Bi-component photocurable acrylate composite adhesive and preparation method thereof
Through the design of a two-component photocurable acrylic composite adhesive, combined with components such as isocyanate-terminated polyurethane prepolymer and polyol, an IPN structure with excellent bonding properties is formed, solving the problem of acrylate pressure-sensitive adhesive and polyurethane The problem of insufficient flexibility and weather resistance after curing of the glue is eliminated, and high bonding strength and stability are achieved.
Patent Information
- Application Number
- CN202410879592.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-15
AI Technical Summary
The acrylate pressure-sensitive adhesive film has poor flexibility after curing and cross-linking, and the polyurethane adhesive has insufficient water resistance and weather resistance after curing and cross-linking, and cannot meet the demand for high bonding quality.
A two-component photocurable acrylic composite adhesive is used to form an IPN structure with excellent bonding strength and stability by combining isocyanate-terminated polyurethane prepolymer with polyol, polyurethane catalyst, photocurable monomer and other components. , and introduce nano-silicon nitride to improve weather resistance.
It achieves good tensile strength, water resistance, weather resistance and low temperature resistance flexibility of the adhesive film, meets the curing speed requirements of different application scenarios, and improves the overall bonding stability and impact resistance toughness.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of adhesives, and in particular to a two-component photocurable acrylate composite adhesive and a preparation method thereof. Background Art
[0002] Acrylic pressure-sensitive adhesive is a photocurable industrial adhesive material with the advantages of fast curing speed and high bonding strength. It is widely used in industrial fields such as automobiles, aviation, and construction. However, the adhesive film formed after curing and cross-linking has poor flexibility, which makes it easy to crack and split at the joint, limiting its promotion and application.
[0003] Polyurethane glue has excellent shear strength, flexibility and impact resistance, and is suitable for various structural bonding fields. However, the adhesive film formed after curing and cross-linking has relatively poor water resistance and weather resistance, and cannot provide long-term and stable bonding effects, which limits its promotion and application.
[0004] In order to improve the problem of poor film flexibility of the above-mentioned acrylic pressure-sensitive adhesive, the prior art mixes water-based acrylic pressure-sensitive emulsion and water-based polyurethane emulsion to form a WPU / PA composite pressure-sensitive latex system. Although the water resistance, weather resistance and flexibility of the resulting adhesive layer are improved, the molecular weight of the polymer chain segment formed by cross-linking in the aqueous system is low, resulting in its overall tensile strength and bonding strength being average, and unable to meet the requirements of high bonding quality in specific application scenarios. To this end, the present application provides a two-component photocurable acrylic composite adhesive and a preparation method thereof. Summary of the invention
[0005] In order to solve the above technical problems, the present application provides a two-component photocurable acrylate composite adhesive and a preparation method thereof.
[0006] The present application provides a two-component photocurable acrylate composite adhesive, which is realized by the following technical scheme:
[0007] A two-component photocurable acrylate composite adhesive comprises component A and component B, wherein component A is composed of the following raw materials in parts by mass: 5-20 parts of an isocyanate-terminated polyurethane prepolymer, 60-80 parts of an acrylate-based resin, 80-200 parts of an organic solvent, and 4-8 parts of a multi-arm polyethylene glycol having a plasticizing effect;
[0008] The B component comprises the following raw materials in parts by weight: 0.05-0.3 parts of a chain extender, 0.5-2 parts of a polyol, 0.05-0.40 parts of a polyurethane catalyst, 0.05-0.5 parts of an initiator, and 1-5 parts of a photocurable monomer;
[0009] The acrylate-based resin in the A component includes one of methacrylate and acrylate;
[0010] The molar amount of -active NCO in the isocyanate-terminated polyurethane prepolymer in component A is 1.05-1.20 times the total molar amount of active functional groups in the chain extender and polyol in component B;
[0011] The polyurethane catalyst is composed of organic bismuth and latent organic polysilazane;
[0012] The organic solvent is at least one of ethyl acetate, acetone, butanone and toluene;
[0013] The chain extender is a small molecule diol; the polyol is polybutadiene diol combined with at least one of polyether polyol, polyester polyol and polycarbonate polyol with a molecular weight of 500-3000;
[0014] The initiator is at least one of potassium persulfate, azobisisobutyl cyanide, ethyl vinyl sulfide and photoinitiator 1173, photoinitiator 184, and photoinitiator TPO;
[0015] The photocurable monomer includes at least one of tris(2-hydroxyethyl)isocyanurate triacrylate, 3(propoxy)propylene glycol triacrylate, and 4(ethoxy)pentaerythritol tetraacrylate.
[0016] The two-component polyurethane adhesive in the present application can achieve dual curing of light curing and heat curing. The content and composition of the curing agent in the two-component polyurethane adhesive can be adjusted to adjust the overall curing speed to meet the needs of different application scenarios, while providing excellent bonding strength and bonding stability. The resulting adhesive layer has good tensile strength, water resistance, weather resistance, and low-temperature resistance and flexibility.
[0017] Preferably, the acrylate-based resin in component A is composed of α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000-5000, methyl methacrylate, and hydroxyethyl methacrylate in a molar ratio of (0.05-0.20):(2-4):(0.5-1).
[0018] By introducing a soft segment of α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000-5000 into the cross-linked network structure, the overall low-temperature toughness and impact toughness are effectively improved while ensuring the overall bonding strength.
