Two-component bonding composition, adhesive, preparation method of two-component bonding composition and adhesive, and photovoltaic module

Through the adhesive of the two-component adhesive composition, modified coating materials and cross-linking reactions are used to solve the heat dissipation problem in the photovoltaic junction box, achieve high thermal conductivity, flame retardancy and heat storage and temperature control properties, and ensure the photovoltaic modules stable operation.

CN118772836APending Publication Date: 2024-10-15TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411030543.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The heat generated by the diodes in the photovoltaic junction box cannot be effectively dissipated, resulting in local high temperatures, which affects the work of the diodes and the safety of the junction box. Traditional silicone potting glue has low thermal conductivity and poor heat storage, temperature control, and anti-aging properties.

Method used

A two-component adhesive composition is provided, including component A and component B. Component A contains hydroxyl-terminated polysiloxane, modified aluminum hydroxide and modified coating material, and component B contains alkyl groups. Silicone oil, cross-linking agent and tin catalyst form an adhesive with high thermal conductivity, flame retardancy, heat storage and temperature control and excellent mechanical properties through phase change and cross-linking reaction.

Benefits of technology

It effectively prevents the temperature inside the photovoltaic junction box from being too high, improves the thermal conductivity, heat dissipation, heat storage performance and anti-aging performance of the adhesive, and ensures the stable operation of photovoltaic modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, in particular to a two-component adhesive composition, an adhesive, a preparation method of the adhesive and a photovoltaic module. The double-component bonding composition provided by the invention comprises a component A and a component B. The component A comprises the following components in parts by weight: 48-53 parts of hydroxyl-terminated polysiloxane, 6-12 parts of modified aluminum hydroxide and 41-46 parts of a modified coating material; the component B is prepared from the following components in parts by weight: 55 to 60 parts of alkyl silicone oil, 36 to 40 parts of a cross-linking agent, 4 to 6 parts of a coupling agent and 0.1 to 0.3 part of a tin catalyst. The adhesive prepared from the two-component adhesive composition provided by the invention has excellent heat conduction and heat dissipation functions, so that the problem that the temperature in the photovoltaic junction box is too high can be effectively prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of adhesives, and in particular to a two-component adhesive composition, an adhesive and a preparation method thereof, and a photovoltaic module. Background Art

[0002] In recent years, photovoltaic modules have been widely used due to their high current and high power. In photovoltaic modules, photovoltaic junction boxes are key components that connect the solar cell module array and the solar charging control device. They can transfer the power generated by the solar photovoltaic module to the external circuit, thereby realizing power transmission.

[0003] During the power transmission process, as the rated current increases, the heat generated by the diodes in the photovoltaic junction box during the current passing through the diodes in a unit time also gradually increases. If the large amount of heat generated by the diodes cannot be dissipated in time, it will affect the use effect of the photovoltaic modules, and in severe cases, it will even burn the photovoltaic junction box. At present, the packaging of photovoltaic junction boxes mainly uses silicone potting glue. Due to its low thermal conductivity, traditional silicone potting glue cannot effectively dissipate the heat generated by the diodes during operation. At this time, the photovoltaic junction box is prone to local high temperature, which will affect the normal operation of the diodes and even cause the failure of the diodes and the bulging of the photovoltaic junction box. At the same time, some potting glues have high thermal conductivity, but they cannot maintain excellent heat storage and temperature control capabilities, anti-aging capabilities, or poor colloidal mechanical properties. Summary of the invention

[0004] Based on this, the present application provides a two-component adhesive composition, an adhesive and a preparation method thereof, and a photovoltaic module. The adhesive prepared from the two-component adhesive composition provided in the present application has excellent thermal conductivity and heat dissipation functions; it also has excellent heat storage performance, anti-aging performance and mechanical properties, so it can effectively prevent the problem of overheating in the photovoltaic junction box.

[0005] In a first aspect of the present application, a two-component adhesive composition is provided, comprising component A and component B.

[0006] In parts by weight, the component A comprises: 48 to 53 parts of terminal hydroxyl polysiloxane, 6 to 12 parts of modified aluminum hydroxide, and 41 to 46 parts of modified coating material;

[0007] In parts by weight, the component B includes: 55 to 60 parts of alkyl silicone oil, 36 to 40 parts of a cross-linking agent, 4 to 6 parts of a coupling agent, and 0.1 to 0.3 parts of a tin catalyst;

[0008] Among them, the modified aluminum hydroxide is aluminum hydroxide modified by a silane coupling agent, the shell layer of the modified coated material includes a titanium-containing compound modified by a silane modifier and boron nitride modified by a silane modifier, the core of the modified coated material includes an alkane with a carbon number of 18 to 30, and the phase transition temperature of the alkane is 28°C to 70°C; the silane coupling agent and the silane modifier each independently contain one or more amino groups.

[0009] In one embodiment, the modified aluminum hydroxide comprises a silane coupling agent and aluminum hydroxide in a mass ratio of 1: (0.01-0.02).

[0010] In one embodiment, the core of the modified coated material includes normal alkanes with 18 to 30 carbon atoms; and / or,

[0011] The titanium-containing compound is titanium dioxide.

[0012] In one embodiment, the modified coating material has one or more of the following characteristics:

[0013] (1) The phase change temperature of the modified coated material is 28°C to 70°C;

[0014] (2) The phase change enthalpy of the modified coated material is 200 J / g~240 J / g;

[0015] (3) The average particle size of the modified coated material is 5 μm to 10 μm.

[0016] In one embodiment, the silane coupling agent and the silane modifier are each independently selected from one or more of formula (I), Formula (I), wherein n1 is selected from a positive integer between 1 and 10; R 11 , R 12 and R 13 Each is independently a C1~C6 alkyl group; R 14 It is amino.

[0017] In one embodiment, the cross-linking agent includes a tetrafunctional silane compound, a trifunctional silane compound, and a difunctional silane compound in a mass ratio of (2.9-3.3):(0.18-0.25):(0.3-0.35).

[0018] In one embodiment, the cross-linking agent has one or more of the following characteristics:

[0019] (1) The structure of the tetrafunctional silane compound is , where R 21 , R 22 , R 23 and R24 Each is independently a C1~C6 alkyl;

[0020] (2) The structure of the trifunctional silane compound is , where R 31 , R 32 , R 33 and R 34 Each is independently a C1~C6 alkyl;

[0021] (3) The structure of the difunctional silane compound is , where R 41 , R 42 , R 43 and R 44 Each is independently a C1~C6 alkyl.

