Ultraviolet light and moisture dual-curing sulfur-resistant three-proofing adhesive and preparation method thereof
Polyurethane acrylate oligomer dual-cured by UV light and moisture, combined with a combination of polyols, forms a cross-linked network, which solves the problem of insufficient sulfur resistance of three-proof adhesives in harsh environments and achieves high sulfur resistance. , adhesion and weather resistance three-proof adhesive.
Patent Information
- Application Number
- CN202411266615.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing three-proof adhesives have insufficient sulfur resistance in harsh environments such as high temperature, high humidity, and salt spray, and cannot effectively prevent sulfide corrosion.
Using UV and moisture dual-cured polyurethane acrylate oligomer, through the combination of diisocyanate, polyester diol, polyester triol and phenyl grafted polybutadiene polyol, double bond groups and The sterically hindered groups form a rich cross-linked network, improve the compactness and adhesion of the film, and enhance the sulfur resistance.
The sulfur resistance, adhesion and weather resistance of the three-proof adhesive have been significantly improved. It can provide strong protective performance in harsh environments and has other excellent properties such as acid and alkali resistance and salt spray resistance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of adhesives, and in particular to a sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, and a preparation method thereof. Background Art
[0002] As electronic products gradually turn to miniaturization, integration and multi-function, the electronic assembly industry is also developing rapidly, and the requirements for the safety performance and reliability of assembled products are becoming higher and higher. Since electronic devices usually need to withstand environments such as high temperature, high dust, humidity, salt spray and mold, consumers are now paying more and more attention to the quality and reliability of products. "Three protections (moisture-proof, salt spray-proof, anti-static)" are mentioned and valued by more and more manufacturers.
[0003] At present, the most widely used three-conformal paint in the market is solvent-based. With the increasingly stringent requirements on safety production, solvent-free three-conformal paint has gradually emerged. UV-curable three-conformal paint has been more and more widely used due to its safety, extremely fast curing speed, excellent moisture resistance and chemical resistance. However, the sulfur-containing substances produced by factors such as natural gas production, crude oil refining, automobile exhaust emissions, and chemical pollution are also gradually increasing. These substances will be further converted into elemental sulfur and H2S under heat or other catalytic effects, and then cause sulfide corrosion to electronic components in related environments. Therefore, in addition to ensuring the excellent protective performance of the three-conformal glue itself, it is imperative to further improve its anti-sulfurization performance. Summary of the invention
[0004] In order to overcome the problem of insufficient sulfur resistance of the above-mentioned prior art dual-curing three-proof adhesive, the present application provides a sulfur-resistant three-proof adhesive that can be dual-cured by ultraviolet light and moisture and a preparation method thereof.
[0005] In the first aspect, the present application provides a sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, using the following technical solution: A sulfur-resistant triple-proof adhesive capable of dual curing by ultraviolet light and moisture comprises the following components in parts by weight: 30-60 parts of dual-curing polyurethane acrylate oligomer, 20-50 parts of acrylic active monomer, 0.1-5 parts of leveling agent, 0.1-5 parts of defoaming agent, 3-8 parts of photoinitiator and 0.05-0.5 parts of polymerization inhibitor.
[0006] By adopting the above technical scheme, a polyurethane acrylate oligomer that is dual-cured by ultraviolet light and moisture is synthesized. On the one hand, the polyurethane acrylate molecule contains acrylic functional groups and urethane bonds, which improves the high wear resistance, adhesion, flexibility, high peel strength and excellent low-temperature resistance of polyurethane and the excellent optical properties and weather resistance of polyacrylate. On the other hand, the polyurethane acrylate oligomer that is dual-cured by ultraviolet light and moisture improves the reaction activity of the UV light curing reaction, making the three-proof adhesive coating cure faster and improving the efficiency of the sizing process.
[0007] The polyurethane acrylate oligomer and the photoinitiator are then mixed, and the acrylate end participates in photocuring to obtain a UV-curing polyurethane acrylate resin, which provides initial strength for the adhesive. At the same time, a three-proof adhesive is prepared by synthesizing a polyurethane acrylate oligomer that is dual-cured by UV light and moisture, and a specific ratio of acrylic active monomers that participate in moisture curing. This allows the three-proof adhesive to have more double bond groups, increases the density of the cross-linking reaction, provides the adhesive with later bonding strength and toughness, increases the elongation at break, and makes the adhesive layer denser, so that the protective performance in harsh atmospheres such as salt spray and high humidity is stronger. It has both high vulcanization resistance and excellent properties such as acid and alkali resistance and salt spray resistance, and can meet the use requirements of various devices.
[0008] In a specific embodiment, the dual-cured polyurethane acrylate oligomer is synthesized by: (1) taking polyester diol, polyester triol, and phenyl-grafted polybutadiene polyol, respectively, and removing water in a vacuum at 120° C. for 4 hours for later use; (2) Take 2 mol of diisocyanate and 0.01-0.1 mol of catalyst, heat to 65-75°C under nitrogen atmosphere, add polyester diol dropwise, and stir for 1-3 h; add 0.5-1 mol of hydroxyl-containing acrylic monomer, then add stabilizer, and stir for 1 h; (3) Maintaining the nitrogen atmosphere, continue to add 1-10 mol of diluted monomer, cool to 45-50°C, add 2-2.5 mol of diisocyanate, add polyester triol and phenyl grafted polybutadiene polyol dropwise, and vacuum stir to degas, thereby obtaining a UV-moisture dual-curing polyurethane acrylate oligomer.
