Blue-light perovskite luminescent material, light-emitting diode and preparation method

By adding 4-bromothiophene-2-carbaldehyde and butylamine in the preparation of perovskite materials, the problem of low performance of blue perovskite light-emitting diodes is solved, spectral stability and high external quantum efficiency are achieved, and the performance of light-emitting diodes is improved. Overall performance.

CN118772877APending Publication Date: 2024-10-15SHANGHAI UNIV

Patent Information

Application Number
CN202410559044.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-07
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The performance of blue perovskite light-emitting diodes lags behind that of red and green perovskite light-emitting diodes, and due to the difficulty in controlling the morphology of nanosheets and the problem of ligand shedding, carrier transmission is limited and surface defects increase, affecting optoelectronics. performance.

Method used

By adding 4-bromothiophene-2-carbaldehyde (BTC) when preparing perovskite materials, its thiophene group is used to guide the two-dimensional growth and crystallization growth kinetics of nanosheets, combined with the use of butylamine to stabilize the nanosheet structure, Reduce carrier non-radiative recombination and fluorescence quantum yield decay.

Benefits of technology

It has achieved spectral stability and high external quantum efficiency of blue perovskite luminescent materials, improved the brightness and performance of light-emitting diodes, and the external quantum efficiency can reach 5.44%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772877A_ABST
    Figure CN118772877A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of photoelectric materials, and particularly relates to a blue-light perovskite luminescent material, a light-emitting diode and a preparation method thereof.The preparation method comprises the steps that lead bromide, oleic acid, oleylamine, didodecane dimethyl ammonium bromide and 4-bromothiophene-2-formaldehyde are added into 1-octadecene, stirring is conducted at the temperature of 120-130 DEG C, and a lead precursor solution is obtained; stirring cesium carbonate and oleic acid at 90-110 DEG C to obtain a cesium precursor solution; and adding the cesium precursor solution into the lead precursor solution, injecting isopropanol, heating the mixed solution to 70-80 DEG C, keeping the temperature for a period of time, transferring the mixed solution into an ice-water bath, injecting toluene to obtain a nanosheet coarse solution, and purifying to obtain the blue luminescent material. The blue light-emitting material comprises a nanometer sheet-shaped cesium-lead-bromine perovskite material. According to the invention, the surface defects of the perovskite nanosheet can be passivated, and the brightness and external quantum efficiency of the light-emitting diode can be improved. The patent of the invention is subsidized by the national key research and development plan 2022YFE0200200.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of optoelectronic materials, and in particular relates to a blue light perovskite luminescent material, a light emitting diode and a preparation method thereof. Background Art

[0002] Perovskite light-emitting diodes (PeLEDs), as a new type of optoelectronic device, have attracted much attention due to their excellent spectral tunability, high color purity brought by narrow half-width, and high external quantum efficiency. At present, with the continuous efforts of researchers, the external quantum efficiency of red and green perovskite light-emitting diodes exceeds 20%, making PeLEDs a strong candidate for next-generation display devices and solid-state lighting applications. However, the device performance of blue perovskite light-emitting diodes lags far behind that of red and green perovskite light-emitting diodes, which seriously hinders the development of perovskite full-color gamut display devices. Therefore, it is urgent to promote the commercial development of PeLEDs and improve the performance of blue PeLEDs.

[0003] So far, there are two main strategies for achieving blue light (460nm-470nm) emission from perovskites: The second strategy involves a mixed halogen method to achieve blue light emission from perovskites. This method introduces chloride ions and bromide ions into the precursor at the same time when preparing perovskite films to form bromine-chlorine mixed perovskite crystals, ultimately achieving regulation of the emission peak position of metal halide perovskites. However, the PeLED prepared by the bromine-chlorine mixing strategy will undergo halogen separation under high voltage, causing the emission spectrum to red-shift. The second strategy involves synthesizing perovskites with quantum confinement effects, broadening the bandgap of perovskite materials, and preparing blue light-emitting diodes. The preparation of nanosheets with strong quantum confinement effects has become an effective way to achieve blue light emission from perovskites. However, since the control of the morphology of nanosheets requires the introduction of a large number of organic insulating ligands, this will seriously hinder the transport of carriers and limit the device performance of the prepared light-emitting diodes. At the same time, the commonly used long-chain oleylamine ligands are easily detached from the perovskite surface, resulting in a large number of defects on the perovskite surface, which affects the photoelectric properties of the perovskite. Therefore, it is very important to find a strategy that can both improve carrier transport and reduce perovskite surface defects to achieve efficient perovskite blue light-emitting diodes. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a blue light perovskite luminescent material, a light emitting diode and a preparation method. The method can prepare a blue light perovskite luminescent material with stable electroluminescence spectrum and excellent performance.

[0005] To achieve the above object, the technical solution included in the present invention is as follows: A method for preparing a blue light perovskite luminescent material, comprising:

[0006] Lead bromide (PbBr2), oleic acid (OA), oleylamine (OLA), didodecyl dimethyl ammonium bromide (DDAB), and 4-bromothiophene-2-carboxaldehyde (BTC) are added to 1-octadecene (ODE), and stirred at 120-130° C. to obtain a lead precursor solution;

[0007] Cesium carbonate (Cs2CO3) and oleic acid (OA) are stirred at 90-110° C. to obtain a cesium precursor solution;

[0008] The cesium precursor solution is added to the lead precursor solution, isopropanol is injected, the mixed solution is heated to 70-80°C, and after keeping warm for a period of time, the mixed solution is transferred to an ice water bath, toluene is injected to obtain a crude nanosheet solution, and the blue light-emitting material is obtained by purification. The blue light-emitting material includes a nanosheet-shaped cesium lead bromine perovskite material passivated with 4-bromothiophene-2-carboxaldehyde.

[0009] The molar ratio of lead bromide, 4-bromothiophene-2-carboxaldehyde and didodecanedimethylammonium bromide is 4:(2.5-4):1.

[0010] Wherein, in the preparation of the lead precursor solution, the volume ratio of 1-octadecene, oleic acid and oleylamine is 8:1:1.