[0019] Preferably, the isocyanate-terminated polyurethane prepolymer comprises diisocyanate, triisocyanate, small molecule diol, polyol, organic bismuth and antioxidant; the polyol is composed of polybutadiene diol, polyether polyol and polycarbonate polyol in a molar ratio of (0.1-0.5):(2-4):(1-2); the diisocyanate is an aliphatic isocyanate or a mixture of an aliphatic isocyanate and an aliphatic isocyanate; the small molecule diol is 1,6-hexanediol and / or 3-methyl-1,5-pentanediol; the triisocyanate is at least one of triphenylmethane triisocyanate, L-lysine triisocyanate and 4,4',4"-triphenylmethane triisocyanate.
[0020] Preferably, the preparation method of the isocyanate-terminated polyurethane prepolymer is as follows: the polyol is heated to 100-110°C and dehydrated under vacuum conditions for 1-4h, the dehydrated polyol obtained is evenly mixed with organic bismuth, antioxidant, small molecule diol, and diisocyanate, and then heated to 60-80°C to react until the system viscosity is 6*103-8*103mPa·s / 25°C, and triisocyanate is added for end-capping treatment. The end-capping reaction conditions are: react at 75-80°C for 1-2h to obtain an isocyanate-terminated polyurethane prepolymer.
[0021] Preferably, the -active NCO molar amount of the isocyanate-terminated polyurethane prepolymer in the A component is 1.18-1.20 times the total molar amount of the active functional groups in the chain extender and the polyol in the B component; the chain extender in the isocyanate-terminated polyurethane prepolymer is a combination of butene glycol and at least one of 1,4-butanediol, 1,6-hexanediol, and 3-methyl-1,5-pentanediol.
[0022] By adopting the above scheme, the introduction of polyurethane molecular chain segments can improve the overall low-temperature toughness and impact toughness. At the same time, the small amount of double bonds contained in the polyurethane molecular chain segments can provide cross-linking points with acrylate-based resins, thereby improving the overall tensile strength.
[0023] Preferably, the initiator is azobisisobutyl cyanide and the photoinitiator TPO in a mass ratio of (0.5-2):(1-2).
[0024] Preferably, the multi-arm polyethylene glycol having a plasticizing effect is a two-arm methacrylate-based, two-arm glycidyl-based, four-arm polyethylene glycol with a molecular weight of 1000-5000.
[0025] By adopting the above technical solution, multi-arm polyethylene glycol with a plasticizing effect is used as the solvent of the polyurethane system, thereby achieving effective adjustment of the viscosity of the finished two-component photocurable acrylic composite adhesive to meet the needs of different application scenarios.
[0026] Preferably, the photocurable monomer is tris(2-hydroxyethyl)isocyanurate triacrylate and 4(ethoxy)pentaerythritol tetraacrylate in a mass ratio of (0.2-0.4):1.
[0027] By adopting the above technical solution, the flexibility, heat resistance and wear resistance of the cured adhesive film can be improved.
[0028] Preferably, the B component further comprises 1-4 parts of nano silicon nitride, and the nano silicon nitride is at least surface-modified by methacryloxysilane.
[0029] By adopting the above technical solution, good weather resistance and reinforcement performance can be achieved, and the overall UV aging resistance can be improved.
[0030] The present application provides a method for preparing a two-component photocurable acrylate composite adhesive, which is achieved by the following scheme:
[0031] A method for preparing a two-component photocurable acrylate composite adhesive comprises the following steps:
[0032] Step 1, preparation of isocyanate terminated polyurethane prepolymer;
[0033] Step 2, preparation of component A: place the accurately measured isocyanate-terminated polyurethane prepolymer, acrylate-based resin, organic solvent, and multi-arm polyethylene glycol with plasticizing effect in a reaction kettle, and stir evenly at 0-10° C. under nitrogen protection to obtain component A;
[0034] At the same time, prepare component B: place the chain extender, polyol, polyurethane catalyst, initiator, and photocurable monomer in a reaction kettle, and stir evenly at 0-10°C under nitrogen protection to obtain component B;
[0035] Step 3: When using, stir component A and component B evenly at 0-10°C under nitrogen protection.
[0036] A method for preparing a two-component photocurable acrylate composite adhesive comprises the following steps:
[0037] Step 1, preparation of isocyanate terminated polyurethane prepolymer;
[0038] Step 2, preparation of component A: place the accurately measured isocyanate-terminated polyurethane prepolymer, acrylate-based resin, organic solvent, and multi-arm polyethylene glycol with plasticizing effect in a reaction kettle, and stir evenly at 0-10° C. under nitrogen protection to obtain component A;
[0039] At the same time, prepare component B: place chain extender, polyol, polyurethane catalyst, initiator, and photocurable monomer in a reaction kettle, stir at 120-240 rpm for 5-20 min at 0-10°C under nitrogen protection, then add accurately measured nano silicon nitride, stir at 80-160 rpm for 20-60 min at 0-10°C and kettle pressure of 0.06-0.08 MPa to prepare component B;
[0040] Step 3: When using, stir component A and component B evenly at 0-10°C under nitrogen protection.
[0041] The preparation method provided in this application is relatively simple, relatively easy to implement, and easy to realize industrial production and manufacturing.
[0042] In summary, this application has the following advantages:
[0043] 1. The two-component polyurethane adhesive in this application can achieve dual curing of light curing and heat curing, and can adjust the overall curing speed while providing the IPN structure formed by curing to ensure that the overall has excellent bonding strength and bonding stability. At the same time, the resulting adhesive layer has good tensile strength, impact toughness, water resistance, weather resistance, and low temperature toughness.
[0044] 2. The preparation method provided in this application is relatively simple, relatively easy to implement, and easy to realize industrial production and manufacturing. DETAILED DESCRIPTION
[0045] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.