[0009] By adopting the above technical scheme, diisocyanate is selected as the starting reactant, and a photocurable carbon-carbon double bond is introduced through two different active NCO groups in the diisocyanate molecule; and then linear polyester diols and polyester triols are added in batches, so that the prepared polyurethane acrylate oligomer resin has good flexibility and adhesion, and also makes the linear structure of the resin have no extra sites that react with sulfur-containing groups, and can increase the overall adhesion performance of the material, accelerate the overall light curing and moisture curing effect of the three-proof adhesive, and on this basis, phenyl is added The branched polybutadiene polyol works together. The phenyl-grafted polybutadiene polyol has double bonds on the main chain segment, which increases the number of double bonds in the system, further promotes cross-linking and curing to form a network structure with rich branched cross-linking, improves the overall light curing and moisture curing effect and sulfur resistance of the three-proof adhesive, and the phenyl steric hindrance group on the side chain of the phenyl-grafted polybutadiene polyol has a shielding effect, improves sulfur resistance and solvent resistance, and also reduces the molecular chain movement ability of various polymers. The system structure is dense and stable, further increases the density of the material, prevents sulfur-containing substances from penetrating and causing sulfidation corrosion, and improves chemical resistance. It can also provide higher weather resistance, thereby making the three-proof adhesive material have high peel strength and excellent low-temperature resistance. Compared with the use of a single polyol, the present application achieves better sulfur resistance, adhesion, acid and alkali resistance by co-participating in the preparation of oligomers with polyester diols, polyester triols and phenyl grafted polybutadiene polyols. This may be because the linear structure of polyester diols and polyester triols does not introduce extra sites for reaction with sulfur-containing groups and the hydroxyl groups with different functionalities increase the richness of cross-linking, which is conducive to the construction of a denser cross-linking network, and the phenyl grafted polybutadiene polyol The double bonds in the main chain can participate in polymerization, further improving the density and adhesion of the film. The side chain phenyl groups form a more effective dispersion in the cross-linked network during the polymerization of the main chain, thereby enhancing the shielding effect of the benzene ring and further improving the sulfur resistance. The structure of polyester diols and polyester triols provides more dispersion space for the benzene ring side chains, avoiding the poor toughness of the formed film and easy cracking, thereby further ensuring the sulfur resistance of the film and preparing a triple-proof adhesive system with excellent adhesion, weather resistance and high vulcanization resistance, as well as other excellent properties such as acid and alkali resistance and salt spray resistance.
[0010] In a specific embodiment, the stirring and degassing is performed at a stirring speed of 100-150 r / min and a degassing time of 3-5 min.
[0011] In a specific embodiment, the mass ratio of the polyester diol, polyester triol and phenyl-grafted polybutadiene polyol is (3-7):(2-5):1.
[0012] By adopting the above technical scheme, by setting the proportion of different polyols within a certain range, on the one hand, the straight-chain polyester polyol can control the adhesion and flexibility of the cross-linked structure of the material and increase the photocuring effect of the material; on the other hand, phenyl-grafted polybutadiene polyol is used to further introduce phenyl into the system, and the side chain phenyl can enhance the density of the material, thereby reducing the penetration of sulfur-containing substances, enhancing the sulfur resistance and also improving the weather resistance of the material; on the other hand, phenyl-grafted polybutadiene polyol can be used to design and prepare multifunctional dual-curing polyurethane acrylate oligomer resins with a large number of double bonds, which is helpful to improve the photocuring activity of the resin, thereby realizing rapid curing of the manufactured product. Too much polyester polyol content will not only affect the density of the material, but also affect the material's sulfur resistance and salt spray corrosion resistance, and thus the hydrolysis resistance, aging resistance, high temperature resistance and yellowing resistance of the three-proof adhesive product will be affected. Too much phenyl grafted polybutadiene polyol will make the material hardness too high and the adhesion insufficient, affecting the flexibility of the adhesive layer, easily causing the adhesive layer to crack, the protective performance is lower, and the vulcanization resistance is insufficient. By adjusting the content within the above range, the long-lasting sulfur resistance effect of the three-proof adhesive is optimized.
[0013] In a specific embodiment, the acrylic active monomer is selected from: one or more of isobornyl acrylate, isooctyl methacrylate, dipropylene glycol diacrylate, tetrahydrofuran acrylate, tetrahydrofuran methacrylate, trimethylolpropane triacrylate, 2-phenoxyethyl acrylate, and ethoxylated trimethylolpropane triacrylate.
[0014] By adopting the above technical solution, polyurethane acrylate oligomers and acrylic active monomers participate in moisture curing together, providing the adhesive with later bonding strength and toughness, and improving the elongation at break; thereby making the adhesive layer denser, and having stronger protection performance in harsh atmosphere environments such as salt spray and high humidity, and having high vulcanization resistance.
[0015] In a specific embodiment, the acrylic reactive monomers are isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate.
[0016] By adopting the above technical scheme, the above acrylic active monomers can be mixed and used to achieve excellent gas barrier and other protective properties, so that the three-proof adhesive can protect the surface of the coated electronic products from being converted into elemental sulfur and hydrogen sulfide under heat or other catalytic effects, thereby causing sulfide corrosion to the electronic components in the relevant environment. Isobornyl acrylate has a highly active propylene group, and the high activity can improve the construction performance, improve the leveling of the coating, and reduce the color difference of the finished three-proof adhesive; combined with trimethylolpropane triacrylate with rich side chains and high hardness, it can significantly reduce the internal stress of the three-proof adhesive material and reduce the volume shrinkage of the three-proof adhesive material. Tetrahydrofuran acrylate can improve the compatibility with the main resin, surface drying speed and bonding strength; thereby significantly improving the adhesion and shrinkage of the photocuring layer, and having considerable impact resistance, abrasion resistance and weather resistance, while not reducing its hardness and flexibility. The phenoxy group in 2-phenoxyethyl acrylate can adjust the viscosity of the system and accelerate the photocuring speed of the system. Therefore, acrylic active monomers and polyurethane acrylate oligomer resins can form a denser cross-linking network. The above materials and their proportions can be used to prepare a three-proof adhesive that has both high vulcanization resistance and other excellent properties such as acid and alkali resistance and salt spray resistance, and has excellent vulcanization resistance.