[0011] Among them, Cs in the cesium precursor solution + The molar concentration is 0.1~0.2mmol / mL.

[0012] After keeping warm for a period of time, the mixed solution is transferred to an ice water bath, the keeping warm time is 10 min to 12 min, and the ice water bath time is 3 min to 5 min.

[0013] Wherein, the volume ratio of toluene to the mixed solution is (2-3):1.

[0014] The purification process includes: adding a first polar solvent to a crude solution of nanosheets, performing a first centrifugal treatment, and obtaining a first precipitate; dissolving the first precipitate in a first organic solvent, adding a second organic solvent containing butylamine and a first polar solvent, and performing a second centrifugal treatment to obtain a second precipitate, wherein the second precipitate includes nanosheet-shaped cesium lead bromine perovskite material.

[0015] Wherein, the first polar solvent includes methyl acetate; and the volume ratio of the crude nanosheet solution to the polar solvent is 1:3.

[0016] The centrifuge speed for the first centrifugal treatment is 4000-5000 rpm, and the centrifugal treatment time is 5-10 minutes.

[0017] The first organic solvent includes n-hexane; the second organic solvent includes toluene, and the mass concentration of the second organic solvent containing butylamine is 10%.

[0018] The volume ratio of the first organic solvent, the second polar solvent and the second organic solvent containing butylamine in the first precipitate is 1:1:(0.001-0.005).

[0019] The second centrifugal treatment has a centrifuge speed of 6000-7000 rpm and a time of 2-3 min.

[0020] The present invention also includes a technical solution of the second aspect, a blue light perovskite luminescent material prepared by the above-mentioned preparation method, the blue light perovskite luminescent material includes a cesium lead bromine perovskite material, and the cesium lead bromine perovskite material is a nanosheet structure.

[0021] Among them, the average lateral size of the nanosheet structure is 23±5nm, and the average thickness of the nanosheet structure is 2.0±0.3nm.

[0022] The present invention also includes a technical solution of the third aspect, a light emitting diode, including a perovskite light emitting layer, and the perovskite light emitting layer includes the above-mentioned blue light perovskite light emitting material.

[0023] It also includes, from bottom to top, a substrate, an anode, a hole injection layer, a hole transport layer, an interface modification layer, an electron transport layer, and a cathode. The perovskite light-emitting layer is located between the interface modification layer and the electron transport layer.

[0024] The anode includes ITO conductive glass, and the thickness of the ITO film is 100-150nm.

[0025] The hole injection layer includes poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid), and the thickness of the hole injection layer is 30 nm to 40 nm.

[0026] The hole transport layer includes poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], and the thickness of the hole transport layer is 30 nm to 35 nm.

[0027] The interface modification layer comprises phenethylammonium bromide, and the thickness of the interface modification layer is 15nm to 25nm.

[0028] The perovskite light-emitting layer includes a nanosheet solution, and the thickness of the perovskite light-emitting layer is 40nm to 50nm.

[0029] The electron transport layer includes 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl) (TPBi), and the thickness of the electron transport layer is 35 nm to 40 nm.

[0030] The cathode comprises Al, and the thickness of the cathode (8) is at least 100 nm.

[0031] The cathode further includes a modified film layer of LiF with a thickness of 1 nm.

[0032] The present invention also includes a technical solution of a fourth aspect, a method for preparing a light emitting diode, comprising:

[0033] Dispersing the blue light perovskite luminescent material prepared by the above preparation method in n-octane or n-hexane to obtain a blue light perovskite luminescent material solution, wherein the concentration of the blue light perovskite luminescent material solution is 10-12 mg / mL;

[0034] A blue light perovskite luminescent material solution is coated on the bottom film layer to obtain a light emitting diode, wherein:

[0035] The bottom film layer comprises a substrate, an anode, a hole injection layer, a hole transport layer and an interface modification layer which are arranged in sequence.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] (1) The preparation method of the blue light perovskite luminescent material of the present invention adds 4-bromothiophene-2-carboxaldehyde (BTC) in the process of preparing the perovskite luminescent material, and provides stronger steric hindrance through its unique thiophene group to guide the two-dimensional growth of nanosheets, adjust their crystal growth dynamics, and effectively improve the crystallinity of perovskite. BTC has a highly electronegative carbonyl group, which can passivate the uncoordinated lead ions on the surface of the perovskite. The bromine atoms in BTC can further improve the binding ability of the ligand with the surface of the nanosheet, ensure its structural stability, reduce the probability of exciton quenching and non-radiative recombination of carriers in the device light-emitting layer, improve the stability of the spectrum, and enhance the brightness and external quantum efficiency of the light-emitting diode, thereby improving the luminescence performance.

[0038] (2) The method for preparing the blue light perovskite luminescent material of the present invention, by adding a toluene solution containing butylamine when purifying the nanosheets, curbs the destruction of the nanosheets by the polar solvent, prevents the agglomeration of the nanosheets, and reduces the attenuation of the fluorescence quantum yield during the purification process.

[0039] (3) The present invention includes the blue light perovskite luminescent material prepared as above, which has a stable spectrum and an external quantum efficiency as high as 5.44%. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1a This is a high-resolution transmission electron microscope image of a blue light perovskite luminescent material prepared by the present invention;

[0041] Figure 1b This is another high-resolution transmission electron microscope image of the blue light perovskite luminescent material prepared by the present invention;

[0042] Figure 2 The fluorescence spectrum and ultraviolet-visible light absorption spectrum of the blue light perovskite luminescent material prepared by the comparative example and the implementation of the present invention;

[0043] Figure 3 is an electroluminescence spectrum diagram of a blue light perovskite luminescent material under different voltages;

[0044] Figure 4 It is the electroluminescence spectrum diagram of the blue light perovskite luminescent material prepared by the present invention under different voltages;

[0045] Figure 5 It is a current density-voltage-brightness diagram of the blue light perovskite luminescent material prepared in the comparative example and the present invention;

[0046] Figure 6 It is a current density-EQE diagram of the blue light perovskite luminescent material prepared in comparative example and the present invention. DETAILED DESCRIPTION

[0047] The present invention is further described in detail below with reference to the accompanying drawings and embodiments.