[0022] In one embodiment, the coupling agent includes a first silane polymer and a second silane polymer in a mass ratio of (1-2):1;

[0023] Wherein, the structure of the first silane polymer is ; n2 is greater than 1, R 51 , R 52 and R 53 Each independently is a C1~C6 alkyl group, R 54 and R 55 Each independently is a C1~C6 alkylene group;

[0024] The structure of the second silane polymer is ; n3 is greater than 1, R 61 , R 62 and R 63 Each independently is a C1~C6 alkyl group, R 64 and R 55 It is a C1~C6 alkylene group.

[0025] In one embodiment, the tin catalyst includes one or more of dibutyltin bis(acetylacetonate), dimethyltin bis(acetylacetonate), diphenyltin bis(acetylacetonate), and diisopropyltin bis(acetylacetonate).

[0026] In one embodiment, the two-component adhesive composition has one or more of the following characteristics:

[0027] (1) The terminal hydroxyl polysiloxane includes one or more of terminal hydroxyl polydimethylsiloxane and terminal hydroxyl polydiethylsiloxane;

[0028] (2) The viscosity of the hydroxy-terminated polysiloxane at 25° C. is 3000 cps to 4000 cps;

[0029] (3) The alkyl silicone oil includes one or more of dimethyl silicone oil and diethyl silicone oil;

[0030] (4) The viscosity of the alkyl silicone oil at 25° C. is 1000 cps to 1500 cps.

[0031] In one embodiment, the mass ratio of the component A to the component B is (4.7-5.2):1.

[0032] The second aspect of the present application provides a method for preparing an adhesive, comprising the following steps:

[0033] Prepare component A by compounding component A in the bonding composition according to any one of the embodiments of the first aspect of the present application;

[0034] The B component is prepared by compounding the B component in the adhesive composition according to any one of the embodiments of the first aspect.

[0035] In one embodiment, the steps of preparing the modified coated material include:

[0036] The alkane, the surfactant and the first organic alkaline solvent are mixed, and heated at a temperature 8° C. to 15° C. higher than the phase transition temperature of the alkane to prepare an oil-in-water solution;

[0037] Adding a titanium source and boron nitride to the oil-in-water solution to prepare a precursor solution;

[0038] Adding a water source, a hydrolysis accelerator and a second organic alkaline solvent to the precursor solution to prepare a coated material;

[0039] The coated material and the silane modifier are mixed in a solvent, and after stirring and modification, the modified coated material is prepared;

[0040] Wherein, the titanium source comprises titanate.

[0041] In one embodiment, the preparation step of the modified coated material has one or more of the following characteristics:

[0042] (1) The mass volume ratio of the alkane, the surfactant and the first organic alkaline solvent is (4-6) g: (1-2) g: (80-120) mL;

[0043] (2) The surfactant includes one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium lauryl polyoxyethylene ether sulfate, sodium hexadecyl sulfate and sodium dodecyl polyoxyethylene ether sulfate;

[0044] (3) The hydrolysis promoter includes an organic acid;

[0045] (4) the first organic alkaline solvent and the second organic alkaline solvent are each independently an amide solvent;

[0046] (5) The mass ratio of the coating material to the silane modifier is 1:(0.01-0.02).

[0047] In one embodiment, the preparation steps of the modified aluminum hydroxide include:

[0048] Aluminum hydroxide, a silane coupling agent and a ball milling medium are ball milled and mixed, and then dried to prepare the modified aluminum hydroxide.

[0049] In one embodiment, the preparation step of the modified aluminum hydroxide has one or more of the following characteristics:

[0050] (1) The mass ratio of the aluminum hydroxide to the silane coupling agent is 1:(0.01-0.02);

[0051] (2) The ball milling medium includes an alcohol solvent and water in a volume ratio of (1-2):1.

[0052] The third aspect of the present application provides an adhesive, which includes the two-component adhesive composition described in any embodiment of the first aspect of the present application, or is prepared by the preparation method described in any embodiment of the second aspect of the present application.

[0053] A fourth aspect of the present application provides a photovoltaic module, characterized in that it includes the adhesive described in the third aspect of the present application or includes an encapsulation adhesive layer formed after the adhesive described in the third aspect of the present application is cured.

[0054] The two-component adhesive composition provided by the present application can make both component A and component B have good compatibility under the premise of reasonable matching of the types and weight proportions of each component. The alkane core in the modified coating material included in component A can realize heat absorption and heat release functions through phase change; when the temperature of the photovoltaic module is high, the titanium-containing compound and boron nitride shell included in the modified coating material have excellent thermal conductivity, which can quickly transfer heat to the core. At this time, the alkane core can absorb heat and undergo phase change, and its high enthalpy value can make the adhesive of the present application have excellent heat storage performance, thereby achieving the effect of reducing the temperature of the photovoltaic module; in addition, the modified aluminum hydroxide contained in component A has excellent flame retardant and filling properties, and its surface is modified by a silane coupling agent, and under the synergy of the silane modifier modified coating material, it can effectively improve the interface bonding between aluminum hydroxide and the terminal hydroxyl polysiloxane matrix and the coating material, and enhance the compatibility of various types of components.

[0055] The alkyl silicone oil, coupling agent, tin catalyst and crosslinking agent included in the B component can be crosslinked and cured with the terminal hydroxyl polysiloxane in the A component after being mixed with the A component to form a dense crosslinking structure to ensure that the adhesive has excellent mechanical properties and excellent aging stability after curing. In summary, the A component and the B component of the adhesive composition provided by the present application have excellent compatibility, and the adhesive prepared therefrom has excellent thermal conductivity and flame retardancy, heat storage and temperature control performance, anti-aging performance and excellent mechanical properties. DETAILED DESCRIPTION

[0056] The following is a further complete and clear description of the two-component adhesive composition, adhesive and preparation method thereof, and photovoltaic module of the present application in conjunction with specific examples. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0057] In this application, "alkane" refers to a compound in which all carbon-carbon bonds are connected by single bonds, and the remaining bonds are combined with hydrogen. Alkanes are divided into two categories: cycloalkanes and chain alkanes. The general formula of chain alkanes is C m H 2m+2 The general formula of cycloalkanes is C m H 2m . In the present application, an alkane having 18 to 30 carbon atoms means that the value of m is 18 to 30. In the present application, "alkyl" may represent a straight chain, branched chain and / or cyclic alkyl group. A phrase containing the term, for example, "C1 to C6 alkyl" refers to an alkyl group containing 1 to 6 carbon atoms, and each occurrence may be independently of each other a C1 alkyl group, a C2 alkyl group, a C3 alkyl group, a C4 alkyl group, a C5 alkyl group, or a C6 alkyl group. Non-limiting examples of alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, isobutyl, 2-ethylbutyl, 3,3-dimethylbutyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, cyclopentyl, 1-methylpentyl, 3-methylpentyl, 4-methyl-2-pentyl, n-hexyl or cyclohexyl.