[0017] In a specific embodiment, the mass ratio of isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is (10-18):(12-21):(8-14):5.
[0018] By adopting the above technical scheme, the above disclosed acrylic active monomer mixing ratio makes the crosslinking effect of the polyurethane acrylate oligomer resin and acrylic active monomer system better. If the content of acrylate isobornyl is too low, the hardness of the three-proof glue material will be high, which is not suitable for flexible use; if the content of trimethylolpropane triacrylate is too low, the impact resistance will be insufficient, and if the content of methacrylate tetrahydrofuran is too low, it will affect the adhesion of the three-proof glue material. If the content of 2-phenoxyethyl acrylate is too low, it will affect the density of the material. If it is too much, it will affect the hardness of the material and the construction performance will be poor. Therefore, the above monomers are mixed and used within a certain mass ratio range, so that the chemical properties of the three-proof glue material after crosslinking and polymerization can be stable, and the pores between the structural network are dense and stable, thereby reducing the penetration capacity of elemental sulfur and negative divalent sulfur, and the penetration barrier is reduced, that is, the vulcanization resistance is enhanced.
[0019] In a specific embodiment, the leveling agent is selected from one or more of BYK-333, BYK-30, BYK-323, and the defoaming agent is one or more of BYK-051, BYK-530, BYK-052N; the photoinitiator is selected from one or more of benzil ketals, hydroxy ketones, amino ketones, and acylphosphine peroxides; the inhibitor is selected from one or more of p-hydroxyanisole, p-benzoquinone, and hydroquinone.
[0020] In a second aspect, the present application provides a method for preparing a sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, using the following technical solution: A method for preparing a sulfur-resistant triple-proof adhesive capable of dual curing by ultraviolet light and moisture comprises the following steps: (a) Add dual-curing polyurethane acrylate oligomer and acrylic reactive monomer into a mixer in proportion, control the temperature at 30-40°C, stir evenly under vacuum, and release the pressure with nitrogen; (b) Add the photoinitiator, leveling agent, defoaming agent and polymerization inhibitor into a mixer, protect from light, stir evenly under vacuum, and release the pressure with nitrogen to obtain a sulfur-resistant three-proof adhesive.
[0021] In a specific embodiment, the vacuum stirring conditions are: temperature 30-40° C., vacuum of -0.08--0.1 MPa, and stirring at a speed of 500-1000 r / min for 1-2 h.
[0022] In summary, this application has the following beneficial effects: 1. By synthesizing UV- and moisture-curable polyurethane acrylate oligomers, diisocyanate is selected as the starting reactant, and a photocurable carbon-carbon double bond is introduced through two different active NCO groups in the diisocyanate molecule; then linear polyester diols and polyester triols are added in batches, so that the prepared polyurethane acrylate oligomer resin has good flexibility and adhesion, and also makes the linear structure of the resin have no extra sites that react with sulfur-containing groups, and can increase the overall adhesion performance of the material, accelerate the overall photocuring and Moisture curing effect, on this basis, phenyl grafted polybutadiene polyol is added to work together. Phenyl grafted polybutadiene polyol has double bonds on the main chain segment, which increases the number of double bonds in the system and further promotes cross-linking and curing; improves the overall light curing and moisture curing effect of the three-proof adhesive, and the phenyl steric hindrance group on the side chain of phenyl grafted polybutadiene polyol reduces the molecular chain movement ability of various polymers. The system structure is dense and stable, providing higher hardness and weather resistance, further increasing the density of the material, preventing sulfur-containing substances from penetrating and causing sulfide corrosion, and improving chemical resistance. By mixing and using a variety of polyols and regulating their content, the prepared adhesive has excellent adhesion, weather resistance and high sulfide resistance, and also has other excellent properties such as acid and alkali resistance and salt spray resistance.
[0023] 2. Isobornyl acrylate has a highly active propylene group, which can improve the construction performance, improve the leveling of the coating, and reduce the color difference of the finished three-proof adhesive; combined with trimethylolpropane triacrylate with rich side chains and high hardness, it can significantly reduce the internal stress of the three-proof adhesive material and reduce the volume shrinkage of the three-proof adhesive material. Tetrahydrofuran methacrylate can improve the compatibility with the main resin, surface drying speed and bonding strength; thereby significantly improving the adhesion and shrinkage of the photocurable layer, and having considerable impact resistance, scratch resistance and weather resistance, while not reducing its hardness and flexibility. A denser cross-linked network is formed through 2-phenoxyethyl acrylate. By mixing and using the above-mentioned acrylic active monomers and adjusting their ratios, it can play an excellent gas barrier and other protective properties, so that the three-proof adhesive can protect the surface of the coated electronic products from being converted into elemental sulfur and hydrogen sulfide under heat or other catalytic effects, thereby causing sulfidation corrosion to electronic components in related environments. DETAILED DESCRIPTION
[0024] The present application is further described in detail below with reference to the embodiments.
