Cs2NaYF6 luminescent material as well as preparation method and application thereof

Through a high-temperature solid-phase one-step synthesis method, the preparation process of Cs2NaYF6 and doped rare earth ions is simplified, solving the problems of complexity and high cost of traditional methods, and achieving stable synthesis and widespread application of the material.

CN118772884APending Publication Date: 2024-10-15JILIN UNIVERSITY

Patent Information

Application Number
CN202410741171.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The synthesis method of traditional Cs2NaYF6 fluorescent materials is complex and costly, making it difficult to achieve large-scale preparation and widespread application.

Method used

Using a high-temperature solid-phase one-step synthesis method, by adjusting the molar ratio of cesium source, sodium source, yttrium oxide and ammonium fluoride, a solid-phase reaction is performed to prepare Cs2NaYF6 and Cs2NaY1-xLnxF6 luminescent materials doped with rare earth ions, simplifying the process and reducing costs. .

Benefits of technology

It achieves the stable synthesis of Cs2NaYF6 and doped rare earth ions, reduces the difficulty and cost of operation, ensures the good luminescence performance of the material, and is suitable for the fields of laser technology, biomarkers and optoelectronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772884A_ABST
    Figure CN118772884A_ABST
Patent Text Reader

Abstract

The invention discloses a Cs2NaYF6 luminescent material as well as a preparation method and application thereof. The preparation method comprises the following steps: carrying out solid-phase reaction on a first mixed reaction system containing a cesium source, a sodium source, yttrium oxide and ammonium fluoride to prepare a Cs2NaYF6 luminescent material; wherein the molar ratio of the cesium source to the sodium source to the yttrium oxide to the ammonium fluoride is 2.2: 1: 1: 6. A high-temperature solid-phase method is adopted for one-step synthesis, the method is simple and easy to operate, the technical threshold is low, components are easy to control, the preparation cost is effectively reduced, the adverse effect of a NaF impure phase is successfully eliminated by adjusting the molar ratio of all reactants, meanwhile, the solid-phase high-temperature reaction is adopted, phase change from Cs3YF6 to Cs2NaYF6 in the crystal growth process is promoted, and the Cs2NaYF6-Cs3YF6-Cs2NaYF6-Cs3YF6-Cs2NaYF6-Cs3YF6- the defect that Cs3YF6 is generated due to inaccurate temperature regulation and control is avoided, so that the luminescent material with good luminescent property is finally and stably synthesized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of luminescent materials, and in particular relates to a Cs2NaYF6 luminescent material and a preparation method and application thereof. Background Art

[0002] Rare earth-doped fluorescent materials have a wide range of applications in lighting, display, and sensing. Among them, perovskite fluoride Cs2NaYF6 is an important fluorescent material with excellent fluorescence properties and can be widely used in laser technology, bio-labeling, and optoelectronic devices. However, traditional synthesis methods have problems such as complex operation, high technical requirements, and high costs, which limit the large-scale preparation and wide application of Cs2NaYF6 fluorescent materials.

[0003] For example, patent CN112625687A discloses a method for preparing a rare earth-doped Cs2NaYF6 nano-luminescent material, which uses cesium fluoride as a cesium source and uses a high-temperature coprecipitation method to prepare the rare earth-doped Cs2NaYF6 nano-luminescent material. For example, patent document CN117586765A discloses a luminescent nano-material and its preparation method and application in protein detection. The above patents are all prepared by high-temperature coprecipitation, which requires precise control of reaction conditions under a nitrogen flow environment, including manual control of reaction temperature, gas flow rate, etc., and the synthesis process has many steps, including the preparation of precursors, volatilization of reactants, high-temperature synthesis, etc., and the conditions are demanding, the operation is difficult, the process is cumbersome, the cost is high, the reaction cycle is long, and it is limited by the solubility of the three-necked flask, and large-scale batch production cannot be achieved. Therefore, it is necessary to provide a method for preparing rare earth-doped Cs2NaYF6 luminescent materials that is simple, easy to operate, has low technical barriers, and is cost-effective to meet the needs of large-scale preparation and ensure that the luminescent performance of the material is stable and superior. Summary of the invention

[0004] The main purpose of the present invention is to provide a Cs2NaYF6 luminescent material and a preparation method and application thereof, so as to overcome the deficiencies of the prior art.

[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0006] An embodiment of the present invention provides a method for preparing a Cs2NaYF6 luminescent material, which comprises: causing a first mixed reaction system comprising a cesium source, a sodium source, yttrium oxide and ammonium fluoride to undergo a solid phase reaction to obtain a Cs2NaYF6 luminescent material; wherein the molar ratio of the cesium source, the sodium source, the yttrium oxide and the ammonium fluoride is 2.2:1:1:6.

[0007] The embodiment of the present invention also provides a Cs2NaYF6 luminescent material prepared by the preparation method described in any one of claims 1-3.