[0058] "Alkylene" refers to a hydrocarbon group with two monovalent radical centers derived from an alkyl group by removing a hydrogen atom, which can be a saturated branched alkyl group or a saturated straight-chain alkyl group. For example, "C1-C6 alkylene" means that the alkyl part contains 1 to 6 carbon atoms, and each time it appears, it can be independently C1 alkylene, C4 alkylene, C5 alkylene, C6 alkylene. Suitable examples include, but are not limited to: methylene (-CH2-), 1,1-ethyl (-CH(CH3)-), 1,2-ethyl (-CH2CH2-), 1,1-propyl (-CH(CH2CH3)-), 1,2-propyl (-CH2CH(CH3)-), 1,3-propyl (-CH2CH2CH2-) and 1,4-butyl (-CH2CH2CH2CH2-).

[0059] In the present application, "amino" refers to a derivative of ammonia, having a structural feature of the formula -N(X)2, wherein each "X" is independently H, substituted or unsubstituted alkyl, substituted or unsubstituted cycloalkyl, substituted or unsubstituted heterocyclyl, etc. Non-limiting types of amino groups include -NH2, -N(alkyl)2, -NH(alkyl), -N(cycloalkyl)2 or -NH(cycloalkyl), etc.

[0060] In a first aspect of the present application, a two-component adhesive composition is provided, comprising component A and component B.

[0061] In parts by weight, the component A comprises: 48 to 53 parts of terminal hydroxyl polysiloxane, 6 to 12 parts of modified aluminum hydroxide, and 41 to 46 parts of modified coating material;

[0062] In parts by weight, the component B includes: 55 to 60 parts of alkyl silicone oil, 36 to 40 parts of a cross-linking agent, 4 to 6 parts of a coupling agent, and 0.1 to 0.3 parts of a tin catalyst;

[0063] Among them, the modified aluminum hydroxide is aluminum hydroxide modified by a silane coupling agent, the shell layer of the modified coated material includes a titanium-containing compound modified by a silane modifier and a boron nitride modified by a silane modifier, the core of the modified coated material includes an alkane with a carbon number of 18 to 30, and the phase transition temperature of the alkane is 28°C to 70°C; the silane coupling agent and the silane modifier each independently contain one or more amino groups.

[0064] The "phase transition temperature of alkanes" refers to the transition temperature between the solid and liquid states of alkanes. It is understandable that the phase transition temperature of the alkanes can be selected from any value between 28°C and 70°C. Specifically, the phase transition temperature of the alkanes includes but is not limited to 28°C, 30°C, 33°C, 35°C, 36°C, 37°C, 38°C, 40°C, 43°C, 45°C, 48°C, 50°C, 55°C, 60°C, 65°C or 70°C. In one example, the core of the modified coated material includes normal alkanes having a carbon number of 18 to 30. By way of example, the normal alkanes include but are not limited to n-octadecane, n-eicosane, n-docosane, n-tetracosane, n-hexacosane, n-octacosane, and n-triacontane.

[0065] The two-component adhesive composition provided by the present application can make both component A and component B have good compatibility under the premise of reasonable matching of the types and weight proportions of each component. The alkane core in the modified coating material included in component A can realize heat absorption and heat release functions through phase change; when the temperature of the photovoltaic module is high, the titanium-containing compound and boron nitride shell included in the modified coating material have excellent thermal conductivity, which can quickly transfer heat to the core. At this time, the alkane core can absorb heat and undergo phase change, and its high enthalpy value can make the adhesive of the present application have excellent heat storage performance, thereby achieving the effect of reducing the temperature of the photovoltaic module; in addition, the modified aluminum hydroxide contained in component A has excellent flame retardant and filling properties, and its surface is modified by a silane coupling agent, and under the synergy of the silane modifier modified coating material, it can effectively improve the interface bonding between aluminum hydroxide and the terminal hydroxyl polysiloxane matrix and the coating material, and enhance the compatibility of various types of components.

[0066] The alkyl silicone oil, coupling agent, tin catalyst and crosslinking agent included in the B component can be crosslinked and cured with the terminal hydroxyl polysiloxane in the A component after being mixed with the A component to form a dense crosslinking structure to ensure that the adhesive has excellent mechanical properties and excellent aging stability after curing. In summary, the A component and the B component of the adhesive composition provided by the present application have excellent compatibility, and the adhesive prepared therefrom has excellent thermal conductivity and flame retardancy, heat storage and temperature control performance, anti-aging performance and excellent mechanical properties.

[0067] In one example, the modified aluminum hydroxide includes a silane coupling agent and aluminum hydroxide in a mass ratio of 1: (0.01~0.02). The amino portion of the silane coupling agent can form a hydrogen bond with the hydroxyl group on the surface of the aluminum hydroxide or generate a covalent bond through a condensation reaction to form a modified aluminum hydroxide. The silane coupling agent has excellent compatibility with the terminal hydroxyl polysiloxane, which can act as a bridge between the terminal hydroxyl polysiloxane matrix and the aluminum hydroxide to improve the interfacial bonding strength. In addition, the modified aluminum hydroxide can be used as a flame retardant, which can release moisture and absorb heat at high temperatures, thereby inhibiting the rise in temperature. It can be understood that in the modified aluminum hydroxide, the mass ratio of the silane coupling agent and the aluminum hydroxide can be selected from any value between 1: (0.01~0.02). Specifically, the mass ratio of the silane coupling agent to aluminum hydroxide includes but is not limited to 1:0.01, 1:0.011, 1:0.012, 1:0.013, 1:0.015, 1:0.018, 1:0.019 or 1:0.02.

[0068] In one example, the titanium-containing compound is titanium dioxide.

[0069] In one example, the phase change temperature of the modified coated material is 28° C. to 70° C. Specifically, the phase change temperature of the modified coated material includes but is not limited to 28° C., 30° C., 33° C., 35° C., 36° C., 37° C., 38° C., 40° C., 43° C., 45° C., 48° C., 50° C., 55° C., 60° C., 65° C. or 70° C.

[0070] In one example, the phase change enthalpy of the modified coated material is 200 J / g~240 J / g. Phase change enthalpy refers to the heat absorbed or released when a material changes from one phase to another. From the perspective of phase change enthalpy, the modified coated material provided in the present application can absorb or release higher energy, that is, even if the ambient temperature changes only slightly, the material can absorb or release a large amount of heat, thereby playing a role in temperature buffering. Specifically, the phase change enthalpy of the modified coated material includes but is not limited to 200 J / g, 205 J / g, 210 J / g, 215 J / g, 220 J / g, 225 J / g, 230 J / g, 235 J / g or 240 J / g.

[0071] The particle size of the modified coated material plays an important role in ensuring its dispersion performance. In one example, the average particle size of the modified coated material is 5 μm to 10 μm. Specifically, the average particle size of the modified coated material includes but is not limited to 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm.