[0048] A method for preparing a blue light perovskite luminescent material, comprising:

[0049] Lead bromide (PbBr2), oleic acid (OA), oleylamine (OLA), didodecyl dimethyl ammonium bromide (DDAB), and 4-bromothiophene-2-carboxaldehyde (BTC) are added to 1-octadecene (ODE), and stirred at 120-130° C. to obtain a lead precursor solution;

[0050] Cesium carbonate (Cs2CO3) and oleic acid (OA) are stirred at 90-110° C. to obtain a cesium precursor solution;

[0051] The cesium precursor solution is added to the lead precursor solution, isopropanol is injected, the mixed solution is heated to 70-80°C, and after keeping warm for a period of time, the mixed solution is transferred to an ice water bath, toluene is injected to obtain a crude nanosheet solution, and the blue light-emitting material is obtained by purification. The blue light-emitting material includes a nanosheet-shaped cesium lead bromine perovskite material passivated with 4-bromothiophene-2-carboxaldehyde.

[0052] The molar ratio of lead bromide, 4-bromothiophene-2-carboxaldehyde and didodecanedimethylammonium bromide is 4:(2.5-4):1.

[0053] Wherein, in the preparation of the lead precursor solution, the volume ratio of 1-octadecene, oleic acid and oleylamine is 8:1:1.

[0054] Among them, Cs in the cesium precursor solution +The molar concentration is 0.1~0.2mmol / mL.

[0055] After keeping warm for a period of time, the mixed solution is transferred to an ice water bath, the keeping warm time is 10 min to 12 min, and the ice water bath time is 3 min to 5 min.

[0056] Wherein, the volume ratio of toluene to the mixed solution is (2-3):1.

[0057] The purification process includes: adding a first polar solvent to a crude solution of nanosheets, performing a first centrifugal treatment, and obtaining a first precipitate; dissolving the first precipitate in a first organic solvent, adding a second organic solvent containing butylamine and a second polar solvent, and performing a second centrifugal treatment to obtain a second precipitate, wherein the second precipitate includes nanosheet-shaped cesium lead bromine perovskite material.

[0058] Wherein, the first polar solvent includes methyl acetate; and the volume ratio of the crude nanosheet solution to the polar solvent is 1:3.

[0059] The centrifuge speed for the first centrifugal treatment is 4000-5000 rpm, and the centrifugal treatment time is 5-10 minutes.

[0060] The first organic solvent includes n-hexane; the second organic solvent includes toluene, and the mass concentration of the second organic solvent containing butylamine is 10%.

[0061] The volume ratio of the first organic solvent, the second polar solvent and the second organic solvent containing butylamine in the first precipitate is 1:1:(0.001-0.005).

[0062] The second centrifugal treatment has a centrifuge speed of 7000-6000 rpm and a time of 3 minutes.

[0063] The present invention also includes a technical solution of the second aspect, a blue light perovskite luminescent material prepared by the above-mentioned preparation method, the blue light perovskite luminescent material includes a cesium lead bromine perovskite material, the cesium lead bromine perovskite material is a nanosheet structure, the average lateral size of the nanosheet is 23±5nm, and the average thickness is 2.0±0.3nm.

[0064] The present invention also includes a technical solution of the third aspect, a light emitting diode, including a perovskite light emitting layer, and the perovskite light emitting layer includes the above-mentioned blue light perovskite light emitting material.

[0065] It also includes, from bottom to top, a substrate, an anode, a hole injection layer, a hole transport layer, an interface modification layer, an electron transport layer, and a cathode. The perovskite light-emitting layer is located between the interface modification layer and the electron transport layer.

[0066] The anode includes ITO conductive glass, and the thickness of the ITO film is 100-150nm.

[0067] The hole injection layer includes poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid), and the thickness of the hole injection layer is 30 nm to 40 nm.

[0068] The hole transport layer includes poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], and the thickness of the hole transport layer is 30 nm to 35 nm.

[0069] The interface modification layer comprises phenethylammonium bromide, and the thickness of the interface modification layer is 15nm to 25nm.

[0070] The perovskite light-emitting layer includes a nanosheet solution, and the thickness of the perovskite light-emitting layer is 40nm to 50nm.

[0071] The electron transport layer includes 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl) (TPBi), and the thickness of the electron transport layer is 35 nm to 40 nm.

[0072] The cathode comprises Al, and the thickness of the cathode (8) is at least 100 nm.

[0073] The cathode further includes a modified film layer of LiF with a thickness of 1 nm.

[0074] The present invention also includes a technical solution of a fourth aspect, a method for preparing a light emitting diode, comprising:

[0075] Dispersing the blue light perovskite luminescent material prepared by the above preparation method in n-octane or n-hexane to obtain a blue light perovskite luminescent material solution, wherein the concentration of the blue light perovskite luminescent material solution is 10-12 mg / mL;

[0076] A blue light perovskite luminescent material solution is coated on the bottom film layer to obtain a light emitting diode, wherein:

[0077] The bottom film layer comprises a substrate, an anode, a hole injection layer, a hole transport layer and an interface modification layer which are arranged in sequence.

[0078] For ease of understanding, the present invention provides the following specific embodiments.

[0079] Comparative Example 1

[0080] 1. Prepare blue light perovskite luminescent materials and their solutions.

[0081] a). Add 0.073 g of PbBr2 and 0.012 g of DDAB into a beaker containing 4 mL of L ODE and stir. After heating to 120°C, add 0.5 mL of OA and OLA respectively until the solution becomes clear and transparent to obtain a lead precursor solution for later use.

[0082] b). Add 0.325 g of Cs2CO3 into a beaker containing 10 mL of OA, heat and stir at 100°C until the solution becomes clear and transparent to obtain a cesium precursor solution for later use.

[0083] c) At room temperature, add 0.5 mL of cesium precursor solution to the lead precursor solution, and inject 0.5 mL of isopropanol after 10 seconds. Stir for 1 minute and heat to 70°C.