[0046] Example
[0047] A two-component photocurable acrylate composite adhesive comprises component A and component B, wherein component A is composed of the following raw materials in parts by mass: 5-20 parts of isocyanate-terminated polyurethane prepolymer, 60-80 parts of acrylate-based resin, 80-200 parts of organic solvent, and 4-8 parts of multi-arm polyethylene glycol with plasticizing effect. Component B comprises the following raw materials in parts by mass: 0.05-0.3 parts of chain extender, 0.5-2 parts of polyol, 0.05-0.40 parts of polyurethane catalyst, 0.05-0.5 parts of initiator, and 1-5 parts of photocurable monomer.
[0048] The acrylate-based resin in component A includes one of methacrylate and acrylate.
[0049] Preferably, the acrylate-based resin is composed of α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000-5000, methyl methacrylate, and hydroxyethyl methacrylate in a molar ratio of (0.05-0.20):(2-4):(0.5-1).
[0050] The isocyanate-terminated polyurethane prepolymer includes diisocyanate, triisocyanate, small molecule diol, polyol, organic bismuth and antioxidant. The polyol is composed of polybutadiene diol, polyether polyol and polycarbonate polyol in a molar ratio of (0.1-0.5):(2-4):(1-2). The diisocyanate is an aliphatic isocyanate or a mixture of an aliphatic isocyanate and an aliphatic isocyanate. The small molecule diol is 1,6-hexanediol and / or 3-methyl-1,5-pentanediol. The triisocyanate is at least one of triphenylmethane triisocyanate, L-lysine triisocyanate and 4,4',4"-triphenylmethane triisocyanate.
[0051] The preparation method of the isocyanate-terminated polyurethane prepolymer is as follows: the polyol is heated to 100-110°C and dehydrated under vacuum for 1-4 hours, the dehydrated polyol obtained is mixed with organic bismuth, antioxidant, small molecule diol and diisocyanate, and then heated to 60-80°C to react until the system viscosity reaches 6*10 3 -8*10 3 mPa·s / 25℃, add triisocyanate for end-capping treatment. The end-capping reaction conditions are: react at 75-80℃ for 1-2h to obtain isocyanate-terminated polyurethane prepolymer.
[0052] The molar amount of -active NCO in the isocyanate-terminated polyurethane prepolymer in component A is 1.05-1.20 times the total molar amount of active functional groups in the chain extender and polyol in component B. Preferably, the molar amount of -active NCO in the isocyanate-terminated polyurethane prepolymer in component A is 1.18-1.20 times the total molar amount of active functional groups in the chain extender and polyol in component B. The chain extender in the isocyanate-terminated polyurethane prepolymer is at least one of butene glycol and 1,4-butanediol, 1,6-hexanediol, and 3-methyl-1,5-pentanediol.
[0053] The polyurethane catalyst is composed of organic bismuth and latent organic polysilazane.
[0054] The organic solvent is at least one of ethyl acetate, acetone, butanone and toluene. Preferably, the organic solvent is ethyl acetate.
[0055] The chain extender is a small molecule diol, such as at least one of 1,4-butanediol, 1,6-hexanediol, and 3-methyl-1,5-pentanediol.
[0056] The polyol is polybutadiene diol combined with at least one of polyether polyol, polyester polyol and polycarbonate polyol with a molecular weight of 500-3000.
[0057] The initiator is potassium persulfate, azobisisobutyl cyanide, ethyl vinyl sulfide, and at least one of photoinitiator 1173, photoinitiator 184, and photoinitiator TPO. Preferably, the initiator is azobisisobutyl cyanide and photoinitiator TPO in a mass ratio of (0.5-2): (1-2). The multi-arm polyethylene glycol with plasticizing effect is a two-arm methacrylate two-arm glycidyl type four-arm polyethylene glycol with a molecular weight of 1000-5000.
[0058] The photocurable monomer includes at least one of tris(2-hydroxyethyl)isocyanuric acid triacrylate, 3(propoxy)propylene glycol triacrylate, and 4(ethoxy)pentaerythritol tetraacrylate. Preferably, the photocurable monomer is tris(2-hydroxyethyl)isocyanuric acid triacrylate and 4(ethoxy)pentaerythritol tetraacrylate in a mass ratio of (0.2-0.4):1.
[0059] A method for preparing a two-component photocurable acrylate composite adhesive comprises the following steps:
[0060] Step 1, preparation of isocyanate terminated polyurethane prepolymer;
[0061] Step 2, preparation of component A: place the accurately measured isocyanate-terminated polyurethane prepolymer, acrylate-based resin, organic solvent, and multi-arm polyethylene glycol with plasticizing effect in a reaction kettle, and stir evenly at 0-10° C. under nitrogen protection to obtain component A;
[0062] At the same time, prepare component B: place the chain extender, polyol, polyurethane catalyst, initiator, and photocurable monomer in a reaction kettle, and stir evenly at 0-10°C under nitrogen protection to obtain component B;
[0063] Step 3: When using, stir component A and component B evenly at 0-10°C under nitrogen protection.
[0064] In order to improve the overall anti-purple aging performance, component B also includes 1-4 parts of nano silicon nitride, which is at least surface-modified by methacryloxysilane. In the preparation process of component B: put the chain extender, polyol, polyurethane catalyst, initiator, and photocuring monomer in a reaction kettle, under nitrogen protection, stir at 120-240rpm for 5-20min at 0-10℃, then add the accurately measured nano silicon nitride, stir at 80-160rpm for 20-60min at 0-10℃ and kettle pressure of 0.06-0.08MPa to prepare component B.
