Fluorescent gold and silver nano-cluster as well as preparation method and application thereof
By using a combination of dithiocarbamate ligands, chloroauric acid, and silver nitrate in biological imaging, fluorescent gold and silver nanoclusters with near-infrared fluorescence, high quantum yield, and low cytotoxicity were successfully prepared to solve the problem. It overcomes the application limitations of fluorescent metal nanoclusters in biological imaging in the existing technology, and achieves stable and efficient biological imaging probes.
Patent Information
- Application Number
- CN202410742518.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-11
AI Technical Summary
It is difficult for existing fluorescent metal nanoclusters to possess near-infrared fluorescence, high quantum yield and good stability at the same time, which limits their application in biological imaging.
Using dithiocarbamates as ligand molecules and protective agents, fluorescent gold and silver nanoclusters were synthesized through a one-pot method, using chloroauric acid and silver nitrate as metal sources, and under the action of reducing agents, nanoclusters with good stability and Water-soluble, near-infrared fluorescent, and high quantum yield fluorescent gold and silver nanoclusters.
It achieves high stability, water solubility and high quantum yield of fluorescent gold and silver nanoclusters, reduces cytotoxicity, and is suitable for large-scale industrial production and biological imaging applications.
Smart Images

Figure CN118772872A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanomaterials, and in particular to a fluorescent gold-silver nanocluster and a preparation method and application thereof. Background Art
[0002] With the rapid development of nanotechnology, nanofluorescent materials have attracted widespread attention as emerging fluorescent materials, and also provided a good development opportunity for the design and development of nanobiosensors. Currently, the most widely studied fluorescent nanomaterials include carbon dots, graphene quantum dots, semiconductor quantum dots, and fluorescent metal nanoclusters. Among them, fluorescent metal nanoclusters have broad application prospects in biological small molecule sensing, biomarker imaging, biomedicine, etc. due to their unique optical properties, easy surface modification and functionalization, low biotoxicity, good light irradiation stability, good biocompatibility, and large Stokes shift.
[0003] At the same time, because biological tissues exhibit very low absorption and self-background fluorescence in the near-infrared spectral window (650-900nm wavelength), and near-infrared fluorescence can penetrate heterogeneous living tissues several centimeters away, the existing technology often uses nanoprobes such as near-infrared organic dyes and semiconductor quantum dots when performing in vivo imaging. However, organic dyes have poor hydrophilicity and photostability, and the semiconductor quantum dots currently reported to be used have high cytotoxicity and self-aggregation in living cells, which greatly limits the practical biological applications of near-infrared dyes and semiconductor quantum dots.
[0004] Therefore, the combination of near-infrared luminescence properties and fluorescent metal nanoclusters has the potential to be applied to in vivo imaging. In particular, the use of near-infrared fluorescent metal nanoclusters can alleviate the limitations of traditional near-infrared organic dyes and semiconductor quantum dots. However, the fluorescent metal nanoclusters reported so far are difficult to simultaneously possess the advantages of near-infrared fluorescence, high quantum yield, and good stability, which greatly limits the application of fluorescent metal nanoclusters in in vivo imaging. Therefore, it is urgent to provide a solution to improve this problem. Summary of the invention
[0005] The purpose of the present invention is to provide a fluorescent gold-silver nanocluster and a preparation method and application thereof. The preparation method is simple to operate, has good stability and high reproducibility, and is conducive to large-scale industrial production of fluorescent gold-silver nanocluster. At the same time, the prepared fluorescent gold-silver nanocluster has good stability, water solubility, near-infrared fluorescence and high quantum yield.
[0006] In the first aspect, the preparation method provided by the present invention adopts dithiocarbamate as a ligand molecule and a protective agent, and adopts chloroauric acid and silver nitrate as metal sources, and synthesizes fluorescent gold-silver nanoclusters by a one-pot method under the action of a reducing agent. The preparation method is simple and has good repeatability, and the prepared fluorescent gold-silver nanoclusters have good stability, water solubility, near-infrared fluorescence, high quantum yield and low cytotoxicity.
[0007] Optionally, the preparation of the dithiocarbamate ligand includes the following steps: stirring and mixing a barium hydroxide solution, a carbamic acid solution and acetone to obtain a precursor solution; dropping carbon disulfide into the precursor solution, stirring for reaction, centrifuging, washing and drying to obtain an intermediate precipitate; dissolving the intermediate precipitate in a sodium carbonate solution and removing the precipitate to obtain a dithiocarbamate ligand solution.
[0008] Optionally, the solute in the amino formic acid substance solution includes at least one of 3-piperidinic acid, DL-piperidinic acid, isoniperidinic acid, 3-methylaminopropionic acid, proline, and hydroxyproline.