[0084] d) When the solution temperature reaches 70°C, keep it warm for 10 minutes, transfer it to an ice water bath, inject 12 mL of toluene, cool and stir for 3 minutes to obtain a mixed solution.

[0085] e) Pour the mixed solution into a centrifuge tube, add 64 mL of methyl acetate, and centrifuge at 4000

[0086] Centrifuge at rpm for 5 min to obtain the first precipitate.

[0087] f). The first precipitate was dissolved in 4 mL of n-hexane, an equal volume of methyl acetate and 40 μL of a toluene solution containing butylamine were added, and the mixture was centrifuged at 7000 rpm for 3 min to obtain a second precipitate, which included the nanosheet-shaped cesium lead bromide perovskite material.

[0088] g). Disperse the precipitate in n-octane to obtain a blue light perovskite luminescent material solution with a concentration of 10 mg / mL.

[0089] 2. Preparation of Perovskite Light Emitting Diodes

[0090] a). Cleaning of the glass substrate containing the ITO transparent electrode, i.e., the anode: Wipe the ITO glass substrate with a dust-free cloth moistened with detergent, and then successively perform ultrasonic cleaning with deionized water, acetone, and isopropanol for 15 minutes each, dry the glass substrate, and treat it with oxygen plasma gas for 15 minutes.

[0091] b) Preparation of hole injection layer: 150 μL of poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution was spin-coated onto ITO at a speed of 4000 rpm for 40 seconds, and annealed at 150° C. for 15 minutes.

[0092] c) Preparation of hole transport layer: Take 120 μL of 6 mg / mL poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] chlorobenzene solution, spin coat it on the hole injection layer at 4000 rpm for 40 s, and anneal at 120°C for 20 min.

[0093] d). Preparation of interface modification layer: Take 150 μL of DMF solution with a concentration of 10 mg / mL phenethylammonium bromide, spin-coat it onto the hole transport layer at 5000 rpm for 30 s, and anneal it at 80° C. for 10 min.

[0094] e) Preparation of perovskite light-emitting layer: Take the blue light perovskite light-emitting material solution prepared in step 1, and spin-coat it onto the interface modification layer at 2000 rpm for 40 seconds.

[0095] f) Preparation of electron transport layer: Transfer the substrate to a vacuum coating machine. TPBi was deposited at an evaporation rate of 1.0 to a thickness of 40 nm.

[0096] g). Preparation of electrode modification layer: LiF was deposited at an evaporation rate of 1 nm thick.

[0097] h). Preparation of cathode: The Al electrode was deposited at an evaporation rate of 100 nm in thickness.

[0098] 3. Experimental test analysis

[0099] The device performance test of the perovskite light-emitting diode of comparative example 1 was carried out. Figure 2 The optical properties of the sample without BTC are shown (green curve), and its photoluminescence peak is 463nm. Its electroluminescence spectrum changes with increasing voltage as shown in Figure 3 As shown in Figure 2, as the voltage increases, a shoulder peak appears at 480nm, indicating that the blue light perovskite luminescent material of Comparative Example 1 is unstable and agglomerated. The current density-voltage-brightness curve is shown in Figure 2. Figure 5 As shown in the curve of “Nanosheets without BTC”, the maximum brightness of the sample without BTC is 56 cd m -2 The external quantum efficiency-current density curve of the sample is as follows Figure 6 As shown in the curve of "Nanosheets without BTC", its maximum external quantum efficiency reaches 1.29%. Specific parameters are shown in Table 1.

[0100] Example 1

[0101] 1. Prepare blue light perovskite luminescent materials and their solutions.

[0102] a). Add 0.073 g of PbBr2, 0.033 g of BTC, and 0.023 g of DDAB (corresponding to a molar ratio of 4:3.4:1) to a beaker containing 4 mL of ODE and stir. After heating to 120°C, add 0.5 mL of OA and OLA respectively until the solution is clear and transparent to obtain a lead precursor solution for standby use.

[0103] b). Add 0.325 g of Cs2CO3 into a beaker containing 10 mL of OA, heat and stir at 100°C until the solution becomes clear and transparent to obtain a cesium precursor solution for later use.

[0104] c) At room temperature, add 0.5 mL of cesium precursor solution to the lead precursor solution, and inject 0.5 mL of isopropanol after 10 seconds. Stir for 1 minute and heat to 70°C.

[0105] d). When the solution temperature reaches 70°C, keep it warm for 10 minutes, then quickly transfer it to an ice water bath, inject 12 mL of toluene, and cool and stir for 3 minutes.

[0106] e) Pour the mixed solution into a centrifuge tube, add 64 mL of methyl acetate, and centrifuge at 4000

[0107] Centrifuge at rpm for 5 min to obtain the first precipitate.

[0108] f). The first precipitate was dissolved in 4 mL of n-hexane, an equal volume of methyl acetate and 40 μL of a toluene solution containing butylamine were added, and the mixture was centrifuged at 7000 rpm for 3 min to obtain a second precipitate. The second precipitate includes the nanosheet-shaped cesium lead bromine perovskite material.

[0109] g). Disperse the precipitate in n-octane to obtain a blue light perovskite luminescent material solution with a concentration of 10 mg / mL.

[0110] 2. Preparation of Perovskite Light Emitting Diodes

[0111] a). Cleaning of the glass substrate containing the ITO transparent electrode, i.e., the anode: Wipe the ITO glass substrate with a dust-free cloth moistened with detergent, and then successively perform ultrasonic cleaning with deionized water, acetone, and isopropanol for 15 minutes each, dry the glass substrate, and treat it with oxygen plasma gas for 15 minutes.

[0112] b) Preparation of hole injection layer: Take 150 μL poly (3,4-ethylenedioxythiophene) - poly (styrene sulfonic acid)

[0113] The aqueous solution was spin-coated onto ITO at a speed of 4000 rpm for 40 s and then heated at 150 °C.

[0114] Anneal for 15 minutes.