[0065] Example 1: A two-component photocurable acrylate composite adhesive includes component A and component B. Component A is made of 8 parts of isocyanate-terminated polyurethane prepolymer, 72 parts of butyl methacrylate, 80 parts of ethyl ester, and 4 parts of two-arm methacrylate-based, two-arm glycidyl-type four-arm polyethylene glycol with a molecular weight of 1000 (purchased from Sinobond).
[0066] Component B is made of 0.12 parts of 3-methyl-1,5-pentanediol, 0.2 parts of polyester polyol PLOS-ZY1200 with a number average molecular weight of 2000, 0.4 parts of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.05 parts of bismuth carboxylate, 0.25 parts of organic polysilazane MY 9150, 0.1 parts of azobisisobutyl cyanide, 0.3 parts of photoinitiator TPO, and 4 parts of tris(2-hydroxyethyl)isocyanurate triacrylate.
[0067] The isocyanate-terminated polyurethane prepolymer is made of 0.80 mol (134.55 g) of hexamethylene diisocyanate (Wanhua HDI), 0.1 mol (26.72 g) of L-lysine triisocyanate, 74.45 g of 3-methyl-1,5-pentanediol, 88 g of polybutadiene diol (hydroxy-terminated polybutadiene of Tianyuan Aerospace Materials, hydroxyl value 0.5±0.03 mmol / g), 296 g of polycarbonate diol PCDL 1012 with a number average molecular weight of 2000, 0.5 g of bismuth carboxylate, and 5 g of antioxidant BHT.
[0068] A method for preparing a two-component photocurable acrylate composite adhesive comprises the following steps:
[0069] Step 1, preparation of an isocyanate-terminated polyurethane prepolymer: heating a polycarbonate diol PCDL 1012 with a number average molecular weight of 2000 to 110° C. and dehydrating it under vacuum for 3 hours; mixing the dehydrated polycarbonate diol PCDL 1012 with a number average molecular weight of 2000, hydroxyl-terminated polybutadiene, bismuth carboxylate, antioxidant BHT, 3-methyl-1,5-pentanediol, and hexamethylene diisocyanate, heating the mixture to 78±0.5° C. and reacting the mixture until the system viscosity reaches 6000-8000 mPa·s / 25° C.; adding L-lysine triisocyanate for end-capping treatment; the end-capping reaction conditions are: reacting at 78±0.5° C. for 80 minutes to obtain an isocyanate-terminated polyurethane prepolymer; the -active NCO molar amount of the isocyanate-terminated polyurethane prepolymer in component A is 1.1875 times the total molar amount of the active functional groups in the chain extender and the polyol in component B;
[0070] Step 2, preparation of component A: place the accurately measured isocyanate-terminated polyurethane prepolymer in step 1, butyl methacrylate, ethyl methacrylate, toluene, two-arm methacrylate group and two-arm glycidyl type four-arm polyethylene glycol in a reaction kettle, and stir at 160 rpm for 5 min at 4±0.5°C under nitrogen protection to obtain component A;
[0071] At the same time, component B was prepared: 3-methyl-1,5-pentanediol, polyester polyol PLOS-ZY1200 with a number average molecular weight of 2000, polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, bismuth carboxylate, organic polysilazane MY 9150, azobisisobutyl cyanide, photoinitiator TPO, and tris(2-hydroxyethyl)isocyanuric acid triacrylate were placed in a reaction kettle, and stirred at 160 rpm for 5 min at 4±0.5°C under nitrogen protection to obtain component B;
[0072] Step 3: When using, stir component A and component B at 160 rpm for 8 min at 4±0.5°C under nitrogen protection to obtain a two-component light-curable acrylate composite adhesive. The two-component light-curable acrylate composite adhesive is applied as follows: at room temperature, the light irradiation equipment has a power of 60-80 W·cm -1 Medium pressure mercury lamp with a light intensity of 400-450mW·cm -2 , the illumination time is 4-8s; or in an oven at 85℃, the illumination equipment power is 60-80W·cm -1 The medium pressure mercury lamp has a light intensity of 400-450mW·cm for two-component light-curable acrylic composite adhesive. -2 , the lighting time is 1-3s.
[0073] The difference between Example 2 and Example 1 is that component A is composed of 8 parts of isocyanate-terminated polyurethane prepolymer, 52 parts of methyl methacrylate, 10 parts of hydroxyethyl methacrylate, 10 parts of α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000 (purchased from Sinobond), 80 parts of ethyl ester, and 4 parts of two-arm methacrylate with a molecular weight of 1000, two-arm glycidyl type four-arm polyethylene glycol.
[0074] The difference between Example 3 and Example 1 is that the isocyanate-terminated polyurethane prepolymer is made of 134.55 g of hexamethylene diisocyanate, 26.72 g of L-lysine triisocyanate, 74.45 g of 3-methyl-1,5-pentanediol, 88 g of polybutadiene diol, 236.8 g of polycarbonate diol PCDL 1012 with a number average molecular weight of 2000, 29.6 g of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.5 g of bismuth carboxylate, and 5 g of antioxidant BHT.
[0075] The difference between Example 4 and Example 1 is that the isocyanate-terminated polyurethane prepolymer is made of 134.55 g of hexamethylene diisocyanate, 36.74 g of triphenylmethane triisocyanate, 74.45 g of 3-methyl-1,5-pentanediol, 88 g of polybutadiene diol, 236.8 g of polycarbonate diol PCDL 1012 with a number average molecular weight of 2000, 29.6 g of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.5 g of bismuth carboxylate, and 5 g of antioxidant BHT.