[0009] Optionally, the process of stirring and mixing the barium hydroxide solution, the carbamic acid solution and the acetone includes: stirring and mixing the barium hydroxide solution and the carbamic acid solution at 0-6° C., and then adding acetone and stirring and mixing.
[0010] Optionally, after the barium hydroxide solution and the carbamic acid substance solution are stirred and mixed, the molar mixing ratio of the barium hydroxide to the carbamic acid substance is 1:1.09.
[0011] Optionally, after stirring and mixing the chloroauric acid solution, the silver nitrate solution and the dithiocarbamate ligand solution, a reducing agent is added, and the mixture is stirred and reacted at 50-100° C. for 1-12 h. After separation and purification, the mixture is dialyzed and freeze-dried at -50° C. to obtain fluorescent gold-silver nanoclusters.
[0012] Optionally, during the process of stirring and mixing the chloroauric acid solution, the silver nitrate solution and the dithiocarbamate ligand solution, the molar mixing ratio of chloroauric acid, silver nitrate and dithiocarbamate ligand is 4:1:40.
[0013] Optionally, the reducing agent comprises ascorbic acid.
[0014] In a second aspect, the present invention also provides a fluorescent gold-silver nanocluster prepared by any of the above optional preparation methods.
[0015] In a third aspect, the present invention also provides an application of fluorescent gold-silver nanoclusters prepared by any of the above optional preparation methods in fluorescent probes.
[0016] Optionally, the fluorescent gold-silver nanoclusters are used as fluorescent probes in in vivo imaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The H-NMR spectrum and C-NMR spectrum of the dithiocarbamate ligand prepared in Preparation Example 1 of the present invention;
[0018] Figure 2 The three-dimensional fluorescence spectrum, ultraviolet absorption spectrum and emission spectrum of the fluorescent gold-silver nanoclusters prepared in Example 1 of the present invention;
[0019] Figure 3 This is a stability spectrum of the fluorescent gold-silver nanoclusters prepared in Example 1 of the present invention;
[0020] Figure 4 This is the anti-interference spectrum of the fluorescent gold-silver nanoclusters prepared in Example 1 of the present invention;
[0021] Figure 5 This is a graph showing the cytotoxicity of the fluorescent gold-silver nanoclusters prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0023] The present invention provides a method for preparing fluorescent gold-silver nanoclusters, comprising synthesizing fluorescent gold-silver nanoclusters by a one-pot method under the action of a reducing agent by using dithiocarbamate as a ligand molecule and a protective agent, chloroauric acid and silver nitrate as metal sources. Specifically, the method for preparing fluorescent gold-silver nanoclusters comprises the following steps:
[0024] S1. In the presence of a reducing agent, a chloroauric acid solution, a silver nitrate solution and a dithiocarbamate ligand solution are stirred and mixed to obtain a reaction solution;
[0025] S2. After reacting the reaction solution at 50-100° C. for 1-12 hours, the solution is separated, purified and dialyzed, and then freeze-dried at -50° C. to obtain fluorescent gold and silver nanoclusters.
[0026] In some embodiments, during the execution of step S1, the reducing agent used includes at least one of ascorbic acid, sodium borohydride, sodium cyanoborohydride, and hydrazine hydrate.
[0027] In some embodiments, after performing step S1 to stir and mix the chloroauric acid solution, the silver nitrate solution and the dithiocarbamate ligand, the molar mixing ratio of chloroauric acid, silver nitrate and the dithiocarbamate ligand is 4:1:40.
[0028] In fact, the preparation of the dithiocarbamate ligand solution used in step S1 includes the following steps:
[0029] D1. Mixing barium hydroxide solution, carbamate solution and acetone to obtain a precursor solution;
[0030] D2, adding carbon disulfide dropwise into the precursor solution, stirring for reaction, centrifuging, washing and drying to obtain an intermediate precipitate;
[0031] D3. Dissolve the intermediate precipitate in sodium carbonate solution and remove the precipitate to obtain a dithiocarbamate ligand solution.
[0032] In some embodiments, the solute of the amino acid solution used in step D1 includes at least one of 3-piperidinic acid, DL-piperidinic acid, isoniperidinic acid, 3-methylaminopropionic acid, proline, and hydroxyproline.
[0033] In some embodiments, after performing step D1 to stir and mix the barium hydroxide solution, the carbamic acid substance solution and acetone, the molar mixing ratio of the barium hydroxide to the carbamic acid substance is 1:1.09.