[0025] Some raw materials used in the preparation examples and embodiments: polyester diol molecular weight 3500 g / mol, model: 7210; polyester triol brand: HKP-24112; hydroxyl-terminated polybutadiene HTPB molecular weight 1000 g / mol, purchased from McCarthy; diisocyanate model: TDI-80; hydroxyl-containing acrylate monomer is ditrimethylolpropane acrylate, model: DI-TMPTA; stabilizer is benzoyl chloride purchased from Shandong Xinyingshun New Materials Co., Ltd.; diluent monomer is isobornyl acrylate model: R7104; polyurethane acrylate oligomer model: EBECRYL 1290; hydroquinone purchased from Shandong Hui'an Chemical Co., Ltd.; p-Hydroxyanisole model: bc65412; catalyst is dimethyltin dioctanoate model: Fomrez UL-28.
[0026] The raw materials used in the examples and comparative examples that are not otherwise specified are all conventional products that can be purchased from the market.
[0027] Preparation Example Preparation of Phenyl Grafted Polybutadiene Polyol Preparation Example 1 Under the protection of nitrogen atmosphere, 0.8 kg of hydroxyl-terminated polybutadiene and 0.5 kg of styrene were mixed evenly, added into a three-necked flask fixed in a constant temperature oil bath at 70 ° C, and 25 g of azobisisobutyronitrile and 1,4-dibutanol mixed solution were added dropwise, the mass ratio of azobisisobutyronitrile and 1,4-dibutanol was 1:2, stirred in the reactor for 2 hours, vacuumed for 0.5 hours, and cooled at room temperature to obtain phenyl-grafted polybutadiene polyol.
[0028] Preparation Example of Dual-Cure Polyurethane Acrylate Oligomer Preparation Example 2 Take 5 mol of polyol, which is polyester diol, polyester triol, and phenyl grafted polybutadiene polyol prepared in Preparation Example 1, wherein the mass ratio of polyester diol, polyester triol, and phenyl grafted polybutadiene polyol prepared in Preparation Example 1 is 3:5:1; vacuum dewatering at 120°C for 4 hours for standby; take 2 mol of diisocyanate and 0.01 mol of catalyst, heat to 75°C under nitrogen atmosphere, dropwise add polyester diol in proportion, and stir for 2 hours; then dropwise add 0.5 mol of hydroxyl-containing acrylate monomer, and then add stabilizer, and stir for 1 hour; then, keep nitrogen atmosphere, add 1 mol of diluent monomer, cool to 50°C, add 2 mol of diisocyanate, dropwise add polyester triol and phenyl grafted polybutadiene polyol prepared in Preparation Example 1, vacuum stirring speed is 150 r / min, and degassing time is 3 minutes, so as to obtain a UV-moisture dual-curing polyurethane acrylate oligomer resin.
[0029] Preparation Example 3 Take 5 mol of polyol, which is polyester diol, polyester triol, and phenyl grafted polybutadiene polyol prepared in Preparation Example 1, wherein the mass ratio of polyester diol, polyester triol, and phenyl grafted polybutadiene polyol prepared in Preparation Example 1 is 3:5:1; vacuum dewatering at 120°C for 4 hours for standby use; take 2 mol of diisocyanate and 0.05 mol of catalyst, heat to 75°C under nitrogen atmosphere, dropwise add polyester diol in proportion, and stir for 2 hours; then dropwise add 1 mol of hydroxyl-containing acrylate monomer, and then add stabilizer, and stir for reaction for 1 hour; then, keep nitrogen atmosphere, add 10 mol of diluent monomer, cool to 50°C, add 2.5 mol of diisocyanate, dropwise add polyester triol and phenyl grafted polybutadiene polyol prepared in Preparation Example 1, stir at a speed of 100 r / min, and degas for 5 minutes, so as to obtain a UV-moisture dual-curing polyurethane acrylate oligomer resin.
[0030] Preparation Example 4 Take 5 mol of polyol, which is polyester diol, polyester triol, and phenyl grafted polybutadiene polyol prepared in Preparation Example 1, wherein the mass ratio of polyester diol, polyester triol, and phenyl grafted polybutadiene polyol prepared in Preparation Example 1 is 7:2:1; vacuum dewatering at 120°C for 4 hours for standby; take 2 mol of diisocyanate and 0.1 mol of catalyst, heat to 75°C under nitrogen atmosphere, dropwise add polyester diol in proportion, and stir for 2 hours; then dropwise add 0.5 mol of hydroxyl-containing acrylate monomer, and then add stabilizer, and stir for 1 hour; then, keep nitrogen atmosphere, add 5 mol of diluent monomer, cool to 50°C, add 2 mol of diisocyanate, dropwise add polyester triol and phenyl grafted polybutadiene polyol prepared in Preparation Example 1, vacuum stirring speed is 150 r / min, and degassing time is 3 minutes, so as to obtain a UV-moisture dual-curing polyurethane acrylate oligomer resin.
[0031] Preparation Example 5 Take 5 mol of polyol, which is polyester diol, polyester triol, and phenyl grafted polybutadiene polyol prepared in Preparation Example 1, wherein the mass ratio of polyester diol, polyester triol, and phenyl grafted polybutadiene polyol prepared in Preparation Example 1 is 2:5:4; dewater under vacuum at 120°C for 4 hours and set aside; take 2 mol of diisocyanate and 0.1 mol of catalyst, heat to 75°C under nitrogen atmosphere, dropwise add polyester diol in proportion, and stir for 2 hours; then dropwise add 0.5 mol of hydroxyl-containing acrylate monomer, and then add stabilizer, stir and react for 1 hour; then, keep nitrogen atmosphere, add 5 mol of diluent monomer, cool to 50°C, add 2 mol of diisocyanate, dropwise add polyester triol and phenyl grafted polybutadiene polyol prepared in Preparation Example 1, vacuum stir at a speed of 150 r / min, and degas for 3 minutes, so as to obtain a UV-moisture dual-curing polyurethane acrylate oligomer resin.