[0076] The difference between Example 5 and Example 1 is that component B is made of 0.12 parts of 3-methyl-1,5-pentanediol, 0.2 parts of polyester polyol PLOS-ZY1200 with a number average molecular weight of 2000, 0.4 parts of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.05 parts of bismuth carboxylate, 0.25 parts of organic polysilazane MY 9150, 0.3 parts of azobisisobutyl cyanide, 0.1 parts of photoinitiator TPO, and 4 parts of tris(2-hydroxyethyl)isocyanurate triacrylate.
[0077] The difference between Example 6 and Example 1 is that component B is made of 0.12 parts of 3-methyl-1,5-pentanediol, 0.2 parts of polyester polyol PLOS-ZY1200 with a number average molecular weight of 2000, 0.4 parts of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.05 parts of bismuth carboxylate, 0.25 parts of organic polysilazane MY 9150, 0.1 parts of azobisisobutyl cyanide, 0.3 parts of ethyl vinyl sulfide, 1 part of tris(2-hydroxyethyl)isocyanuric acid triacrylate, and 3 parts of tris(2-hydroxyethyl)isocyanuric acid triacrylate.
[0078] The difference between Example 7 and Example 1 is that component A is made of 12 parts of isocyanate-terminated polyurethane prepolymer, 52 parts of methyl methacrylate, 10 parts of hydroxyethyl methacrylate, 10 parts of α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000, 80 parts of ethyl ester, and 6 parts of two-arm methacrylate-ω-glycidyl four-arm polyethylene glycol with a molecular weight of 1000.
[0079] Component B is made of 0.18 parts of 3-methyl-1,5-pentanediol, 0.3 parts of polyester polyol PLOS-ZY1200 with a number average molecular weight of 2000, 0.6 parts of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.08 parts of bismuth carboxylate, 0.32 parts of organic polysilazane MY 9150, 0.1 parts of azobisisobutyl cyanide, 0.3 parts of photoinitiator TPO, and 4 parts of tris(2-hydroxyethyl)isocyanurate triacrylate.
[0080] The difference between Example 8 and Example 1 is that component A is made of 20 parts of isocyanate-terminated polyurethane prepolymer, 52 parts of methyl methacrylate, 10 parts of hydroxyethyl methacrylate, 10 parts of α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000, 80 parts of ethyl ester, and 8 parts of two-arm methacrylate-ω-glycidyl four-arm polyethylene glycol with a molecular weight of 1000.
[0081] Component B is made of 0.3 parts of 3-methyl-1,5-pentanediol, 0.5 parts of polyester polyol PLOS-ZY1200 with a number average molecular weight of 2000, 0.75 parts of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.12 parts of bismuth carboxylate, 0.42 parts of organic polysilazane MY 9150, 0.1 parts of azobisisobutyl cyanide, 0.3 parts of photoinitiator TPO, and 4 parts of tris(2-hydroxyethyl)isocyanurate triacrylate.
[0082] The difference between Example 9 and Example 1 is that component A is made of 12 parts of isocyanate-terminated polyurethane prepolymer, 52 parts of methyl methacrylate, 10 parts of hydroxyethyl methacrylate, 10 parts of α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000, 80 parts of ethyl ester, and 6 parts of two-arm methacrylate-ω-glycidyl four-arm polyethylene glycol with a molecular weight of 1000. The isocyanate-terminated polyurethane prepolymer is prepared from 134.55 g of hexamethylene diisocyanate, 26.72 g of L-lysine triisocyanate, 74.45 g of 3-methyl-1,5-pentanediol, 88 g of polybutadiene diol, 236.8 g of polycarbonate diol PCDL 1012 with a number average molecular weight of 2000, 29.6 g of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.5 g of bismuth carboxylate, and 5 g of antioxidant BHT.
[0083] Component B is made of 0.18 parts of 3-methyl-1,5-pentanediol, 0.3 parts of polyester polyol PLOS-ZY1200 with a number average molecular weight of 2000, 0.6 parts of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.08 parts of bismuth carboxylate, 0.32 parts of organic polysilazane MY 9150, 0.1 parts of azobisisobutyl cyanide, 0.3 parts of photoinitiator TPO, 1 part of tris(2-hydroxyethyl)isocyanurate triacrylate, and 3 parts of tris(2-hydroxyethyl)isocyanurate triacrylate.
[0084] The difference between Example 10 and Example 1 is that component A is made of 12 parts of isocyanate-terminated polyurethane prepolymer, 52 parts of methyl methacrylate, 10 parts of hydroxyethyl methacrylate, 10 parts of α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000, 80 parts of ethyl ester, and 6 parts of two-arm methacrylate-ω-glycidyl four-arm polyethylene glycol with a molecular weight of 1000. The isocyanate-terminated polyurethane prepolymer is prepared from 134.55 g of hexamethylene diisocyanate, 26.72 g of L-lysine triisocyanate, 74.45 g of 3-methyl-1,5-pentanediol, 88 g of polybutadiene diol, 236.8 g of polycarbonate diol PCDL 1012 with a number average molecular weight of 2000, 29.6 g of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.5 g of bismuth carboxylate, and 5 g of antioxidant BHT.