[0034] In fact, during the process of performing step D1, the barium hydroxide solution used is an aqueous solution of barium hydroxide, and the carbamic acid substance is an aqueous solution of carbamic acid substances. Specifically, the barium hydroxide solution can be prepared by stirring and dissolving barium hydroxide octahydrate in deionized water, and the carbamic acid substance can be stirred and dissolved in deionized water to prepare the carbamic acid substance solution.
[0035] In some embodiments, during the process of performing step D1, the barium hydroxide solution and the carbamic acid solution are stirred and mixed at 0-6° C., and then acetone is added and stirred and mixed to obtain a precursor solution.
[0036] In some embodiments, during the step D2 of adding carbon disulfide dropwise to the precursor solution, the total duration of the carbon disulfide addition is controlled to be 14 minutes, and the mass ratio of the added carbon disulfide to the carbamic acid substance is 0.595:1.
[0037] In some embodiments, after the stirring reaction in step D2 is performed and centrifuged, a barium salt precipitate can be separated, and the precipitate obtained by centrifugation is repeatedly washed with acetone to remove the reactants and impurities attached to the precipitate, and an intermediate precipitate is obtained after vacuum drying.
[0038] In some embodiments, performing step D3 to dissolve the intermediate precipitate in a sodium carbonate solution can remove barium ions in the intermediate precipitate, thereby preparing a dithiocarbamate ligand solution.
[0039] In fact, in the process of performing separation and purification in step S2, polyacrylamide gel electrophoresis can be used. Specifically, in the process of performing dialysis in step S2, the dialysis bag used is MW1500D, and the dialysis time is controlled to be 10-15 days.
[0040] Preparation Example 1
[0041] Preparation Example 1 of the present invention provides a method for preparing a dithiocarbamate ligand, comprising the following steps:
[0042] D1. Weigh 0.7865 g of barium hydroxide hydrate and dissolve it in 4 mL of deionized water to prepare a barium hydroxide solution; weigh 0.2964 g of 3-piperidinic acid and dissolve it in 3 mL of deionized water to prepare a 3-piperidinic acid solution; at 6° C., stir and mix the barium hydroxide solution, 3-piperidinic acid and 18 mL of acetone to prepare a precursor solution;
[0043] D2, adding 0.14 mL of carbon disulfide dropwise into the precursor solution, stirring at 800 rpm for 2 h, centrifuging at 12500 rpm to separate the precipitate, washing the precipitate three times with acetone, and vacuum drying the precipitate to obtain an intermediate precipitate;
[0044] D3. Dissolve the intermediate precipitate in a sodium carbonate aqueous solution, stir and mix, and then filter out the precipitate to obtain a dithiocarbamate ligand solution.
[0045] Explore Example
[0046] This exploratory example provides a method for preparing fluorescent gold-silver nanoclusters, comprising the following steps:
[0047] S1. Stir and mix 20-200 μL of 20 mmol / L chloroauric acid solution and 10-140 μL of 10 mmol / L silver nitrate solution, then add 160-320 μL of 100 mmol / L dithiocarbamate ligand solution and 50-300 μL of 100 mmol / L ascorbic acid solution, add ultrapure water, stir and mix, and then dilute to 1000 μL to obtain a reaction solution;
[0048] S2. The reaction solution is heated in a 50-100°C water bath environment for 1-12 hours to obtain a fluorescent gold-silver nanocluster mixed solution. The mixed solution is separated and purified by polyacrylamide gel electrophoresis, and then dialyzed using a MW1500D dialysis bag for 10-15 days. The dialyzed product is vacuum freeze-dried at -50°C to obtain fluorescent gold-silver nanoclusters.
[0049] With the increase of the dosage of chloroauric acid solution, the fluorescence intensity and yield of the fluorescent gold-silver nanoclusters gradually increased and then gradually weakened, and the optimal dosage was reached at 120 μL; with the increase of the dosage of silver nitrate solution, the fluorescence intensity and yield of the fluorescent gold-silver nanoclusters gradually increased and then gradually balanced, and the optimal dosage was reached at 60 μL; with the increase of the dosage of dithiocarbamate ligand, the fluorescence intensity and yield gradually increased and then gradually weakened, and the optimal dosage was 240 μL; with the increase of the dosage of ascorbic acid, the fluorescence intensity and yield gradually increased and then gradually weakened, and the optimal dosage was 150 μL; with the increase of reaction temperature, the fluorescence intensity gradually increased and then gradually balanced, and the optimal reaction temperature was 80 °C; with the increase of reaction time, the fluorescence intensity gradually increased and then weakened, and the optimal reaction time was 4 h.