[0032] Preparation Example 6 Take 5 mol of polyol, which is polyester diol, and remove water in vacuum at 120°C for 4 hours for use; take 2 mol of diisocyanate and 0.1 mol of catalyst, heat to 75°C under nitrogen atmosphere, add polyester diol drop by drop in proportion, and stir for 2 hours; then add 0.5 mol of hydroxyl-containing acrylate monomer drop by drop, and then add stabilizer, stir and react for 1 hour; then, keep the nitrogen atmosphere, add 5 mol of diluted monomer, cool to 50°C, add 2 mol of diisocyanate, stir in vacuum at a speed of 150 r / min, and degas for 3 minutes to obtain a UV-moisture dual-curing polyurethane acrylate oligomer resin.
[0033] Preparation Example 7 Take 5 mol of polyol, which is polyester triol, and dehydrate it in vacuum at 120°C for 4 hours for use; take 2 mol of diisocyanate and 0.1 mol of catalyst, heat them to 75°C under nitrogen atmosphere, add polyester triol drop by drop in proportion, and stir for 2 hours; then add 0.5 mol of hydroxyl-containing acrylate monomer drop by drop, and then add stabilizer, stir and react for 1 hour; then, keep the nitrogen atmosphere, add 5 mol of diluted monomer, cool to 50°C, add 2 mol of diisocyanate, stir in vacuum at a speed of 150 r / min, and degas for 3 minutes to obtain a UV-moisture dual-curing polyurethane acrylate oligomer resin.
[0034] Preparation Example 8 Take 5 mol of polyol, the polyol is the phenyl grafted polybutadiene polyol prepared in Preparation Example 1, dehydrate under vacuum at 120° C. for 4 hours and set aside; take 2 mol of diisocyanate and 0.1 mol of catalyst, heat to 75° C. under nitrogen atmosphere, add dropwise the phenyl grafted polybutadiene polyol prepared in Preparation Example 1 in proportion, and stir for 2 hours; then add dropwise 0.5 mol of hydroxyl-containing acrylate monomer, and then add stabilizer, and stir to react for 1 hour; then, keep the nitrogen atmosphere, add 5 mol of diluted monomer, cool to 50° C., add 2 mol of diisocyanate, stir in vacuum at a speed of 150 r / min, and degas for 3 minutes to obtain a UV-moisture dual-curing polyurethane acrylate oligomer resin.
[0035] Preparation Example 9 Take 5 mol of polyol, which is polyester diol and polyester triol, wherein the mass ratio of polyester diol to polyester triol is 4:5; remove water under vacuum at 120°C for 4 hours and set aside; take 2 mol of diisocyanate and 0.1 mol of catalyst, heat to 75°C under nitrogen atmosphere, dropwise add polyester diol in proportion, and stir for 2 hours; then dropwise add 0.5 mol of hydroxyl-containing acrylate monomer, and then add stabilizer, and stir to react for 1 hour; then, keep nitrogen atmosphere, add 5 mol of diluted monomer, cool to 50°C, add 2 mol of diisocyanate, add polyester triol dropwise in proportion, stir at a vacuum speed of 150 r / min, and degas for 3 minutes, so as to obtain a UV-moisture dual-curing polyurethane acrylate oligomer resin.
[0036] Preparation Example 10 Take 5 mol of polyol, which is polyester diol and phenyl grafted polybutadiene polyol prepared in Preparation Example 1, wherein the mass ratio of polyester diol to phenyl grafted polybutadiene polyol prepared in Preparation Example 1 is 8:1; dewater under vacuum at 120°C for 4 hours and set aside; take 2 mol of diisocyanate and 0.1 mol of catalyst, heat to 75°C under nitrogen atmosphere, dropwise add polyester diol in proportion, and stir for 2 hours; then dropwise add 0.5 mol of hydroxyl-containing acrylate monomer, and then add stabilizer, stir and react for 1 hour; then, keep nitrogen atmosphere, add 5 mol of diluent monomer, cool to 50°C, add 2 mol of diisocyanate, add phenyl grafted polybutadiene polyol prepared in Preparation Example 1 dropwise, vacuum stir at a speed of 150 r / min, and degas for 3 minutes, so as to obtain a UV-moisture dual-curing polyurethane acrylate oligomer resin.
[0037] Preparation Example 11 Take 5 mol of polyol, which is polyester triol and phenyl grafted polybutadiene polyol prepared in Preparation Example 1, wherein the mass ratio of polyester triol to phenyl grafted polybutadiene polyol prepared in Preparation Example 1 is 8:1; remove water in vacuum at 120°C for 4 hours and set aside; take 2 mol of diisocyanate and 0.1 mol of catalyst, heat to 75°C under nitrogen atmosphere, dropwise add polyester triol in proportion, and stir for 2 hours; then dropwise add 0.5 mol of hydroxyl-containing acrylate monomer, and then add stabilizer, stir and react for 1 hour; then, keep nitrogen atmosphere, add 5 mol of diluent monomer, cool to 50°C, add 2 mol of diisocyanate, add phenyl grafted polybutadiene polyol prepared in Preparation Example 1 dropwise, vacuum stir at a speed of 150 r / min, and degas for 3 minutes, so as to obtain a UV-moisture dual-curing polyurethane acrylate oligomer resin.