[0085] Component B is made of 0.18 parts of 3-methyl-1,5-pentanediol, 0.3 parts of polyester polyol PLOS-ZY1200 with a number average molecular weight of 2000, 0.6 parts of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.08 parts of bismuth carboxylate, 0.32 parts of organic polysilazane MY 9150, 0.1 parts of azobisisobutyl cyanide, 0.3 parts of photoinitiator TPO, 1 part of tris(2-hydroxyethyl)isocyanuric acid triacrylate, 3 parts of tris(2-hydroxyethyl)isocyanuric acid triacrylate, and 3 parts of α-nano silicon nitride (brand Ron, average particle size 20nm). Nano silicon nitride is surface modified with KH570 coupling agent (γ-methacryloxypropyltrimethoxysilane). Specifically, 5 g of α-nano silicon nitride was placed in 200 mL of KH570 coupling agent aqueous solution (the KH570 coupling agent content in the KH570 coupling agent aqueous solution was 5 wt%), and then magnetically stirred at 200 rpm for 10 min and ultrasonically dispersed for 0.5 h, with an ultrasonic frequency of 44 kHz and an ultrasonic power of 450 W. After the ultrasonic dispersion treatment was completed, the mixture was allowed to stand for 0.5 h, drained and taken out, and then placed under 95° C. / 0.10 Pa for 1 h of vacuum drying to obtain the finished α-nano silicon nitride.
[0086] A method for preparing a two-component photocurable acrylate composite adhesive comprises the following steps:
[0087] Step 1, preparation of an isocyanate-terminated polyurethane prepolymer: heating a polycarbonate diol PCDL 1012 with a number average molecular weight of 2000 and a polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000 to 110° C. and dehydrating them under vacuum for 3 hours respectively; the dehydrated polycarbonate diol PCDL1012 with a number average molecular weight of 2000 and the polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, hydroxyl-terminated polybutadiene, bismuth carboxylate, antioxidant BHT, 3-methyl-1,5-pentanediol, and hexamethylene diisocyanate are uniformly mixed and then heated to 78±0.5° C. to react until the system viscosity reaches 6000-8000 mPa·s / 25° C., and then L-lysine triisocyanate is added for end-capping treatment. The end-capping reaction conditions are: 78±0.5° C. for reaction for 80 minutes to obtain an isocyanate-terminated polyurethane prepolymer;
[0088] Step 2, preparation of component A: accurately measure the isocyanate-terminated polyurethane prepolymer in step 1, methyl methacrylate, hydroxyethyl methacrylate, α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000, ethyl ester, toluene, two-arm methacrylate with a molecular weight of 1000, and two-arm glycidyl four-arm polyethylene glycol in a reaction kettle, and stir at 160 rpm for 5 min at 4±0.5°C under nitrogen protection to obtain component A;
[0089] At the same time, component B is prepared: 3-methyl-1,5-pentanediol, polyester polyol PLOS-ZY1200 with a number average molecular weight of 2000, polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, bismuth carboxylate, organic polysilazane MY 9150, azobisisobutyl cyanide, photoinitiator TPO, 1 part of tris(2-hydroxyethyl)isocyanuric acid triacrylate, and 3 parts of tris(2-hydroxyethyl)isocyanuric acid triacrylate are placed in a reaction kettle, and stirred at 120 rpm for 10 min at 4±0.5°C under nitrogen protection, and then the nano silicon nitride surface modified by KH570 coupling agent is accurately measured and stirred at 100 rpm for 30 min at 4±0.5°C and a kettle pressure of 0.06-0.065 MPa to obtain component B;
[0090] Step 3: When using, stir component A and component B at 120 rpm for 10 min at 4±0.5°C under nitrogen protection to obtain a two-component photocurable acrylate composite adhesive.
[0091] The difference between Comparative Example 1 and Example 1 is that a two-component photocurable acrylate composite adhesive includes component A and component B, wherein component A is made of 80 parts of butyl methacrylate and 80 parts of ethyl methacrylate, and component B is made of 0.1 parts of azobisisobutyl cyanide, 0.3 parts of ethyl vinyl sulfide, and 4 parts of tris(2-hydroxyethyl)isocyanurate triacrylate.
[0092] The difference between Comparative Example 2 and Example 1 is that component A is made of 8 parts of isocyanate-terminated polyurethane prepolymer, 72 parts of butyl methacrylate, 80 parts of ethyl acetate, and 10 parts of acetone.
[0093] The difference between Comparative Example 3 and Example 1 is that a two-component photocurable acrylate composite adhesive includes component A and component B, wherein component A is made of 8 parts of allnex EBECRYL 4396 aliphatic polyurethane acrylate, 72 parts of butyl methacrylate, 75 parts of ethyl ester, and 15 parts of acetone. Component B is made of 0.1 parts of azobisisobutyl cyanide, 0.3 parts of photoinitiator TPO, and 4 parts of tris(2-hydroxyethyl)isocyanurate triacrylate.
[0094] The difference between Comparative Example 4 and Example 1 is that the isocyanate-terminated polyurethane prepolymer is made of 200.2g of 4,4'-diphenylmethane diisocyanate MDI, 37.6g of end-capping agent-4,4'-diphenylmethane diisocyanate, 41.64g of ethylene glycol, 88g of polybutadiene diol, 200g of polycarbonate diol PCDL 1012 with a number average molecular weight of 2000, 70g of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.5g of bismuth carboxylate, and 5g of antioxidant BHT. Preparation of isocyanate-terminated polyurethane prepolymer: 200g of polycarbonate diol PCDL with a number average molecular weight of 2000 1012 and 70g of polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000 are heated to 110°C and dehydrated under vacuum conditions for 3h. The dehydrated polycarbonate diol PCDL1012 with a number average molecular weight of 2000, polytetramethylene ether glycol PTMEG BASF PolyTHF with a number average molecular weight of 1000, 0.5g of bismuth carboxylate, 5g of antioxidant BHT, 41.64g of ethylene glycol, and 200.2g of 4,4'-diphenylmethane diisocyanate MDI are mixed evenly and heated to 72±0.5°C to react until the system viscosity is 6000-8000mPa·s / 25°C, and then 37.6g of 4,4'-diphenylmethane diisocyanate MDI is added for end-capping treatment. The end-capping reaction conditions are: 72±0.5°C for reaction for 60min to obtain an isocyanate-terminated polyurethane prepolymer.