[0072] In one example, the silane coupling agent and the silane modifier are each independently selected from one or more of formula (I), Formula (I), wherein n1 is selected from a positive integer between 1 and 10; R 11 , R 12 and R 13 Each is independently a C1~C6 alkyl group; R 14 It is amino.

[0073] Preferably, n1 is 3 or 4; R 11 , R 12 and R 13 Each is independently methyl, ethyl or propyl; R 14 For example, the silane coupling agent and the silane modifier include but are not limited to γ-aminopropyltriethoxysilane ,γ-aminopropyltrimethoxysilane or γ-aminopropyltripropoxysilane .

[0074] In one example, the crosslinking agent includes a tetrafunctional silane compound, a trifunctional silane compound, and a difunctional silane compound in a mass ratio of (2.9~3.3):(0.18~0.25):(0.3~0.35). Alkyl compounds with different numbers of functional groups are compounded to form a crosslinking agent to form a diverse crosslinking network. Among them, the tetrafunctional silane compound can provide a high density of crosslinking points to enhance the rigidity and stability of the system; the trifunctional silane compound introduces a certain degree of flexibility while maintaining the strength of the network; and the difunctional silane compound helps to form a more flexible link, which overall improves the complexity and mechanical properties of the crosslinked network. Specifically, in the cross-linking agent, the mass ratio of the tetrafunctional silane compound, the trifunctional silane compound and the difunctional silane compound includes but is not limited to 3:0.22:0.3, 3:0.22:0.31, 3:0.22:0.32, 3:0.22:0.33, 3:0.22:0.34, 3:0.22:0.35, 3.1:0.22:0.3, 3.1:0.22:0.31, 3.1:0.22:0.32, 3.1:0.22:0.33, 3.1:0.22:0.3 4. 3.1:0.22:0.35, 3.15:0.22:0.3, 3.15:0.22:0.31, 3.15:0.22:0.32, 3.15:0.22:0.33, 3.15:0.22:0.34, 3.15:0.22:0.35, 3.2:0.22:0.3, 3.2:0.22:0.31, 3.2:0.22:0.32, 3.2:0.22:0.33, 3.2:0.22:0.34 or 3.2:0.22:0.35.

[0075] In one example, the structure of the tetrafunctional silane compound is , where R 21 , R 22 , R 23 and R 24 Each is independently a C1~C6 alkyl.

[0076] Preferably, R 21 , R 22 , R 23 and R 24 Each independently is a C1-C3 alkyl group. For example, the tetrafunctional silane compound includes but is not limited to tetraethyl orthosilicate , Methyl orthosilicate And propyl orthosilicate .

[0077] In one example, the structure of the trifunctional silane compound is , where R 31 , R 32 , R 33 and R 34 Each is independently a C1~C6 alkyl.

[0078] Preferably, R 31 , R 32 , R 33 and R 34 Each independently is a C1-C3 alkyl group. For example, the trifunctional silane compound includes but is not limited to methyltrimethoxysilane and ethyltriethoxysilane .

[0079] In one example, the structure of the difunctional silane compound is , where R 41 , R 42 , R 43 and R 44 Each is independently a C1~C6 alkyl.

[0080] Preferably, R 41 , R 42 , R 43 and R 44 Each independently is a C1 to C3 alkyl group. For example, the difunctional silane compound includes but is not limited to dimethyldimethoxysilane , diethyldiethoxysilane and dimethyldiethoxysilane .

[0081] In one example, the coupling agent includes a first silane polymer and a second silane polymer in a mass ratio of (1~2):1.

[0082] Wherein, the structure of the first silane polymer is ; n2 is greater than 1, R 51 , R 52 and R 53 Each independently is a C1~C6 alkyl group, R 54 and R 55 Each is independently a C1~C6 alkylene group.

[0083] Preferably, R 51 , R 52 and R 53 Each independently is a C1~C3 alkyl group, R 54 and R 55 Each independently represents a C1-C3 alkylene group. For example, the structure of the first silane polymer includes but is not limited to N-aminoethyl-γ-aminopropyltrimethoxysilane oligomer and N-aminoethyl-γ-aminopropyltriethoxysilane oligomer Specifically, the viscosity of the first silane polymer is ≤100 mPa·s.

[0084] The structure of the second silane polymer is ; n3 is greater than 1, R 61 , R 62 and R 63 Each independently is a C1~C6 alkyl group, R 64 and R 55 It is a C1~C6 alkylene group.

[0085] Preferably, the R 61 , R 62 and R 63 Each independently is a C1~C3 alkyl group, R 64 and R 55 is a C1-C3 alkylene group. For example, the second silane polymer includes but is not limited to γ-aminopropyltrimethoxysilane oligomer , and γ-aminopropyltriethoxysilane oligomer .

[0086] In one example, the tin catalyst includes one or more of dibutyltin diacetylacetonate, dimethyltin diacetylacetonate, diphenyltin diacetylacetonate, and diisopropyltin diacetylacetonate. The above tin catalysts all include acyl and ketone groups, which are coordination groups and can form a stable chelate structure, so that the catalyst can have good thermal stability and chemical stability; the alkyltin or phenyltin part can be used as an efficient Lewis acid catalyst to promote the dehydration condensation of terminal hydroxyl polysiloxane.

[0087] In one example, the terminal hydroxyl polysiloxane includes one or more of terminal hydroxyl polydimethylsiloxane and terminal hydroxyl polydiethylsiloxane. It is understandable that in the present application, the terminal hydroxyl polydiethylsiloxane can be a monohydroxyl-terminated polysiloxane or a dihydroxyl-terminated polysiloxane. Specifically, the terminal hydroxyl polysiloxane is one or more of α,ω-dihydroxy polydimethylsiloxane, α-hydrogen-ω-hydroxy-polydimethylsiloxane, α,ω-dihydroxy polydiethylsiloxane and α-hydrogen-ω-hydroxy-polydiethylsiloxane. Hydroxyl-terminated polysiloxane is selected, which can be effectively cross-linked and cured with the alkyl silicone oil in component B to ensure the mechanical properties of the adhesive.

[0088] In one example, the viscosity of the hydroxy-terminated polysiloxane at 25° C. is 3000 cps to 4000 cps. It is understood that the viscosity of the hydroxy-terminated polysiloxane at 25° C. includes but is not limited to 3000 cps, 3500 cps, 3800 cps, 4000 cps, 4200 cps, 4500 cps, 4800 cps or 5000 cps.

[0089] In one example, the alkyl silicone oil includes one or more of dimethyl silicone oil and diethyl silicone oil. Dimethyl silicone oil is polydimethylsiloxane, which is methyl-terminated; diethyl silicone oil is polydiethylsiloxane, which is ethyl-terminated.