[0038] Example Example 1
[0039] A sulfur-resistant three-proof adhesive capable of dual curing by ultraviolet light and moisture, comprising the following components in parts by weight: 300 g of the dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 500 g of an acrylic acid active monomer, 10 g of a leveling agent, 1 g of a defoaming agent, 30 g of a photoinitiator, and 0.5 g of an inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; The mass ratio of isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 18:12:8:5; the leveling agent is BYK-323; the defoaming agent is BYK-530; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is p-hydroxyanisole.
[0040] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000 r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0041] Example 2 A sulfur-resistant three-proof adhesive capable of dual curing with ultraviolet light and moisture, comprising the following components in parts by weight: 550 g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450 g of acrylic acid active monomer, 2 g of leveling agent, 1 g of defoaming agent, 42 g of photoinitiator, and 5 g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; acrylic acid The mass ratio of isobornyl ester, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:14:14:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0042] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0043] Example 3 A sulfur-resistant three-proof adhesive capable of dual curing with ultraviolet light and moisture, comprising the following components in parts by weight: 550 g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450 g of acrylic acid active monomer, 2 g of leveling agent, 1 g of defoaming agent, 42 g of photoinitiator, and 5 g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; acrylic acid The mass ratio of isobornyl ester, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0044] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0045] Example 4 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by weight: 550 g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450 g of acrylic acid active monomer, 2 g of leveling agent, 1 g of defoaming agent, 42 g of photoinitiator, and 5 g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiators are photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0046] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0047] Example 5 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by weight: 550 g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450 g of acrylic active monomer, 2 g of leveling agent, 1 g of defoaming agent, 42 g of photoinitiator, and 5 g of polymerization inhibitor, wherein the acrylic active monomer is trimethylolpropane triacrylate; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0048] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0049] Example 6 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by weight: 550 g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450 g of acrylic acid active monomer, 2 g of leveling agent, 1 g of defoaming agent, 42 g of photoinitiator, and 5 g of polymerization inhibitor, wherein the acrylic acid active monomer is 2-phenoxyethyl acrylate; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiators are photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0050] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0051] Example 7 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by mass: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate and trimethylolpropane triacrylate; the mass ratio of isobornyl acrylate and trimethylolpropane triacrylate is 15:25; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0052] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0053] Example 8 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by mass: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate and tetrahydrofuran methacrylate; the mass ratio of isobornyl acrylate and tetrahydrofuran methacrylate is 15:25; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0054] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0055] Example 9 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by mass: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate and 2-phenoxyethyl acrylate; the mass ratio of isobornyl acrylate to 2-phenoxyethyl acrylate is 15:25; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0056] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0057] Example 10 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by mass: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is trimethylolpropane triacrylate and 2-phenoxyethyl acrylate; the mass ratio of trimethylolpropane triacrylate to 2-phenoxyethyl acrylate is 12:28; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0058] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0059] Embodiment 11 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by mass: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, and tetrahydrofuran methacrylate; the mass ratio of isobornyl acrylate, trimethylolpropane triacrylate, and tetrahydrofuran methacrylate is 15:17:8; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO, and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO, and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0060] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0061] Example 12 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by mass: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450g of acrylic acid active monomers, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomers are isobornyl acrylate, trimethylolpropane triacrylate and 2-phenoxyethyl acrylate; the mass ratio of isobornyl acrylate, trimethylolpropane triacrylate and 2-phenoxyethyl acrylate is 15:20:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0062] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0063] Embodiment 13 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by mass: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate; the mass ratio of isobornyl acrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 27:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0064] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0065] Embodiment 14 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by mass: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate; the mass ratio of trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 27:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the polymerization inhibitor is hydroquinone.
[0066] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0067] Embodiment 15 A sulfur-resistant three-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by weight: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 3, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; acrylic acid The mass ratio of isobornyl ester, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0068] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0069] Example 16 A sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by weight: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 4, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; acrylic acid The mass ratio of isobornyl ester, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0070] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0071] Embodiment 17 A sulfur-resistant three-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by weight: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 5, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; acrylic acid The mass ratio of isobornyl ester, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0072] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0073] Embodiment 18 A sulfur-resistant three-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by weight: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 6, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; acrylic acid The mass ratio of isobornyl ester, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0074] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0075] Embodiment 19 A sulfur-resistant three-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by weight: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 7, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; acrylic acid The mass ratio of isobornyl ester, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0076] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0077] Embodiment 20 A sulfur-resistant three-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by weight: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 8, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; acrylic acid The mass ratio of isobornyl ester, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0078] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0079] Embodiment 21 A sulfur-resistant three-proof adhesive that can be dual-cured by ultraviolet light and moisture, comprising the following components in parts by weight: 550g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 9, 450g of acrylic acid active monomer, 2g of leveling agent, 1g of defoaming agent, 42g of photoinitiator, and 5g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; acrylic acid The mass ratio of isobornyl ester, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0080] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0081] Embodiment 22 A sulfur-resistant three-proof adhesive capable of dual curing with ultraviolet light and moisture, comprising the following components in parts by weight: 550 g of the dual-cured polyurethane acrylate oligomer prepared in Preparation Example 10, 450 g of an acrylic acid active monomer, 2 g of a leveling agent, 1 g of a defoaming agent, 42 g of a photoinitiator, and 5 g of an inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; The mass ratio of isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0082] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0083] Embodiment 23 A sulfur-resistant three-proof adhesive capable of dual curing with ultraviolet light and moisture, comprising the following components in parts by weight: 550 g of dual-cured polyurethane acrylate oligomer prepared in Preparation Example 11, 450 g of acrylic acid active monomer, 2 g of leveling agent, 1 g of defoaming agent, 42 g of photoinitiator, and 5 g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; The mass ratio of isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0084] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0085] Comparative Example Comparative Example 1 A sulfur-resistant triple-proof adhesive capable of dual curing with ultraviolet light and moisture, comprising the following components in parts by weight: 550 g of polyurethane acrylate oligomer, 450 g of acrylic acid active monomer, 2 g of leveling agent, 1 g of defoaming agent, 42 g of photoinitiator, and 5 g of polymerization inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; The mass ratio of ester, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, and the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1; the inhibitor is hydroquinone, and the model of the polyurethane acrylate oligomer is EBECRYL 1290.