[0095] Performance test: 1. Tensile strength and tensile fracture rate test method: Preparation of adhesive film: The two-component photocurable acrylate composite adhesive in Examples 1-10 and Comparative Examples 1-4 were coated on release paper at a power of 80 W·cm -1 The medium pressure mercury lamp has a light intensity of 450mW·cm -2 , after the illumination time is 5s, it is placed at a temperature of 85°C and a humidity of 65% RH for heat curing for 5 minutes to form a standard dumbbell-shaped specimen film; the standard dumbbell-shaped specimen film is subjected to a tensile test on an electronic tensile testing machine at a tensile rate of 50mm / min. 2. Test method for moisture and heat aging resistance: The prepared standard dumbbell-shaped specimen film is placed at 85°C / 85% RH and aged for 21 days, and then the tensile strength and tensile fracture rate are tested. 3. 180 peel strength test method: It is measured according to the ASTM D3330 test method. 4. Low-temperature folding resistance: The two-component photocurable acrylate composite adhesive in Examples 1-10 and Comparative Examples 1-4 are respectively coated on the SOLIV microfiber cloth, with a thickness of 45-50 microns and a power of 80W·cm -1 The medium pressure mercury lamp has a light intensity of 450mW·cm -2After the illumination time is 5s, they are placed at a temperature of 85°C and a humidity of 65% RH for heat curing for 5min, namely test samples 1-10 and control test samples 1-4. After the test samples 1-10 and control test samples 1-4 are placed in an environment of 80°C and 85% humidity for 504 hours, they are bent 5,000 times (bending angle 22.5°) at -20°C using a CS-6078-RL leather low-temperature folding tester to observe whether they crack.
[0096] Table 1: Test parameter table of two-component photocurable acrylate composite adhesive in Examples 1-10 and Comparative Examples 1-4
[0097]
[0098]
[0099] It can be seen from Examples 1-10 and Comparative Example 1 and Table 1 that the two-component polyurethane adhesive in the present application can achieve dual curing of light curing and heat curing, can adjust the overall curing speed while providing excellent bonding strength and bonding stability, and the resulting adhesive layer has good tensile strength, water resistance, weather resistance, and low temperature resistance and flexibility.
[0100] Combining Examples 1-10 and Comparative Example 2 with Table 1, it can be seen that the use of two-arm methacrylate-based, two-arm glycidyl-based four-arm polyethylene glycol with a molecular weight of 1000 can act as a plasticizer and improve the flexibility of the formed film. The α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000 in Example 2 can also act as a plasticizer, which is beneficial to improving the resilience, bonding strength, and low-temperature impact toughness of the formed film.
[0101] It can be seen from Examples 1-10 and Comparative Example 4 and Table 1 that the use of homemade isocyanate-terminated polyurethane prepolymers can improve the mechanical properties, resilience, bonding strength, and low-temperature impact toughness of the film formed by the cured cross-linking.
[0102] Combining Example 1 and Example 3-4 with Table 1, it can be seen that the comprehensive performance of the adhesive film formed by cross-linking the isocyanate-terminated polyurethane prepolymer terminated with L-lysine triisocyanate is relatively good. And the comprehensive performance of the adhesive film formed by cross-linking the polyurethane prepolymer prepared with polybutadiene diol, polycarbonate diol PCDL 1012, polytetramethylene ether glycol PTMEG BASF PolyTHF as polyols is relatively good.
[0103] It can be seen from Example 1 and Example 5 and Table 1 that the initiator composition formed by compounding azobisisobutyl cyanide and photoinitiator TPO in a mass ratio of 1:3 can better improve the mechanical properties of the adhesive film formed by cross-linking.
[0104] It can be seen from Example 1 and Example 6 and Table 1 that the photocurable monomer formed by compounding tris(2-hydroxyethyl)isocyanurate triacrylate and tris(2-hydroxyethyl)isocyanurate triacrylate can improve the mechanical properties, low temperature flexibility, weather resistance and bonding strength of the cross-linked film.
[0105] Combining Example 1 and Examples 7-8 with Table 1, it can be seen that the addition amount of the homemade isocyanate-terminated polyurethane prepolymer is preferably controlled to be 8-12 parts, which can ensure the mechanical properties, low temperature flexibility, weather resistance and bonding strength of the cross-linked film.
[0106] It can be seen from Example 1 and Examples 9-10 and Table 1 that the addition of α-nano silicon nitride can improve the aging resistance and weather resistance of the effective film while ensuring the bonding strength and mechanical properties of the film formed by cross-linking.