[0090] In one example, the viscosity of the alkyl silicone oil at 25° C. is 1000 cps to 1500 cps. It is understood that the viscosity of the alkyl silicone oil at 25° C. includes but is not limited to 1000 cps, 1100 cps, 1200 cps, 1300 cps, 1400 cps or 1500 cps.

[0091] In one example, the mass ratio of the component A to the component B is (4.7-5.2):1. Defining the mass ratio of the component A to the component B can fully cross-link the two components to give the adhesive excellent thermal conductivity, flame retardancy and mechanical properties. Specifically, the mass ratio of the component A to the component B includes but is not limited to 4.7:1, 4.8:1, 4.9:1, 5:1, 5.1:1 or 5.2:1.

[0092] The second aspect of the present application provides a method for preparing an adhesive, comprising the following steps:

[0093] Prepare the component A by compounding the component A in the bonding composition described in any one of the examples of the first aspect of the present application;

[0094] The component B is prepared by compounding the component B in the adhesive composition according to any one of claims 1 to 11.

[0095] In one example, the specific preparation steps of the component A include: preparing the components in the adhesive composition described in any example of the first aspect of the present application, stirring under vacuum conditions, and preparing the component A. In the step of preparing component A, the process parameters of the vacuum conditions include: the vacuum degree is -0.095MPa~-0.05MPa. Specifically, the vacuum degree includes but is not limited to -0.095 MPa, -0.09 MPa, -0.08 MPa, -0.07 MPa, -0.06 MPa or -0.05 MPa.

[0096] In one example, the specific preparation steps of the component B include: preparing the components in the adhesive composition described in any example of the first aspect of the present application, stirring under vacuum conditions, and preparing the component B. In the step of preparing component B, the process parameters of the vacuum conditions include: the vacuum degree is -0.095MPa~-0.05MPa. Specifically, the vacuum degree includes but is not limited to -0.095 MPa, -0.09 MPa, -0.08 MPa, -0.07 MPa, -0.06 MPa or -0.05 MPa.

[0097] In one example, the steps of preparing the modified coated material include:

[0098] a1. Mixing the alkane, the surfactant and the first organic alkaline solvent, and heating at a temperature 8° C. to 15° C. higher than the phase transition temperature of the alkane to prepare an oil-in-water solution;

[0099] a2. Adding a titanium source and boron nitride to the oil-in-water solution to prepare a precursor solution;

[0100] a3, adding a water source, a hydrolysis accelerator and a second organic alkaline solvent to the precursor solution to prepare a coated material;

[0101] a4. Mixing the coating material and the silane modifier in a solvent to prepare the modified coating material.

[0102] To ensure sufficient dispersion of the alkane, in one example, in step a1, the mass volume ratio of the alkane, the surfactant and the first organic alkaline solvent is (4-6) g: (1-2) g: (80-120) mL. Specifically, the mixed mass volume ratio of the alkane, the surfactant and the first organic alkaline solvent includes but is not limited to 4g:1.5g:100mL, 4g:1.6g:100mL, 4g:1.7g:100mL, 4g:2g:100mL, 5g:1.5g:100mL, 5g:1.6g:100mL, 5g:1.7g:100mL, 5g:2g:100mL, 5g:1.5g:110mL, 5g:1.6g:110mL, 5g:1.7g:110mL, 5g:2g:110mL, 6g:1.5g:100mL, 6g:1.6g:100mL, 6g:1.7g:100mL or 6g:2g:100mL.

[0103] In one example, in step a1, the surfactant includes one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium lauryl polyoxyethylene ether sulfate, sodium hexadecyl sulfate and sodium dodecyl polyoxyethylene ether sulfate.

[0104] In one example, in step a1, the first organic alkaline solvent is an amide solvent. For example, the first organic alkaline solvent includes but is not limited to formamide, acetamide and propionamide.

[0105] To ensure that the alkane changes from solid to liquid. In one example, in step a1, heating is performed at a temperature 8°C to 15°C higher than the phase transition temperature of the alkane. Specifically, the heating temperature higher than the phase transition temperature of the alkane includes, but is not limited to, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C or 15°C.

[0106] In one example, in step a2, the titanium source includes titanate, for example, the titanate includes one or more of tetrabutyl titanate, tetrapropyl titanate and tetraethyl titanate.

[0107] To ensure that the titanium source and boron nitride are fully dispersed around the alkane and reduce the waste of raw materials. In one example, in step a2, the mass ratio of the alkane, the titanium source, and the boron nitride included in the water-in-oil solution is (4-6): (4-6): (0.15-0.25). Specifically, the mass ratio of the alkane, the titanium source, and the boron nitride included in the water-in-oil solution includes but is not limited to 4:6:0.15, 4:6:0.18, 4:6:0.19, 4:6:0.2, 4:6:0.21, 4:6:0.23, 4:6:0.25, 5:5:0.15, 5:5:0.18, 5:5:0.19, 5:5:0.2, 5:5:0.21, 5:5:0.23 or 5:5:0.25.

[0108] In one example, the specific steps of step a2 include: adding a titanium source to the oil-in-water solution, stirring, and then adding boron nitride and stirring to prepare a precursor solution.

[0109] In one example, in step a2, the boron nitride is a boron nitride nanosheet. The average particle size of the boron nitride nanosheet is 200nm-400nm. Boron nitride nanosheets have better dispersibility than boron nitride powder, and the boron nitride nanosheets can fully disperse the coated material in coordination with the silane modifier.

[0110] In one example, in step a3, the hydrolysis promoter includes an organic acid. For example, the organic acid includes but is not limited to acetic acid, propionic acid, formic acid, citric acid and benzoic acid.

[0111] In an acidic environment, the ester bond in the titanate breaks, which accelerates the hydrolysis reaction rate of the titanate; in addition, the addition of a water source provides the necessary reactants for the hydrolysis of the titanate, which reacts with the titanate to generate a hydroxyl complex of titanium, which further condenses to form titanium dioxide. As the reaction proceeds, the generated hydroxyl complex of titanium and titanium dioxide form aggregates with a high degree of polymerization, and settle due to gravity to generate a precipitate to obtain a coated material. In this step, the second organic alkaline solvent is added as a solvent. Under the reaction conditions of the present application, it has good compatibility with the hydrolysis promoter, and its presence can stabilize the reaction system and better control the hydrolysis and condensation rates of the titanate.

[0112] In one example, in step a3, the second organic alkaline solvent is an amide solvent. For example, the second organic alkaline solvent includes but is not limited to formamide, acetamide and propionamide.

[0113] In one example, in step a4, the mass ratio of the coating material to the silane modifier is 1:(0.01-0.02). Specifically, the mass ratio of the coating material to the silane modifier includes but is not limited to 1:0.01, 1:0.011, 1:0.012, 1:0.015, 1:0.018, 1:0.019 or 1:0.02.

