This embodiment also provides a plywood, which is prepared by hot pressing the above-mentioned weak acid-polyol-based adhesive with a board; the board includes a veneer and a core board. The preparation method of plywood includes the following steps: evenly apply the weak acid-polyol-based adhesive on one side of two veneers, then place the core board on the glued side of one veneer, and then place the glued side of another glued veneer on the core board, keeping the wood grain directions perpendicular to each other to complete the assembly; then use a hot press to hot press the assembled board to obtain plywood, which is placed at room temperature before use. Among them, the double-sided glue application amount of the adhesive when used is 200g / m 2 The hot pressing temperature was 130°C, the pressure was 1.3 MPa, and the time was 10 min.

[0043] Example 2

[0044] This embodiment provides a weak acid-polyol-based adhesive, which is mainly prepared from the following raw materials in parts by weight: 25.3 parts of oxalic acid, 21.7 parts of polypropylene glycol, 3 parts of tetrabutyl titanate, 12.5 parts of epoxy resin, and 50 parts of water. The weak acid-polyol-based adhesive has a solid content of 50% and a viscosity of 23752 mPa·s after testing.

[0045] This embodiment also provides a method for preparing the above-mentioned weak acid-polyol-based adhesive, comprising the following steps:

[0046] Step 1, oxalic acid, polypropylene glycol and water are mixed, and reacted at 80° C. with low speed stirring (100 r / min) for 0.5 hour;

[0047] Step 2, adding tetrabutyl titanate to the system after the reaction in step 1, and reacting at 95° C. with high-speed stirring (300 r / min) for 1.5 hours;

[0048] Step three, adding epoxy resin to the system after the reaction in step two, stirring until uniform, to obtain the weak acid-polyol based adhesive of this embodiment.

[0049] This embodiment also provides the use of the above-mentioned weak acid-polyol-based adhesive in the preparation of plywood.

[0050] This embodiment also provides a plywood, which is prepared by hot pressing the above-mentioned weak acid-polyol-based adhesive with a board; the board includes a veneer and a core board. The preparation method of the plywood includes the following steps: evenly apply the weak acid-polyol-based adhesive on one side of two veneers, then place the core board on the glued side of one veneer, and then place the glued side of another glued veneer on the core board, keeping the wood grain directions perpendicular to each other to complete the assembly; then use a hot press to hot press the assembled board to obtain plywood, which is placed at room temperature before use. Among them, the double-sided glue application amount of the adhesive when used is 220g / m 2 The hot pressing temperature was 110°C, the pressure was 1.4 MPa, and the time was 12 min.

[0051] Test Example 1: Catalyst Test

[0052] This test example investigates the effects of adhesives prepared with different types of catalysts and different amounts of catalysts on the mechanical properties of plywood (dry shear strength, dry wood breakage rate, wet shear strength, wet wood breakage rate) after being applied to the preparation of plywood. Among them, in each test group, when preparing the adhesive, except for the different types or amounts of catalysts, other adhesive compositions and preparation processes are the same as in Example 1, and the process conditions for preparing plywood with the adhesive are also carried out with reference to Example 1. After the plywood is prepared, the plywood obtained in each test group is subjected to performance tests. Among them, Table 1 shows the effects of different types of catalysts on the performance of plywood when the catalyst dosage is 5 parts. Table 2 shows the effects of different catalyst dosages on the performance of plywood when the catalyst is ferric chloride hexahydrate.

[0053] Table 1. Effect of catalyst type on plywood properties

[0054]

[0055] Table 2. Effect of catalyst dosage on plywood properties

[0056]

[0057] From the results of Table 1 and Table 2, it can be seen that Example 1 of the present invention uses ferric chloride hexahydrate as a catalyst and when the addition amount is 5 parts, catalyzes the esterification reaction of weak acid and polyol, can achieve the best bonding strength (0.85MPa), and the wood breakage rate is moderate, so that the board can be effectively prevented from breaking, and the brittleness of the board is not significantly affected. In addition, further tests show that the bonding strength of the plywood obtained in Example 2 is 0.76MPa, which meets the requirements of Class II plywood in the national standard GB / T 9846-2015 "Ordinary Plywood".

[0058] Test Example 2: Hot Press Test

[0059] This test example investigates the effects of different hot pressing temperatures and hot pressing times on the dry shear strength, dry wood breakage rate, wet shear strength, and wet wood breakage rate of plywood. When preparing plywood, except for changing the hot pressing temperature and time, other raw material compositions and process parameters are the same as those in Example 1. The settings of the hot pressing temperature and time and the test results are shown in Table 3.