[0107] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A two-component photocurable acrylate composite adhesive, Features: It includes component A and component B. The component A is composed of the following raw materials in parts by mass: 5-20 parts of isocyanate-terminated polyurethane prepolymer, 60-80 parts of acrylate-based resin, 80-200 parts of organic solvent, and 4-8 parts of multi-arm polyethylene glycol with plasticizing effect; The B component comprises the following raw materials in parts by weight: 0.05-0.3 parts of a chain extender, 0.5-2 parts of a polyol, 0.05-0.40 parts of a polyurethane catalyst, 0.05-0.5 parts of an initiator, and 1-5 parts of a photocurable monomer; The acrylate-based resin in the A component includes one of methacrylate and acrylate; The molar amount of -active NCO in the isocyanate-terminated polyurethane prepolymer in component A is 1.05-1.20 times the total molar amount of active functional groups in the chain extender and polyol in component B; The polyurethane catalyst is composed of organic bismuth and latent organic polysilazane; The organic solvent is at least one of ethyl acetate, acetone, butanone and toluene; The chain extender is a small molecule diol; the polyol is polybutadiene diol combined with at least one of polyether polyol, polyester polyol and polycarbonate polyol with a molecular weight of 500-3000; The initiator is at least one of potassium persulfate, azobisisobutyl cyanide, ethyl vinyl sulfide and photoinitiator 1173, photoinitiator 184, and photoinitiator TPO; The photocurable monomer includes at least one of tris(2-hydroxyethyl)isocyanurate triacrylate, 3(propoxy)propylene glycol triacrylate, and 4(ethoxy)pentaerythritol tetraacrylate.
2. A two-component photocurable acrylate composite adhesive according to claim 1, Features: The acrylate resin in the component A is composed of α-methacrylate-ω-glycidyl polyethylene glycol with a molecular weight of 2000-5000, methyl methacrylate, and hydroxyethyl methacrylate in a molar ratio of (0.05-0.20):(2-4):(0.5-1).
3. A two-component photocurable acrylate composite adhesive according to claim 1, Features: The isocyanate-terminated polyurethane prepolymer comprises diisocyanate, triisocyanate, small molecule diol, polyol, organic bismuth and antioxidant; the polyol is composed of polybutadiene diol, polyether polyol and polycarbonate polyol in a molar ratio of (0.1-0.5):(2-4):(1-2); the diisocyanate is an aliphatic isocyanate or a mixture of an aliphatic isocyanate and an aliphatic isocyanate; the small molecule diol is 1,6-hexanediol and / or 3-methyl-1,5-pentanediol; the triisocyanate is at least one of triphenylmethane triisocyanate, L-lysine triisocyanate and 4,4',4"-triphenylmethane triisocyanate.
4. A two-component photocurable acrylate composite adhesive according to claim 3, Features: The preparation method of the isocyanate-terminated polyurethane prepolymer is as follows: the polyol is heated to 100-110° C. and dehydrated under vacuum for 1-4 hours, the dehydrated polyol obtained is mixed with organic bismuth, antioxidant, small molecule diol and diisocyanate, and then heated to 60-80° C. to react until the system viscosity reaches 6*10 3 -8*10 3 mPa·s / 25℃, add triisocyanate for end-capping treatment. The end-capping reaction conditions are: react at 75-80℃ for 1-2h to obtain isocyanate-terminated polyurethane prepolymer.
5. The two-component photocurable acrylate composite adhesive according to claim 1, Features: The chain extender in the isocyanate-terminated polyurethane prepolymer is a combination of butene glycol and at least one of 1,4-butanediol, 1,6-hexanediol, and 3-methyl-1,5-pentanediol.
6. A two-component photocurable acrylate composite adhesive according to claim 1, Features: The initiator is azobisisobutyl cyanide and photoinitiator TPO in a mass ratio of (0.5-2):(1-2); the multi-arm polyethylene glycol with plasticizing effect is a two-arm methacrylate-based, two-arm glycidyl-based, four-arm polyethylene glycol with a molecular weight of 1000-5000.
7. The two-component photocurable acrylate composite adhesive according to claim 1, Features: The photocurable monomer is composed of tris(2-hydroxyethyl)isocyanurate triacrylate and 4(ethoxy)pentaerythritol tetraacrylate in a mass ratio of (0.2-0.4):
1.
8. The two-component photocurable acrylate composite adhesive according to claim 1, Features: The B component also includes 1-4 parts of nano silicon nitride, and the nano silicon nitride is at least surface-modified by methacryloxysilane.
9. A method for preparing a two-component photocurable acrylate composite adhesive according to any one of claims 1 to 7, Features: The method comprises the following steps: step 1, preparing an isocyanate-terminated polyurethane prepolymer; Step 2, preparation of component A: place the accurately measured isocyanate-terminated polyurethane prepolymer, acrylate-based resin, organic solvent, and multi-arm polyethylene glycol with plasticizing effect in a reaction kettle, and stir evenly at 0-10° C. under nitrogen protection to obtain component A; At the same time, prepare component B: place the chain extender, polyol, polyurethane catalyst, initiator, and photocurable monomer in a reaction kettle, and stir evenly at 0-10°C under nitrogen protection to obtain component B; Step 3: When using, stir component A and component B evenly at 0-10°C under nitrogen protection.
10. A method for preparing the two-component photocurable acrylate composite adhesive according to claim 8, Features: The method comprises the following steps: step 1, preparing an isocyanate-terminated polyurethane prepolymer; Step 2, preparation of component A: place the accurately measured isocyanate-terminated polyurethane prepolymer, acrylate-based resin, organic solvent, and multi-arm polyethylene glycol with plasticizing effect in a reaction kettle, and stir evenly at 0-10° C. under nitrogen protection to obtain component A; At the same time, prepare component B: place chain extender, polyol, polyurethane catalyst, initiator, and photocurable monomer in a reaction kettle, stir at 120-240 rpm for 5-20 min at 0-10°C under nitrogen protection, then add accurately measured nano silicon nitride, stir at 80-160 rpm for 20-60 min at 0-10°C and kettle pressure of 0.06-0.08 MPa to prepare component B; Step 3: When using, stir component A and component B evenly at 0-10°C under nitrogen protection.
Citation Information
Cited By
Acrylic hardening coating, preparation method thereof and acrylic product
CN119799154A