[0114] In one example, in step a4, the solvent includes anhydrous ethanol and water in a volume ratio of (1-2): 1. Specifically, the volume ratio of anhydrous ethanol and water includes but is not limited to 1:1, 1.1:1, 1.2:1, 1.3:1, 1.5:1, 1.6:1, 1.8:1, 1.9:1 or 2:1.

[0115] In one example, the specific steps of step a4 include:

[0116] The coated material and the silane modifier are mixed in a solvent, and after stirring and modification, the modified coated material is prepared. The process parameters for stirring and modification include: a stirring speed of 1500rpm to 2500rpm. Specifically, the speed includes but is not limited to 1500rpm, 1600rpm, 1800rpm, 1900rpm, 2000rpm, 2100rpm, 2200rpm, 2400rpm or 2500rpm.

[0117] In one example, the preparation steps of the modified aluminum hydroxide include:

[0118] Aluminum hydroxide, a silane coupling agent and a ball milling medium are ball milled and mixed, and after drying, the modified aluminum hydroxide is prepared. It can be understood that the modified aluminum hydroxide is aluminum hydroxide modified by a silane coupling agent. During the ball milling process, defects and active sites on the surface of aluminum hydroxide are generated, which is conducive to the condensation reaction of the silane coupling agent with the hydroxyl groups on the surface of aluminum hydroxide to form Si-O-Al bonds; in addition, the silane coupling agent contains amino groups, wherein the amino groups can not only form chemical bonds with aluminum hydroxide, but also have excellent compatibility with the matrix of the terminal hydroxyl polysiloxane, thereby enabling aluminum hydroxide to have excellent dispersibility.

[0119] In one example, the mass ratio of the aluminum hydroxide to the silane coupling agent is 1:(0.01-0.02). Specifically, the mass ratio of the aluminum hydroxide to the silane coupling agent includes but is not limited to 1:0.01, 1:0.011, 1:0.012, 1:0.015, 1:0.018, 1:0.019 or 1:0.02.

[0120] In one example, the ball milling medium includes an alcohol solvent and water in a volume ratio of (1-2): 1. Specifically, the volume ratio of the alcohol solvent and water includes but is not limited to 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1 or 2:1.

[0121] The third aspect of the present application provides an adhesive, which includes the two-component adhesive composition described in any example of the first aspect of the present application, or is prepared by the preparation method described in any example of the second aspect of the present application.

[0122] The fourth aspect of the present application provides a photovoltaic module, characterized by comprising the adhesive described in the third aspect of the present application or comprising a packaging adhesive layer formed after the adhesive described in the third aspect of the present application is cured. It can be understood that the photovoltaic module of the present application includes but is not limited to a photovoltaic junction box.

[0123] When the two-component adhesive provided in the present application is mixed, the catalyst can activate the cross-linking agent, so that the cross-linking agent begins to undergo a hydrolysis reaction under the action of water or moisture to generate a silanol group -Si-OH; the generated silanol group will undergo a condensation reaction with the hydroxyl group on the terminal hydroxyl polysiloxane to generate a Si-O-Si bond, thereby allowing the system to form a three-dimensional cross-linked network and achieve a transition from liquid to solid.

[0124] The following further specific examples are provided to explain the present application in detail. It should also be understood that the following examples are only used to further explain the present application and cannot be understood as limiting the scope of protection of the present application. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present application belong to the scope of protection of the present application. The specific process parameters of the following embodiments are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not necessarily limited to the specific values ​​of the embodiments below.

[0125] [raw material]

[0126] γ-Aminopropyltriethoxysilane: purchased from Jiangsu Chenguang Coupling Agent Co., Ltd., model KH550;

[0127] N-aminoethyl-γ-aminopropyltrimethoxysilane oligomer: purchased from: United Silicon Chemical; model Dynasylan®1146;

[0128] γ-Aminopropyltriethoxysilane oligomer: purchased from: United Silicon Chemical; model Dynasylan®1151 XX;

[0129] Dibutyltin bis(acetylacetonate): purchased from: West Asia Reagents.

[0130] Preparation Example 1

[0131] (1) 5 g of n-hexacosane (phase transition temperature: 56° C.), 1.6 g of sodium dodecyl sulfate and 100 mL of formamide were mixed in a three-necked flask, heated in a water bath at a temperature 14° C. higher than the phase transition temperature of the n-hexacosane, i.e., 70° C., and then stirred at a speed of 2000 r / min for 2 h to prepare an oil-in-water solution;

[0132] (2) Add 5 g of tetrabutyl titanate to the oil-in-water solution and stir for 2 h to disperse it around the micelles of the n-hexacosanoid emulsion; then add 0.2 g of boron nitride nanosheets and stir for 0.5 h to prepare a precursor solution;

[0133] (3) After adding 0.12 g of glacial acetic acid to the precursor solution and stirring for 10 min, 4 mL of deionized water and 25 mL of formamide were slowly added dropwise, and the reaction was continued for 3.5 h to obtain a white precipitate, thereby preparing a coated material, wherein the outer shell of the coated material is titanium dioxide and boron nitride, and the core of the coated material is n-hexacosane;

[0134] (6) Wash the coated material with anhydrous ethanol five times and then dry it for storage.

[0135] (7) The coated material and γ-aminopropyltriethoxysilane KH550 were mixed in a solvent (the volume ratio of anhydrous ethanol and water was 1:1) at a mass ratio of 1:0.02, and the mixture was stirred at a speed of 2000 rpm / min for 1 h for modification. The modified powder was then collected by filtration, dried at 80°C for 5 h, and cooled to room temperature to prepare a silane coupling agent modified coated material. The phase transition temperature of the silane coupling agent modified coated material was 56°C, the phase change enthalpy was 238 J / g, and the average particle size was 7.0 μm.

[0136] Preparation Example 2

[0137] Aluminum hydroxide powder and γ-aminopropyltriethoxysilane KH550 are placed in a ball mill at a mass ratio of 1:0.02; anhydrous ethanol aqueous solution (volume ratio of anhydrous ethanol: water = 2:1) is added until the powder is just submerged; the ball mill is started to modify the aluminum hydroxide powder by ball milling for 30 minutes, and the modified powder is placed in a drying oven and dried at 80°C for 5 hours, cooled to room temperature, and ground to obtain modified aluminum hydroxide powder.

[0138] Embodiment 1 to Embodiment 6

[0139] In the two-component adhesive composition of each embodiment, component A includes: terminal hydroxyl polysiloxane, modified aluminum hydroxide of Preparation Example 2, and silane coupling agent modified coating material of Preparation Example 1; component B includes: alkyl silicone oil, crosslinking agent, coupling agent and tin catalyst. The specific component types and mass fractions are shown in Table 1.