[0115] c) Preparation of hole transport layer: Take 120 μL of 6 mg / mL poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] chlorobenzene solution, spin coat it on the hole injection layer at 4000 rpm for 40 s, and anneal at 120°C for 20 min.

[0116] d) Preparation of interface modification layer: Take 150 μL of DMF solution with a concentration of 10 mg / mL phenethylammonium bromide, spin-coat it on the hole transport layer at 5000 rpm for 30 seconds, and then spin-coat it at 80°C.

[0117] Anneal for 10 minutes.

[0118] e) Preparation of perovskite light-emitting layer: Take the blue light perovskite light-emitting material solution prepared in step 1, spin-coat it onto the interface modification layer at 2000 rpm for 40 seconds;

[0119] f) Preparation of electron transport layer: Transfer the substrate to a vacuum coating machine. TPBi was deposited at an evaporation rate of 1.0 to a thickness of 40 nm.

[0120] g). Preparation of electrode modification layer: LiF was deposited at an evaporation rate of 1 nm thick.

[0121] h). Preparation of cathode: The Al electrode was deposited at an evaporation rate of 100 nm in thickness.

[0122] 3. Experimental test analysis

[0123] The device performance test of the blue light emitting diode based on the perovskite nanosheet of this embodiment was carried out. Figure 1a and Figure 1b This is a high-resolution transmission electron microscope image of cesium lead bromine perovskite material containing BTC, showing that it has a lamellar structure and exhibits high crystallinity. The lattice spacing of 0.41nm corresponds to the (110) plane of the orthorhombic phase CsPbBr3 perovskite. Figure 2 The optical properties of the sample containing BTC are shown (blue curve), with a photoluminescence peak of 463nm and a half-peak width of 17nm, which is narrower than that of the sample without BTC. For the cesium lead bromide perovskite material passivated with 4-bromothiophene-2-carboxaldehyde, the electroluminescence spectrum is shown in Figure 4 As shown in Figure 1, as the voltage increases, the luminescence peak does not move significantly. The current density-voltage-brightness curve is shown in Figure 1. Figure 5 As shown, the maximum brightness of the sample containing BTC reaches 227cdm -2 , is the maximum brightness of the sample without BTC (56 cd m -2 ) is nearly 4 times. The external quantum efficiency-current density curve of this sample is shown in Figure 6 As shown in Table 1, the maximum external quantum efficiency of the sample containing BTC reaches 5.44%, which is nearly 5 times the maximum external quantum efficiency of the sample without BTC (1.29%). Specific performance parameters are shown in Table 1.

[0124] Example 2

[0125] 1. Prepare blue light perovskite luminescent materials and their solutions.

[0126] a). Add 0.073g of PbBr2, 0.033g of BTC, and 0.023g of DDAB (corresponding to a molar ratio of 4:3.4:1) to a beaker containing 4mL of LODE and stir, then heat to 120°C.

[0127] Then, 0.5 mL of OA and OLA were added in sequence until the solution became clear and transparent to obtain a lead precursor solution for later use.

[0128] b). Add 0.325 g of Cs2CO3 into a beaker containing 10 mL of OA, heat and stir at 100°C until the solution becomes clear and transparent to obtain a cesium precursor solution for later use.

[0129] c) At room temperature, add 0.5 mL of cesium precursor solution to the lead precursor solution, and inject 0.5 mL of isopropanol after 10 seconds. Stir for 1 minute and heat to 75°C.

[0130] d). When the solution temperature reaches 75°C, keep it warm for 10 minutes, then quickly transfer it to an ice water bath, inject 12 mL of toluene, and cool and stir for 3 minutes.

[0131] e) Pour the mixed solution into a centrifuge tube, add 64 mL of methyl acetate, and centrifuge at 4000

[0132] Centrifuge at rpm for 5 min to obtain the first precipitate.

[0133] f). The first precipitate was dissolved in 4 mL of n-hexane, an equal volume of methyl acetate and 40 μL of a toluene solution containing butylamine were added, and the mixture was centrifuged at 7000 rpm for 3 min to obtain a second precipitate. The second precipitate includes the nanosheet-shaped cesium lead bromine perovskite material.

[0134] g). Disperse the precipitate in n-octane to obtain a blue light perovskite luminescent material solution with a concentration of 10 mg / mL.

[0135] 2. Preparation of Perovskite Light Emitting Diodes

[0136] a). Cleaning of the glass substrate containing the ITO transparent electrode, i.e., the anode: Wipe the ITO glass substrate with a dust-free cloth moistened with detergent, and then successively perform ultrasonic cleaning with deionized water, acetone, and isopropanol for 15 minutes each, dry the glass substrate, and treat it with oxygen plasma gas for 15 minutes.

[0137] b) Preparation of hole injection layer: 150 μL of poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution was spin-coated onto ITO at a speed of 4000 rpm for 40 seconds, and annealed at 150° C. for 15 minutes.

[0138] c) Preparation of hole transport layer: Take 120 μL of 6 mg / mL poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] chlorobenzene solution, spin coat it on the hole injection layer at 4000 rpm for 40 s, and anneal at 120°C for 20 min.

[0139] d) Preparation of interface modification layer: Take 150 μL of DMF solution with a concentration of 10 mg / mL phenethylammonium bromide, spin-coat it on the hole transport layer at 5000 rpm for 30 seconds, and then spin-coat it at 80°C.

[0140] Anneal for 10 minutes.

[0141] e) Preparation of perovskite light-emitting layer: Take the blue light perovskite light-emitting material solution prepared in step 1, spin-coat it onto the interface modification layer at 2000 rpm for 40 seconds;

[0142] f) Preparation of electron transport layer: Transfer the substrate to a vacuum coating machine. TPBi was deposited at an evaporation rate of 1.0 to a thickness of 40 nm.

[0143] g). Preparation of electrode modification layer: LiF was deposited at an evaporation rate of 1 nm thick.

[0144] h). Preparation of cathode: The Al electrode was deposited at an evaporation rate of 100 nm in thickness.