[0086] Add polyurethane acrylate oligomer and acrylic acid active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0087] Comparative Example 2 A sulfur-resistant three-proof adhesive capable of dual curing by ultraviolet light and moisture, comprising the following components in parts by weight: 550 g of the dual-cured polyurethane acrylate oligomer prepared in Preparation Example 2, 100 g of an acrylic acid active monomer, 2 g of a leveling agent, 1 g of a defoaming agent, 42 g of a photoinitiator, and 5 g of an inhibitor, wherein the acrylic acid active monomer is isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate, and 2-phenoxyethyl acrylate; acrylic acid; The mass ratio of isobornyl ester, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is 15:12:8:5; the leveling agent is BYK-333; the defoaming agent is BYK-051; the photoinitiator is photoinitiator 184, photoinitiator TPO and photoinitiator LTM, the mass ratio of photoinitiator 184, photoinitiator TPO and photoinitiator LTM is 2.7:0.5:1, and the inhibitor is hydroquinone.
[0088] Add dual-curing polyurethane acrylate oligomer and acrylic active monomer into the mixer in proportion, control the temperature at 30°C, stir evenly under vacuum, and release the pressure with nitrogen; add photoinitiator, leveling agent, defoamer, and inhibitor into the mixer in proportion, protect from light, stir for 1 hour at 40°C, vacuum degree of -0.08MPa, and speed of 1000r / min, and release the pressure with nitrogen to obtain sulfur-resistant UV-curing triple-proof adhesive.
[0089] Performance Testing The sulfur-resistant triple-proof adhesive prepared in the embodiment and comparative example can be cured by ultraviolet light and moisture. The ultraviolet light curing conditions are as follows: a high-pressure mercury lamp with a main wavelength of 365 nm is used for ultraviolet light curing, and the radiation intensity is 40-50 mW / cm 2 , curing time 20 seconds; Moisture curing conditions: Place it in a room with constant temperature and humidity (23±2℃, 50±10%RH) in absolute darkness and observe the curing state of the glue every 24 hours. a. Adhesion test: According to GB / T9286, the UV curing energy is 1500mJ / cm 2 , and then place it in moisture curing for 5 days. The adhesion of the three-proof adhesive must reach 5B, which is qualified; b. Sulfur resistance: After the (2835) LED chip is cured, the three-proof adhesive is placed in a 250ML flask, 3g of sulfur powder is added, and the flask is sealed and placed at 90℃ for 2 days. Then the light decay is tested. The luminous flux under different conditions is tested using an integrating sphere, and then the attenuation value is calculated; c. Hardness test: in accordance with GB / T531.1-2008; see Table 1 for the comparison results: Table 1 Performance test results
[0090] As can be seen from Table 1, the sulfur-resistant triple-proof adhesive that can be dual-cured by UV light and moisture obtained in the above embodiment has high hardness while meeting the coating requirements in terms of various properties such as curing speed, adhesion, sulfur resistance, color difference, and hardness. The surface of the adhesive after curing is very smooth and has excellent anti-friction performance, which can play a good protective role.
[0091] By comparing Example 3 with Examples 15-23 and Comparative Example 1, it can be seen that the sulfur-resistant triple-proof adhesive that can be dual-cured by ultraviolet light and moisture prepared in Example 3 is superior to Comparative Example 1 and Examples 18-23 in terms of curing speed, adhesion, sulfur resistance, and hardness performance indicators. It is analyzed that compared with the use of a single polyol, the present application achieves better sulfur resistance, adhesion, and acid and alkali resistance by co-participating in the preparation of oligomers by polyester diols, polyester triols, and phenyl-grafted polybutadiene polyols. This may be because the linear structure of polyester diols and polyester triols does not introduce redundant sites that react with sulfur-containing groups, and hydroxyl groups of different functionalities increase the richness of crosslinking, which is conducive to a denser crosslinking network. The double bonds of the main chain of the phenyl-grafted polybutadiene polyol can participate in the polymerization, further improving the density and adhesion of the film. The side chain phenyl groups form a more effective dispersion in the cross-linked network during the polymerization of the main chain, thereby improving the shielding effect of the benzene ring and further improving the sulfur resistance. The structures of polyester diols and polyester triols provide more dispersion space for the benzene ring side chains, avoiding the poor toughness of the formed film and easy cracking, thereby further ensuring the sulfur resistance of the film. Therefore, the prepared polyurethane acrylate oligomer resin ensures the adhesion, weather resistance and high vulcanization resistance of the material, and also has other excellent properties of a three-proof adhesive system such as acid and alkali resistance and salt spray resistance.