[0060] Table 3. Effects of hot pressing temperature and time on plywood properties

[0061]

[0062] As shown in Table 3, the shear strength of plywood increases with the increase of hot pressing temperature and hot pressing time. When the hot pressing temperature is 110℃, it has met the requirements of the national standard GB / T 9846-2015 (≥0.7MPa). In addition, considering that too high a temperature will damage the wood structure in the wood and cause the wood to break, and during the hot pressing process, the wood is easy to carbonize, affecting the color and easy to break. Therefore, the hot pressing condition finally determined is 110-130℃ hot pressing for 10 minutes.

[0063] Test Example 3: Formaldehyde Release Test

[0064] This test example is carried out in accordance with the 4.61 dryer method in the national standard GB / T 17657-2022 "Test Methods for Physical and Chemical Properties of Artificial Boards and Faced Artificial Boards" to determine the formaldehyde emission of the plywood in Example 1 and Example 2. The test process is: 300-500mL of distilled water is placed at the bottom of the glass dryer, a stainless steel wire sample holder is placed, 10 plywood specimens with a length of 150mm and a width of 50mm are placed on the stainless steel wire support net, and the formaldehyde released by the specimens is collected. Prepare formaldehyde calibration solution and acetylacetone-ammonium acetate solution, accurately draw 25mL of formaldehyde solution into a 100mL stoppered conical flask, and measure 25mL of acetylacetone-ammonium acetate solution, plug the bottle stopper, and shake well. Then put it in a water bath at (65±2)℃ and heat it for 10min, then put the solution in a dark place at 20℃ and store it for (60±5)min, and use a spectrophotometer to measure the absorbance of the solution at a wavelength of 412nm. The same method is used to determine the background concentration of formaldehyde. The concentration of the formaldehyde solution is calculated according to the formula.

[0065] The concentration of formaldehyde solution is calculated according to formula (1), accurate to 0.01 mg / L:

[0066] c = f × (A S - A b ) × 1800 / A (1)

[0067] Wherein, c represents the mass concentration of formaldehyde, in milligrams per liter (mg / L); f is the slope of the standard curve, in milligrams per milliliter (mg / mL); A s A is the absorbance of formaldehyde solution; b represents the absorbance of the blank solution; A is the surface area of ​​the specimen, in square centimeters (cm 2 ). The results are shown in Table 4.

[0068] Table 4. Formaldehyde emission from plywood

[0069]

[0070] It can be seen from Table 4 that the plywood prepared by the weak acid-polyol based adhesive of the present invention has a formaldehyde emission of ≤0.4 mg / L, which meets the requirements of the E0 grade of plywood in the group standard T / CNFPIA 1001-2019 "Formaldehyde Emission Limits for Artificial Panels".

[0071] Test Example 4: Storage Test

[0072] This test example investigates the effect of different days of storage of the adhesive on the performance of plywood. The specific operation is: the weak acid-polyol-based adhesive of Example 1 is stored for 7 days, 14 days, 21 days, 28 days, and 35 days, and then three-layer plywood is prepared and mechanical strength tested according to the plywood process in Example 1. The results are shown in Table 5.

[0073] Table 5. Effect of adhesive storage days on plywood performance

[0074]

[0075]

[0076] As shown in Table 5, the weak acid-polyol green adhesive stored for more than one month can still be used, and the prepared plywood meets the requirements of Class II plywood in the national standard GB / T 9846-2015 "Ordinary Plywood". This shows that the adhesive of the present invention is not prone to glue clumping, has high bonding strength, and the prepared plywood has excellent comprehensive performance.

[0077] In summary, the weak acid-polyol-based adhesive provided by the present invention is a green, environmentally friendly, formaldehyde-free adhesive prepared with weak acid and polyol as the matrix, which is suitable for the existing plywood industry and can effectively avoid the problem of formaldehyde release. In addition, the raw materials of the adhesive are simple and easy to obtain, with a high solid content, and can be pressed at 110-130°C, while ensuring the bonding strength of the pressed plate without affecting the brittleness of the board; in addition, the adhesive improves the efficiency of hot pressing, improves the phenomenon of glue clumping, and the adhesive can still be used after being placed for more than one month. The plywood made of the adhesive has excellent comprehensive performance, and solves the shortcomings of conventional plywood adhesives such as high curing temperature and long curing time, improves the gluing speed and gluing quality, and has good application prospects in the field of plywood.