[0145] 3. Experimental test analysis

[0146] The device performance test of the blue light emitting diode based on the perovskite nanosheet of this embodiment is carried out, and the various performances are shown in Table 1. Compared with Comparative Example 1, the holding temperature of this embodiment is adjusted to 75°C. Increasing the holding temperature can effectively improve the crystallinity of the nanosheet, ensure that the peak position of the device is stable and does not move during operation, so as to prepare a blue light emitting diode with stable spectrum.

[0147] Example 3

[0148] 1. Prepare blue light perovskite luminescent materials and their solutions.

[0149] a). Add 0.073g of PbBr2, 0.033g of BTC, and 0.023g of DDAB (corresponding to a molar ratio of 4:3.4:1) to a beaker containing 4mL of LODE and stir, then heat to 120°C.

[0150] Then, 0.5 mL of OA and OLA were added in sequence until the solution became clear and transparent to obtain a lead precursor solution for later use.

[0151] b). Add 0.325 g of Cs2CO3 into a beaker containing 10 mL of OA, heat and stir at 100°C until the solution becomes clear and transparent to obtain a cesium precursor solution for later use.

[0152] c). At room temperature, add 0.5 mL of cesium precursor solution to the lead precursor solution, inject 0.5 mL of isopropanol after 10 seconds, stir for 1 minute, and heat to 80°C.

[0153] d). When the solution temperature reaches 80°C, keep it warm for 10 minutes, then quickly transfer it to an ice water bath, inject 12 mL of toluene, and cool and stir for 3 minutes.

[0154] e) Pour the mixed solution into a centrifuge tube, add 64 mL of methyl acetate, and centrifuge at 4000

[0155] Centrifuge at rpm for 5 min to obtain the first precipitate.

[0156] f). The first precipitate was dissolved in 4 mL of n-hexane, an equal volume of methyl acetate and 40 μL of a toluene solution containing butylamine were added, and the mixture was centrifuged at 7000 rpm for 3 min to obtain a second precipitate. The second precipitate includes the nanosheet-shaped cesium lead bromine perovskite material.

[0157] g). Disperse the precipitate in n-octane to obtain a blue light perovskite luminescent material solution with a concentration of 10 mg / mL.

[0158] 2. Preparation of perovskite light-emitting diodes

[0159] a). Cleaning of the glass substrate containing the ITO transparent electrode, i.e., the anode: Wipe the ITO glass substrate with a dust-free cloth moistened with detergent, and then successively perform ultrasonic cleaning with deionized water, acetone, and isopropanol for 15 minutes each, dry the glass substrate, and treat it with oxygen plasma gas for 15 minutes.

[0160] b) Preparation of hole injection layer: 150 μL of poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution was spin-coated onto ITO at a speed of 4000 rpm for 40 seconds, and annealed at 150° C. for 15 minutes.

[0161] c) Preparation of hole transport layer: Take 120 μL of 6 mg / mL poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] chlorobenzene solution, spin coat it on the hole injection layer at 4000 rpm for 40 s, and anneal at 120°C for 20 min.

[0162] d). Preparation of interface modification layer: Take 150 μL of DMF solution with a concentration of 10 mg / mL phenethylammonium bromide, spin-coat it onto the hole transport layer at 5000 rpm for 30 s, and anneal it at 80° C. for 10 min.

[0163] e) Preparation of perovskite light-emitting layer: Take the blue light perovskite light-emitting material solution prepared in step 1, spin-coat it onto the interface modification layer at 2000 rpm for 40 seconds;

[0164] f) Preparation of electron transport layer: Transfer the substrate to a vacuum coating machine. TPBi was deposited at an evaporation rate of 1.0 to a thickness of 40 nm.

[0165] g). Preparation of electrode modification layer: LiF was deposited at an evaporation rate of 1 nm thick.

[0166] h). Preparation of cathode: The Al electrode was deposited at an evaporation rate of 100 nm in thickness.

[0167] 3. Experimental test analysis

[0168] The device performance test of the blue light emitting diode based on the perovskite nanosheet of this embodiment is carried out, and the various performances are shown in Table 1. Compared with Comparative Example 1, the insulation temperature of this embodiment is adjusted to 80°C. Increasing the insulation temperature can effectively improve the crystallinity of the nanosheet and improve the stability of the device during operation. In addition, the increase in temperature will cause the thickness of the nanosheet to increase, resulting in the phenomenon of red shift of the luminescence peak. In this embodiment, the luminescence peak of the device is slightly red shifted compared with Comparative Example 1.

[0169] Example 4

[0170] 1. Prepare blue light perovskite luminescent materials and their solutions.

[0171] a). Add 0.073g of PbBr2, 0.025g of BTC, and 0.023g of DDAB (corresponding to a molar ratio of 4:2.5:1) to a beaker containing 4mL of LODE and stir, then heat to 120°C.

[0172] Then, 0.5 mL of OA and OLA were added in sequence until the solution became clear and transparent to obtain a lead precursor solution for later use.

[0173] b). Add 0.325 g of Cs2CO3 into a beaker containing 10 mL of OA, heat and stir at 100°C until the solution becomes clear and transparent to obtain a cesium precursor solution for later use.

[0174] c) At room temperature, add 0.5 mL of cesium precursor solution to the lead precursor solution, and inject 0.5 mL of isopropanol after 10 seconds. Stir for 1 minute and heat to 75°C.

[0175] d). When the solution temperature reaches 75°C, keep it warm for 10 minutes, then quickly transfer it to an ice water bath, inject 12 mL of toluene, and cool and stir for 3 minutes.

[0176] e) Pour the mixed solution into a centrifuge tube, add 64 mL of methyl acetate, and centrifuge at 4000

[0177] Centrifuge at rpm for 5 min to obtain the first precipitate.

[0178] f). The first precipitate was dissolved in 4 mL of n-hexane, an equal volume of methyl acetate and 40 μL of a toluene solution containing butylamine were added, and the mixture was centrifuged at 7000 rpm for 3 min to obtain a second precipitate. The second precipitate includes the nanosheet-shaped cesium lead bromine perovskite material.