[0092] By comparing Example 3 with Examples 4-14 and Comparative Example 2, it can be seen that the sulfur-resistant three-proof adhesive that can be cured by ultraviolet light and moisture prepared in Example 3 is superior to Comparative Example 2 and Examples 4-14 in terms of curing speed, adhesion, sulfur resistance, color difference, and hardness performance indicators. It is analyzed that the mixed use of acrylic acid active monomers can play an excellent gas barrier and other protective properties, and acrylate isobornyl ester improves the leveling of the coating. Combined with trimethylolpropane triacrylate with rich side chains and high hardness, it can significantly reduce the internal stress of the three-proof adhesive material and has considerable impact resistance. In combination with methacrylic acid Tetrahydrofuran can improve the compatibility with the main resin, surface drying speed and bonding strength; the phenoxy group in 2-phenoxyethyl acrylate can adjust the system viscosity and accelerate the system light curing speed, so as to prepare a polyolefin elastomer system three-proof adhesive with high vulcanization resistance and other excellent properties such as acid, alkali resistance and salt spray resistance. The density of the adhesive film is improved by mixing the four monomers, and it has excellent vulcanization resistance. The mixing ratio of acrylic active monomers can make the chemical properties of the three-proof adhesive material after cross-linking polymerization stable, and the pores between the structural network are dense and stable, thereby reducing the elemental sulfur and S 2- The permeability is reduced and the permeation barrier is reduced, that is, the sulfide resistance is enhanced.
[0093] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A sulfur-resistant and anti-corrosive adhesive that can be cured by UV light and moisture. Features: The invention comprises the following components in parts by weight: 30-60 parts of dual-cured polyurethane acrylate oligomer, 20-50 parts of acrylic active monomer, 0.1-5 parts of leveling agent, 0.1-5 parts of defoaming agent, 3-8 parts of photoinitiator and 0.05-0.5 parts of polymerization inhibitor.
2. The sulfur-resistant triple-proof adhesive capable of dual curing by ultraviolet light and moisture according to claim 1, Features: The dual-cured polyurethane acrylate oligomer has the following specific synthesis steps: (1) taking polyester diol, polyester triol, and phenyl-grafted polybutadiene polyol, respectively, and removing water in a vacuum at 120° C. for 4 hours for later use; (2) Take 2 mol of diisocyanate and 0.01-0.1 mol of catalyst, heat to 65-75°C under nitrogen atmosphere, add polyester diol dropwise, and stir for 1-3 hours; add 0.5-1 mol of hydroxyl-containing acrylic monomer, then add stabilizer, and stir for 1 hour; (3) Maintaining the nitrogen atmosphere, continue to add 1-10 mol of dilution monomer, cool to 45-50°C, add 2-2.5 mol of diisocyanate, add polyester triol and phenyl grafted polybutadiene polyol dropwise, and vacuum stir to degas, thereby obtaining a dual-curing polyurethane acrylate oligomer.
3. The sulfur-resistant triple-proof adhesive capable of dual curing by ultraviolet light and moisture according to claim 2, Features: The mass ratio of the polyester diol, polyester triol and phenyl-grafted polybutadiene polyol is (3-7): (2-5):
1.
4. The sulfur-resistant triple-proof adhesive capable of dual curing by ultraviolet light and moisture according to claim 2, Features: In the step (3), the stirring and degassing is performed at a stirring speed of 100-150 r / min and a degassing time of 3-5 min.
5. The sulfur-resistant triple-proof adhesive capable of dual curing by ultraviolet light and moisture according to claim 1, Features: The acrylic active monomer is selected from one or more of isobornyl acrylate, isooctyl methacrylate, dipropylene glycol diacrylate, tetrahydrofuran acrylate, tetrahydrofuran methacrylate, trimethylolpropane triacrylate, 2-phenoxyethyl acrylate, and ethoxylated trimethylolpropane triacrylate.
6. The sulfur-resistant triple-proof adhesive capable of dual curing by ultraviolet light and moisture according to claim 5, Features: The acrylic active monomers are isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate.
7. The sulfur-resistant triple-proof adhesive capable of dual curing by ultraviolet light and moisture according to claim 6, Features: The mass ratio of isobornyl acrylate, trimethylolpropane triacrylate, tetrahydrofuran methacrylate and 2-phenoxyethyl acrylate is (10-18):(12-21):(8-14):
5.
8. The sulfur-resistant triple-proof adhesive capable of dual curing by ultraviolet light and moisture according to claim 1, Features: The leveling agent is selected from one or more of BYK-333, BYK-30, and BYK-323; the defoaming agent is selected from one or more of BYK-051, BYK-530, and BYK-052N; the photoinitiator is selected from one or more of benzil ketals, hydroxy ketones, amino ketones, and acylphosphine peroxides; the inhibitor is selected from one or more of p-hydroxyanisole, p-benzoquinone, and hydroquinone.
9. A method for preparing a sulfur-resistant and anti-corrosion adhesive capable of dual curing by ultraviolet light and moisture according to any one of claims 1 to 8, Features: The steps include: (a) Add dual-curing polyurethane acrylate oligomer and acrylic reactive monomer into a mixer in proportion, control the temperature at 30-40°C, stir evenly under vacuum, and release the pressure with nitrogen; (b) Add the photoinitiator, leveling agent, defoaming agent and polymerization inhibitor into a mixer, protect from light, stir evenly under vacuum, and release the pressure with nitrogen to obtain a sulfur-resistant three-proof adhesive.
10. A method for preparing a sulfur-resistant and anti-corrosive adhesive capable of dual curing by ultraviolet light and moisture according to claim 9, Features: The vacuum stirring conditions in (a) and (b) are as follows: a temperature of 30-40° C., a vacuum of minus 0.08-minus 0.1 MPa, and stirring at a speed of 500-1000 r / min for 1-2 h.
Citation Information
Patent Citations
UV-LED and moisture dual-curing three-proofing adhesive and preparation method thereof
CN111978914A
Ultraviolet curing adhesive with brine resistance, and preparation method thereof
CN113667446A
Modified polyurethane acrylate resin, adhesive and preparation method of modified polyurethane acrylate resin
CN116903825A
Polybutadiene polyurethane acrylate photosensitive resin and preparation method thereof
CN118459717A