Claims

1. A weak acid-polyol based adhesive, characterized in that: It is mainly prepared from the following raw materials in parts by weight: 25-35 parts of weak acid, 16-24 parts of polyol, 3-5 parts of catalyst, 10-15 parts of curing agent, and 40-50 parts of water; Wherein, the weak acid is lactic acid or oxalic acid; the polyol is polyvinyl alcohol or polypropylene glycol; the catalyst is ferric chloride hexahydrate or tetrabutyl titanate; and the curing agent is diphenylmethane diisocyanate or epoxy resin.

2. The weak acid-polyol based adhesive according to claim 1, characterized in that: The weak acid-polyol based adhesive has a solid content of 50% to 60% and a viscosity of 20000 to 40000 mPa•s.

3. The weak acid-polyol based adhesive according to claim 1, characterized in that: The weak acid-polyol-based adhesive is mainly prepared from the following raw materials in parts by weight: 32.7 parts of weak acid, 17.3 parts of polyol, 5 parts of catalyst, 10 parts of curing agent, and 45 parts of water; wherein the weak acid is lactic acid; the polyol is polyvinyl alcohol; the catalyst is ferric chloride hexahydrate; and the curing agent is diphenylmethane diisocyanate; Alternatively, the weak acid-polyol based adhesive is mainly prepared from the following raw materials in parts by weight: 25.3 parts of weak acid, 21.7 parts of polyol, 3 parts of catalyst, 12.5 parts of curing agent, and 50 parts of water; wherein the weak acid is oxalic acid; the polyol is polypropylene glycol; the catalyst is tetrabutyl titanate; and the curing agent is epoxy resin.

4. The weak acid-polyol based adhesive according to claim 1 or 3, characterized in that: The polyvinyl alcohol is polyvinyl alcohol 1799; the polypropylene glycol is polypropylene glycol 400; and the epoxy resin is epoxy resin T31.

5. A method for preparing a weak acid-polyol based adhesive as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1, mixing a weak acid, a polyol and water, and performing a low-speed stirring reaction; Step 2, adding a catalyst to the system after the low-speed stirring reaction in step 1, and performing a high-speed stirring reaction; Step 3, adding a curing agent to the system after the high-speed stirring reaction in step 2, and stirring until uniform, thereby obtaining the weak acid-polyol-based adhesive.

6. The method for preparing the weak acid-polyol based adhesive according to claim 5, characterized in that: The temperature of the low-speed stirring reaction is 80-90°C, the reaction time is 0.5-1h, and the stirring speed is 100-150r / min; the temperature of the high-speed stirring reaction is 90-110°C, the reaction time is 1-2h, and the stirring speed is 300-400r / min.

7. An application of the weak acid-polyol based adhesive according to any one of claims 1 to 4, characterized in that: Used as adhesive in the preparation of plywood.

8. A plywood, characterized in that: The board is prepared by hot pressing the weak acid-polyol-based adhesive as described in any one of claims 1 to 4 with a board; the board includes a veneer and a core board.

9. The plywood according to claim 8, characterized in that The method for preparing the plywood comprises the following steps: The weak acid-polyol-based adhesive is evenly coated on one side of two veneers, and then the core board is placed on the glued side of one veneer, and then the glued side of another glued veneer is placed on the core board, keeping the wood grain directions perpendicular to each other to complete the assembly; the assembled boards are hot pressed to obtain the plywood.

10. The plywood according to claim 9, characterized in that The double-sided sizing amount of the weak acid-polyol based adhesive is 180-220 g / m 2 ; The hot pressing is performed at a temperature of 110-130° C., a pressure of 1-1.5 MPa, and a time of 8-12 min.

Citation Information

Patent Citations

  • Adhesive for aldehyde-free plywood, and preparation method thereof, and plywood and preparation method thereof

    CN110872481A

  • Environment-friendly adhesive for organic acid-polyol-based formaldehyde-free high-performance plywood as well as preparation method and application of environment-friendly adhesive

    CN116355560A

  • Adhesive for wood and method for manufacturing plywood

    JP2006257272A

Cited By

  • Preparation method and application of adhesive for low-temperature curing high-bonding-strength environment-friendly plywood

    CN119119926A