[0179] g). Disperse the precipitate in n-octane to obtain a blue light perovskite luminescent material solution with a concentration of 10 mg / mL.

[0180] 2. Preparation of Perovskite Light Emitting Diodes

[0181] a). Cleaning of the glass substrate containing the ITO transparent electrode, i.e., the anode: Wipe the ITO glass substrate with a dust-free cloth moistened with detergent, and then successively perform ultrasonic cleaning with deionized water, acetone, and isopropanol for 15 minutes each, dry the glass substrate, and treat it with oxygen plasma gas for 15 minutes.

[0182] b) Preparation of hole injection layer: 150 μL of poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution was spin-coated onto ITO at a speed of 4000 rpm for 40 seconds, and annealed at 150° C. for 15 minutes.

[0183] c) Preparation of hole transport layer: Take 120 μL of 6 mg / mL poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] chlorobenzene solution, spin coat it on the hole injection layer at 4000 rpm for 40 s, and anneal at 120°C for 20 min.

[0184] d) Preparation of interface modification layer: Take 150 μL of DMF solution with a concentration of 10 mg / mL phenethylammonium bromide, spin-coat it on the hole transport layer at 5000 rpm for 30 seconds, and then spin-coat it at 80°C.

[0185] Anneal for 10 minutes.

[0186] e) Preparation of perovskite light-emitting layer: Take the blue light perovskite light-emitting material solution prepared in step 1, spin-coat it onto the interface modification layer at 2000 rpm for 40 seconds;

[0187] f) Preparation of electron transport layer: Transfer the substrate to a vacuum coating machine. TPBi was deposited at an evaporation rate of 1.0 to a thickness of 40 nm.

[0188] g). Preparation of electrode modification layer: LiF was deposited at an evaporation rate of 1 nm thick.

[0189] h). Preparation of cathode: The Al electrode was deposited at an evaporation rate of 100 nm in thickness.

[0190] 3. Experimental test analysis

[0191] The device performance test of the blue light emitting diode based on the perovskite nanosheet of this embodiment is carried out, and the various performances are shown in Table 1. Compared with Comparative Example 1, the BTC dosage (0.025 g) is adjusted in this embodiment. Compared with Comparative Example 1, the maximum EQE and brightness of the prepared light emitting diode are improved by adding BTC in this embodiment, which proves that BTC can effectively passivate the surface defects of the nanosheets and enhance their radiative recombination.

[0192] Example 5

[0193] 1. Prepare blue light perovskite luminescent materials and their solutions.

[0194] a). Add 0.073 g of PbBr2, 0.036 g of BTC, and 0.023 g of DDAB (corresponding to a molar ratio of 4:3.6:1) to a beaker containing 4 mL of ODE and stir, then heat to 120 °C.

[0195] Then, 0.5 mL of OA and OLA were added in sequence until the solution became clear and transparent to obtain a lead precursor solution for later use.

[0196] b). Add 0.325 g of Cs2CO3 into a beaker containing 10 mL of OA, heat and stir at 100°C until the solution becomes clear and transparent to obtain a cesium precursor solution for later use.

[0197] c) At room temperature, add 0.5 mL of cesium precursor solution to the lead precursor solution, and inject 0.5 mL of isopropanol after 10 seconds. Stir for 1 minute and heat to 75°C.

[0198] d). When the solution temperature reaches 75°C, keep it warm for 10 minutes, then quickly transfer it to an ice water bath, inject 12 mL of toluene, and cool and stir for 3 minutes.

[0199] e) Pour the mixed solution into a centrifuge tube, add 64 mL of methyl acetate, and centrifuge at 4000

[0200] Centrifuge at rpm for 5 min to obtain the first precipitate.

[0201] f). The first precipitate was dissolved in 4 mL of n-hexane, an equal volume of methyl acetate and 40 μL of a toluene solution containing butylamine were added, and the mixture was centrifuged at 7000 rpm for 3 min to obtain a second precipitate. The second precipitate includes the nanosheet-shaped cesium lead bromine perovskite material.

[0202] g). Disperse the precipitate in n-octane to obtain a blue light perovskite luminescent material solution with a concentration of 10 mg / mL.

[0203] 2. Preparation of perovskite light-emitting diodes

[0204] a). Cleaning of the glass substrate containing the ITO transparent electrode, i.e., the anode: Wipe the ITO glass substrate with a dust-free cloth moistened with detergent, and then successively perform ultrasonic cleaning with deionized water, acetone, and isopropanol for 15 minutes each, dry the glass substrate, and treat it with oxygen plasma gas for 15 minutes.

[0205] b) Preparation of hole injection layer: 150 μL of poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) aqueous solution was spin-coated onto ITO at a speed of 4000 rpm for 40 seconds, and annealed at 150° C. for 15 minutes.

[0206] c) Preparation of hole transport layer: Take 120 μL of 6 mg / mL poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] chlorobenzene solution, spin coat it on the hole injection layer at 4000 rpm for 40 s, and anneal at 120°C for 20 min.

[0207] d). Preparation of interface modification layer: Take 150 μL of DMF solution with a concentration of 10 mg / mL phenethylammonium bromide, spin-coat it onto the hole transport layer at 5000 rpm for 30 s, and anneal it at 80° C. for 10 min.

[0208] e) Preparation of perovskite light-emitting layer: Take the blue light perovskite light-emitting material solution prepared in step 1, spin-coat it onto the interface modification layer at 2000 rpm for 40 seconds;

[0209] f) Preparation of electron transport layer: Transfer the substrate to a vacuum coating machine. TPBi was deposited at an evaporation rate of 1.0 to a thickness of 40 nm.

[0210] g). Preparation of electrode modification layer: LiF was deposited at an evaporation rate of 1 nm thick.

[0211] h). Preparation of cathode: The Al electrode was deposited at an evaporation rate of 100 nm in thickness.