[0140] The preparation steps of the adhesive of each embodiment are as follows:

[0141] Preparation steps of component A: add terminal hydroxyl polysiloxane, modified aluminum hydroxide in Preparation Example 2 and silane coupling agent modified coated material in Preparation Example 1 into a planetary mixer according to weight parts, stir evenly in vacuum in the planetary mixer with a vacuum degree of -0.095 MPa, and discharge the material after 0.5 h for standby use.

[0142] Preparation steps of component B: alkyl silicone oil, crosslinking agent, coupling agent and tin catalyst are added into a planetary mixer according to weight parts, and vacuum stirred evenly in the planetary mixer with a vacuum degree of -0.095 MPa. After 0.5 h, the material is discharged for standby use.

[0143] Mix component A and component B according to the mass ratio.

[0144] Table 1

[0145]

[0146] Comparative Example 1

[0147] In the two-component adhesive composition of Comparative Example 1, component A includes: terminal hydroxyl polysiloxane and modified aluminum hydroxide of Preparation Example 2; component B includes: alkyl silicone oil, crosslinking agent, coupling agent and tin catalyst. The specific component types and mass fractions are shown in Table 2.

[0148] The preparation steps of the adhesive of Comparative Example 1 are as follows:

[0149] Preparation steps of component A: Add terminal hydroxyl polysiloxane and modified aluminum hydroxide of Preparation Example 2 into a planetary mixer according to weight parts, stir evenly in the planetary mixer under vacuum with a vacuum degree of -0.095 MPa, and discharge the material after 0.5 h for standby use.

[0150] Preparation steps of component B: alkyl silicone oil, crosslinking agent, coupling agent and tin catalyst are added into a planetary mixer according to weight parts, and vacuum stirred evenly in the planetary mixer with a vacuum degree of -0.095 MPa. After 0.5 h, the material is discharged for standby use.

[0151] Mix component A and component B according to the mass ratio.

[0152] Comparative Example 2

[0153] In the two-component adhesive composition of Comparative Example 2, component A includes: terminal hydroxyl polysiloxane, aluminum hydroxide and the silane coupling agent modified coating material in Preparation Example 1; component B includes: alkyl silicone oil, crosslinking agent, coupling agent and tin catalyst. The specific component types and mass fractions are shown in Table 2.

[0154] The preparation steps of the adhesive of each embodiment are as follows:

[0155] Preparation steps of component A: Add terminal hydroxyl polysiloxane, aluminum hydroxide and the silane coupling agent modified coated material in Preparation Example 1 into a planetary mixer according to their weight parts, and stir them evenly in a vacuum in the planetary mixer with a vacuum degree of -0.095 MPa. After 0.5 h, discharge the material for standby use.

[0156] Preparation steps of component B: alkyl silicone oil, crosslinking agent, coupling agent and tin catalyst are added into a planetary mixer according to weight parts, and vacuum stirred evenly in the planetary mixer with a vacuum degree of -0.095 MPa. After 0.5 h, the material is discharged for standby use.

[0157] Mix component A and component B according to the mass ratio.

[0158] Comparative Example 3

[0159] In the two-component adhesive composition of Comparative Example 3, component A includes: terminal hydroxyl polysiloxane and the silane coupling agent modified coating material in Preparation Example 1; component B includes: alkyl silicone oil, crosslinking agent, coupling agent and tin catalyst. The specific component types and mass fractions are shown in Table 1.

[0160] The preparation steps of the adhesive of each embodiment are as follows:

[0161] Preparation steps of component A: Add terminal hydroxyl polysiloxane and the silane coupling agent modified coating material in Preparation Example 1 into a planetary mixer according to weight parts, and vacuum stir evenly in the planetary mixer with a vacuum degree of -0.095 MPa. After 0.5 h, discharge the material for standby use.

[0162] Preparation steps of component B: alkyl silicone oil, crosslinking agent, coupling agent and tin catalyst are added into a planetary mixer according to weight parts, and vacuum stirred evenly in the planetary mixer with a vacuum degree of -0.095 MPa. After 0.5 h, the material is discharged for standby use.

[0163] Mix component A and component B according to the mass ratio.

[0164] Table 2

[0165]

[0166] The adhesives prepared in the above embodiments and comparative examples were subjected to the following tests:

[0167] (1) Mixed viscosity: Test the mixed viscosity of the adhesive according to GB-T 2794-2013;

[0168] (2) Thermal conductivity: Refer to GB / T11205 standard to test thermal conductivity;

[0169] (2) Tensile strength: Test the tensile strength of the adhesive according to GB / T 528 standard;

[0170] (3) Enthalpy value: Enthalpy value was measured by differential scanning calorimetry (DSC);

[0171] (4) Colloid state after HAST treatment: Perform highly accelerated temperature and humidity stress test (HAST) according to JESD22-A110, at a temperature of 121°C and a humidity of 100% RH. Visually inspect the state of the colloid after 72 hours.

[0172] The test results of the adhesives prepared in the embodiments and comparative examples are shown in Table 3:

[0173] Table 3

[0174]

[0175] In the embodiment, the viscosity and thermal conductivity of the adhesive using the modified coating material as the filler are not significantly different from those of the comparative example. However, in the embodiment of the adhesive using the modified coating material as the filler, the enthalpy value of the adhesive at the phase change temperature is much higher than that of the comparative example 1, indicating that the adhesive provided in the embodiment of the present application has a good heat storage and temperature control function, that is, the adhesive provided in the embodiment of the present application can absorb a large amount of heat, and cause the adhesive to undergo a slight temperature change. Therefore, the adhesive provided in the present application can effectively prevent the problem of excessive temperature in the photovoltaic junction box. In addition, it can be seen from comparative examples 2 and 3 that the aging stability of the adhesive can be improved by compounding the modified coating material and the modified aluminum hydroxide, and it can be ensured that the mechanical properties of the adhesive meet the requirements (≥0.8Mpa).

[0176] By comparing Example 3 and Example 6, it is found that in Example 6, dimethyldimethoxysilane crosslinking agent is not selected, so that the thermal conductivity and enthalpy value of the adhesive are slightly reduced; in Example 7, γ-aminopropyltriethoxysilane oligomer coupling agent is not selected, and the enthalpy value of the adhesive in Example 7 is slightly reduced.

[0177] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0178] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solutions of the present application in detail, but cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present application, which all belong to the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent of this application shall be based on the contents of the attached claims, and the description can be used to interpret the contents of the claims.