[0050] Example 1
[0051] Based on the optimal parameters explored in the exploratory example, this embodiment 1 provides a method for preparing fluorescent gold-silver nanoclusters, comprising the following steps:
[0052] S1, 120 μL of 20 mmol / L chloroauric acid solution and 60 μL of 10 mmol / L silver nitrate solution were stirred and mixed, and then 240 μL of 100 mmol / L dithiocarbamate ligand solution and 150 μL of 100 mmol / L ascorbic acid solution were added, and ultrapure water was added, stirred and mixed, and the volume was fixed to 1000 μL to obtain a reaction solution;
[0053] S2. The reaction solution was heated in a water bath at 80°C for 4 hours to obtain a fluorescent gold-silver nanocluster mixed solution. The mixed solution was separated and purified by polyacrylamide gel electrophoresis, and then dialyzed for 13 days using a MW1500D dialysis bag. The dialyzed product was freeze-dried at -50°C to obtain fluorescent gold-silver nanoclusters.
[0054] Performance Testing
[0055] The dithiocarbamate ligand prepared in Preparation Example 1 was characterized by H NMR and C NMR, respectively. Figure 1 (A) and Figure 1 (B)
[0056] The fluorescent gold-silver nanoclusters prepared in Example 1 were characterized by three-dimensional excitation-emission matrix spectroscopy. Figure 2 (A) and UV-visible light and absorption spectroscopy characterization. Figure 2 (B)
[0057] The stability of the fluorescent gold and silver nanoclusters (10 mM PBS buffer pH 7.4) prepared in Example 1 was investigated as follows Figure 3 As shown, the anti-interference performance is investigated as follows Figure 4 As shown; the cytotoxicity of the fluorescent gold-silver nanoclusters prepared in Example 1 was investigated as follows Figure 5 shown.
[0058] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A method for preparing fluorescent gold and silver nanoclusters, characterized in that: Fluorescent gold-silver nanoclusters were synthesized by a one-pot method using dithiocarbamate as ligand molecule and protective agent, chloroauric acid and silver nitrate as metal sources in the presence of a reducing agent.
2. The preparation method according to claim 1, characterized in that: The preparation of the dithiocarbamate ligand comprises the following steps: The precursor solution is prepared by mixing the barium hydroxide solution, the carbamic acid substance solution and acetone; Add carbon disulfide dropwise into the precursor solution, stir for reaction, centrifuge, wash and dry to obtain an intermediate precipitate; The intermediate precipitate is dissolved in a sodium carbonate solution and the precipitate is removed to prepare a dithiocarbamate ligand solution.
3. The preparation method according to claim 2, characterized in that: The solute in the amino formic acid substance solution includes at least one of 3-piperidinic acid, DL-piperidinic acid, isoniperidinic acid, 3-methylaminopropionic acid, proline and hydroxyproline.
4. The preparation method according to claim 3, characterized in that: The process of stirring and mixing the barium hydroxide solution, the carbamic acid solution and the acetone includes: stirring and mixing the barium hydroxide solution and the carbamic acid solution at 0-6°C, and then adding acetone and stirring and mixing; wherein, after the barium hydroxide solution and the carbamic acid solution are stirred and mixed, the molar mixing ratio of the barium hydroxide to the carbamic acid is 1:1.
09.
5. The preparation method according to any one of claims 1 to 4, characterized in that: After the chloroauric acid solution, silver nitrate solution and dithiocarbamate ligand solution are stirred and mixed, a reducing agent is added, and the mixture is stirred and reacted at 50-100° C. for 1-12 hours. After separation and purification, the mixture is dialyzed and freeze-dried at -50° C. to obtain fluorescent gold-silver nanoclusters.
6. The preparation method according to claim 5, characterized in that: During the process of stirring and mixing the chloroauric acid solution, the silver nitrate solution and the dithiocarbamate ligand solution, the molar mixing ratio of chloroauric acid, silver nitrate and dithiocarbamate ligand is 4:1:
40.
7. The preparation method according to claim 5, characterized in that: The reducing agent includes at least one of ascorbic acid, sodium borohydride, sodium cyanoborohydride and hydrazine hydrate.
8. A fluorescent gold-silver nanocluster prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the fluorescent gold-silver nanoclusters prepared by the preparation method according to any one of claims 1 to 7 in fluorescent probes.
10. The use according to claim 9, characterized in that: The invention includes the application of the fluorescent gold-silver nanoclusters as fluorescent probes in biological in vivo imaging.
Citation Information
Patent Citations
Method for preparing CdTe quantum dots in aqueous phase and at low temperature
CN102191038A
Preparation method of gold-silver bimetal nanocluster capable of generating near-infrared electrochemical luminescence radiation