[0212] 3. Experimental test analysis

[0213] The device performance test of the blue light emitting diode based on perovskite nanosheets of this embodiment was carried out, and various performances are shown in Table 1. Compared with Comparative Example 1, the BTC dosage in this embodiment was adjusted to 0.036g. Based on Examples 3-5, it is shown that the performance of the light emitting diode is improved by adding different amounts of BTC, indicating that BTC can effectively passivate the surface defects of the nanosheets and inhibit non-radiative recombination. At the same time, the addition of BTC can effectively control the growth dynamics of the nanosheets based on the coordination of aldehydes based on lead ions in the stage of synthesizing blue light-emitting materials, and ultimately achieve the regulation of the light-emitting peak position of the light-emitting diode. With the increase of BTC, the performance of the light-emitting diode shows a trend of first increasing and then decreasing.

[0214] Table 1. Performance parameters of light emitting diodes of various embodiments and comparative examples.

[0215]

[0216] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a blue light perovskite luminescent material, characterized in that: include: Add lead bromide, oleic acid, oleylamine, didodecyl dimethyl ammonium bromide, and 4-bromothiophene-2-carboxaldehyde to 1-octadecene, and stir at 120-130° C. to obtain a lead precursor solution; Cesium carbonate and oleic acid are stirred at 90-110° C. to obtain a cesium precursor solution; The cesium precursor solution is added to the lead precursor solution, isopropanol is injected, the mixed solution is heated to 70-80°C, and after keeping warm for a period of time, the mixed solution is transferred to an ice water bath, toluene is injected to obtain a crude nanosheet solution, and the blue light-emitting material is obtained by purification. The blue light-emitting material includes a nanosheet-shaped cesium lead bromine perovskite material passivated with 4-bromothiophene-2-carboxaldehyde.

2. The preparation method according to claim 1, characterized in that: The molar ratio of lead bromide, 4-bromothiophene-2-carboxaldehyde and didodecyl dimethyl ammonium bromide is 4:(2.5-4):1; and / or, In the preparation of the lead precursor solution, the volume ratio of 1-octadecene, oleic acid and oleylamine is 8:1:

1.

3. The preparation method according to claim 1, characterized in that: The cesium precursor solution contains Cs + The molar concentration is 0.1~0.2mmol / mL.

4. The preparation method according to claim 1, characterized in that: After the insulation period, the mixed solution is transferred to an ice water bath, wherein the insulation period is 10 to 12 minutes and the ice water bath period is 3 to 5 minutes; and / or, The volume ratio of the toluene to the mixed solution is (2-3):

1.

5. The preparation method according to claim 1, characterized in that: The purification process comprises: Adding a first polar solvent to the crude nanosheet solution, performing a first centrifugal treatment, and obtaining a first precipitate; The first precipitate is dissolved in a first organic solvent, a second organic solvent containing butylamine and a first polar solvent are added, and centrifugation is performed for a second time to obtain a second precipitate, wherein the second precipitate includes the nanosheet-shaped cesium lead bromine perovskite material.

6. The preparation method according to claim 5, characterized in that: The first polar solvent includes methyl acetate; the volume ratio of the crude nanosheet solution to the polar solvent is 1:3; the centrifuge speed of the first centrifugal treatment is 4000-5000 rpm, and the centrifugal treatment time is 5-10 minutes; The first polar solvent includes methyl acetate, the first organic solvent includes n-hexane; the second organic solvent includes toluene, and the mass concentration of the second organic solvent containing butylamine is 10%; The volume ratio of the first organic solvent, the first polar solvent, and the second organic solvent containing butylamine in the first precipitate is 1:1:(0.001-0.005); The centrifuge speed of the second centrifugal treatment is 6000-7000 rpm, and the time is 2-3 minutes.

7. A blue light perovskite luminescent material, characterized in that: The blue light perovskite luminescent material is prepared by the preparation method described in any one of claims 1 to 6, wherein the cesium lead bromine perovskite material comprises a cesium lead bromine perovskite material, and the cesium lead bromine perovskite material is a nanosheet structure; optionally, the average lateral size of the nanosheet structure is 18-28nm, and the average thickness of the nanosheet structure is 1.7-2.3nm.

8. A light emitting diode, characterized in that: It comprises a perovskite light-emitting layer (6), wherein the perovskite light-emitting layer (6) comprises the blue light perovskite light-emitting material according to claim 7.

9. The light emitting diode according to claim 8, characterized in that: It also includes, from bottom to top, a substrate, an anode, a hole injection layer, a hole transport layer, an interface modification layer, an electron transport layer, and a cathode, wherein the perovskite light-emitting layer is located between the interface modification layer and the electron transport layer; The anode includes ITO conductive glass, and the thickness of the ITO film is 100-150nm; The hole injection layer comprises poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid), and the thickness of the hole injection layer is 30nm to 40nm; The hole transport layer comprises poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], and the thickness of the hole transport layer is 30 nm to 35 nm; The interface modification layer comprises phenethylammonium bromide, and the thickness of the interface modification layer is 15nm to 25nm; The perovskite light-emitting layer comprises a nanosheet solution, and the thickness of the perovskite light-emitting layer is 40nm to 50nm. The electron transport layer includes 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl), and the thickness of the electron transport layer is 35nm to 40nm; The cathode comprises Al, and the thickness of the cathode (8) is at least 100 nm; the cathode also comprises a modified film layer of LiF with a thickness of 1 nm.

10. A method for preparing a light emitting diode, characterized in that: include: Dispersing the blue light perovskite luminescent material prepared by the preparation method according to any one of claims 1 to 6 in n-octane or n-hexane to obtain a blue light perovskite luminescent material solution, wherein the mass concentration of the blue light perovskite luminescent material solution is 10 to 12 mg / mL; The blue light perovskite luminescent material solution is coated on the bottom film layer to obtain the perovskite luminescent layer, wherein the bottom film layer includes a substrate, an anode, a hole injection layer, a hole transport layer and an interface modification layer arranged in sequence.

Citation Information

Patent Citations

  • Perovskite photoelectronic device with defect passivation

    CN114072923A

Cited By

  • Preparation method and application of blue-light CsPbBr3 perovskite quantum dots

    CN120966475A

  • Synthesis method of blue-light perovskite nanosheet based on monophenyl phosphate modification

    CN122465586A