Claims

1. A two-component adhesive composition, characterized in that: It includes component A and component B. In parts by weight, the component A comprises: 48 to 53 parts of terminal hydroxyl polysiloxane, 6 to 12 parts of modified aluminum hydroxide, and 41 to 46 parts of modified coating material; In parts by weight, the component B includes: 55 to 60 parts of alkyl silicone oil, 36 to 40 parts of a cross-linking agent, 4 to 6 parts of a coupling agent, and 0.1 to 0.3 parts of a tin catalyst; Among them, the modified aluminum hydroxide is aluminum hydroxide modified by a silane coupling agent, the shell layer of the modified coated material includes a titanium-containing compound modified by a silane modifier and boron nitride modified by a silane modifier, the core of the modified coated material includes an alkane with a carbon number of 18 to 30, and the phase transition temperature of the alkane is 28°C to 70°C; the silane coupling agent and the silane modifier each independently contain one or more amino groups.

2. The two-component adhesive composition according to claim 1, characterized in that: The modified aluminum hydroxide comprises a silane coupling agent and aluminum hydroxide in a mass ratio of 1:(0.01-0.02).

3. The two-component adhesive composition according to claim 1, characterized in that: The core of the modified coated material includes normal alkanes with 18 to 30 carbon atoms; and / or, The titanium-containing compound is titanium dioxide.

4. The two-component adhesive composition according to any one of claims 1 to 3, characterized in that: The modified coated material has one or more of the following characteristics: (1) The phase change temperature of the modified coated material is 28°C to 70°C; (2) The phase change enthalpy of the modified coated material is 200 J / g~240 J / g; (3) The average particle size of the modified coated material is 5 μm to 10 μm.

5. The two-component adhesive composition according to any one of claims 1 to 3, characterized in that: The silane coupling agent and the silane modifier are each independently selected from one or more of formula (I), Formula (I), wherein n1 is selected from a positive integer between 1 and 10; R 11 , R 12 and R 13 Each is independently a C1~C6 alkyl group; R 14 It is amino.

6. The two-component adhesive composition according to any one of claims 1 to 3, characterized in that: The cross-linking agent comprises a tetrafunctional silane compound, a trifunctional silane compound and a difunctional silane compound in a mass ratio of (2.9-3.3):(0.18-0.25):(0.3-0.35).

7. The two-component adhesive composition according to claim 6, characterized in that: The cross-linking agent has one or more of the following characteristics: (1) The structure of the tetrafunctional silane compound is , where R 21 , R 22 , R 23 and R 24 Each is independently a C1~C6 alkyl; (2) The structure of the trifunctional silane compound is , where R 31 , R 32 , R 33 and R 34 Each is independently a C1~C6 alkyl; (3) The structure of the difunctional silane compound is , where R 41 , R 42 , R 43 and R 44 Each is independently a C1~C6 alkyl.

8. The two-component adhesive composition according to any one of claims 1 to 3, characterized in that: The coupling agent comprises a first silane polymer and a second silane polymer in a mass ratio of (1-2):1; Wherein, the structure of the first silane polymer is ; n2 is greater than 1, R 51 , R 52 and R 53 Each independently is a C1~C6 alkyl group, R 54 and R 55 Each independently is a C1~C6 alkylene group; The structure of the second silane polymer is ; n3 is greater than 1, R 61 , R 62 and R 63 Each independently is a C1~C6 alkyl group, R 64 and R 55 It is a C1~C6 alkylene group.

9. The two-component adhesive composition according to any one of claims 1 to 3, characterized in that: The tin catalyst includes one or more of dibutyltin bisacetylacetonate, dimethyltin bisacetylacetonate, diphenyltin bisacetylacetonate and diisopropyltin bisacetylacetonate.

10. The two-component adhesive composition according to any one of claims 1 to 3, characterized in that: The two-component adhesive composition has one or more of the following characteristics: (1) The terminal hydroxyl polysiloxane includes one or more of terminal hydroxyl polydimethylsiloxane and terminal hydroxyl polydiethylsiloxane; (2) The viscosity of the hydroxy-terminated polysiloxane at 25° C. is 3000 cps to 4000 cps; (3) The alkyl silicone oil includes one or more of dimethyl silicone oil and diethyl silicone oil; (4) The viscosity of the alkyl silicone oil at 25° C. is 1000 cps to 1500 cps.

11. The two-component adhesive composition according to any one of claims 1 to 3, characterized in that: The mass ratio of the component A to the component B is (4.7-5.2):

1.

12. A method for preparing an adhesive, characterized in that: The following steps are involved: Prepare the component A by compounding the component A in the adhesive composition according to any one of claims 1 to 11; The component B is prepared by compounding the component B in the adhesive composition according to any one of claims 1 to 11.

13. The preparation method according to claim 12, characterized in that: The preparation steps of the modified coated material include: The alkane, the surfactant and the first organic alkaline solvent are mixed, and heated at a temperature 8° C. to 15° C. higher than the phase transition temperature of the alkane to prepare an oil-in-water solution; Adding a titanium source and boron nitride to the oil-in-water solution to prepare a precursor solution; Adding a water source, a hydrolysis accelerator and a second organic alkaline solvent to the precursor solution to prepare a coated material; Mixing the coating material and the silane modifier in a solvent to prepare the modified coating material; Wherein, the titanium source comprises titanate.

14. The preparation method according to claim 13, characterized in that: The preparation steps of the modified coated material have one or more of the following characteristics: (1) The mass volume ratio of the alkane, the surfactant and the first organic alkaline solvent is (4-6) g: (1-2) g: (80-120) mL; (2) The surfactant includes one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium lauryl polyoxyethylene ether sulfate, sodium hexadecyl sulfate and sodium dodecyl polyoxyethylene ether sulfate; (3) The hydrolysis promoter includes an organic acid; (4) the first organic alkaline solvent and the second organic alkaline solvent are each independently an amide solvent; (5) The mass ratio of the coating material to the silane modifier is 1:(0.01-0.02).

15. The preparation method according to claim 12 or 13, characterized in that: The preparation steps of the modified aluminum hydroxide include: Aluminum hydroxide, a silane coupling agent and a ball milling medium are ball milled and mixed, and then dried to prepare the modified aluminum hydroxide.

16. The preparation method according to claim 15, characterized in that: The preparation steps of the modified aluminum hydroxide have one or more of the following characteristics: (1) The mass ratio of the aluminum hydroxide to the silane coupling agent is 1:(0.01-0.02); (2) The ball milling medium includes an alcohol solvent and water in a volume ratio of (1-2):

1.

17. An adhesive, characterized in that: The adhesive comprises the two-component adhesive composition according to any one of claims 1 to 11, or is prepared by the preparation method according to any one of claims 12 to 16.

18. A photovoltaic module, characterized in that: The invention comprises the adhesive according to claim 17 or comprises a packaging adhesive layer formed after the adhesive according to claim 17 is cured.