[0008] The present invention also provides the above-mentioned preparation method for preparing Cs2NaY doped with rare earth ions. 1-x Ln x F6 luminescent material, wherein Ln is selected from Yb and / or Er, 0 <x<1。

[0009] The embodiment of the present invention also provides a Cs2NaY doped with rare earth ions. 1-x Ln x The method for preparing F6 luminescent material comprises: causing a second mixed reaction system comprising a cesium source, a sodium source, yttrium oxide, a rare earth oxide and ammonium fluoride to undergo a solid phase reaction to obtain Cs2NaY doped with rare earth ions 1-x Ln x F6 luminescent material; wherein the molar ratio of the cesium source, the sodium source, the yttrium oxide, the rare earth oxide and the ammonium fluoride is 2.2:1:1-x:x:6, Ln is selected from Yb and / or Er, 0 <x<1。

[0010] The embodiment of the present invention also provides Cs2NaY doped with rare earth ions prepared by the above-mentioned preparation method. 1-x Ln x F6 luminescent material.

[0011] The embodiment of the present invention also provides the aforementioned Cs2NaYF6 luminescent material or Cs2NaY 1-x Ln x The use of F6 luminescent materials in the fields of laser technology, bio-labeling or optoelectronic devices.

[0012] Compared with the prior art, the invention has the following beneficial effects: the invention adopts a high temperature solid phase one-step synthesis of Cs2NaYF6 luminescent material and Cs2NaY doped with rare earth ions 1-x Ln x F6 luminescent material is simple and easy to operate, has low technical threshold, and is easy to control in composition, which effectively reduces the preparation cost. By adjusting the molar ratio of each reactant, the Cs2NaYF6 or Cs2NaY 1- x Ln x The adverse effect of NaF impurity in the F6 generation process was promoted by solid-phase high-temperature reaction, which promoted the phase transition of Cs3YF6 to Cs2NaYF6 during the crystal growth process and avoided the disadvantage of inaccurate temperature control leading to the generation of Cs3YF6. As a result, the Cs2NaYF6 luminescent material with good luminescence performance and Cs2NaYF6 doped with rare earth ions were finally stably synthesized. 1-x Ln x F6 luminescent material. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0014] Figure 1 It is a flow chart of a simple preparation method for rare earth doped Cs2NaYF6 in a typical embodiment of the present invention;

[0015] Figure 2 It is the XRD (X-ray diffraction) diagram of Cs2NaYF6, Cs2NaYF6:6%Er, Cs2NaYF6:6%Er, 4%Yb and Cs2NaYF6 standard card prepared in Examples 1-3 of the present invention;

[0016] Figure 3a-Figure 3b is a SEM (scanning electron microscope) image of Cs2NaYF6 prepared in Example 1 of the present invention;

[0017] Figure 4 It is the XRD (X-ray diffraction) diagram of the sample prepared in Comparative Example 1 of the present invention and the NaF, Cs3YF6, Cs2NaYF6 standard cards;

[0018] Figure 5 It is the emission spectrum of Cs2NaYF6 doped with 6% Er and 4% Yb, 6% Er prepared in Examples 2 and 3 of the present invention in the visible light region (the excitation light source is a 980nm laser);

[0019] Figure 6 This is the emission spectrum of Cs2NaYF6 doped with 6% Er and 4% Yb, 6% Er prepared in Example 2-3 of the present invention in the near-infrared region (the excitation light source is a 980nm laser). DETAILED DESCRIPTION

[0020] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. It adopts a high-temperature solid-phase one-step synthesis of Cs2NaYF6, adjusts the molar ratio of each reactant, and eliminates the NaF impurity phase present in the Cs2NaYF6 generation process. Adjust the reaction temperature to avoid the disadvantage of generating Cs3YF6 due to inaccurate temperature control, so as to finally synthesize a rare earth-doped Cs2NaYF6 luminescent material with good luminescence performance in a stable manner. Reduce the dependence on environmental conditions and reaction equipment, reduce the difficulty of operation, simplify the process, and reduce costs, so as to meet both daily experimental needs and large-scale production.

[0021] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Specifically, as one aspect of the technical solution of the present invention, a method for preparing a Cs2NaYF6 luminescent material is involved, which includes: causing a first mixed reaction system containing a cesium source, a sodium source, yttrium oxide and ammonium fluoride to undergo a solid phase reaction to obtain a Cs2NaYF6 luminescent material; wherein the molar ratio of the cesium source, the sodium source, the yttrium oxide and the ammonium fluoride is 2.2:1:1:6.

[0023] In some preferred embodiments, the cesium source includes cesium carbonate, but is not limited thereto.

[0024] In some preferred embodiments, the sodium source includes sodium carbonate, but is not limited thereto.

[0025] In some preferred embodiments, the preparation method specifically includes: placing a cesium source, a sodium source, yttrium oxide and ammonium fluoride in a grinding device and grinding them in the same direction for 15-20 minutes, then performing a high-temperature solid-phase reaction at 700°C in an air atmosphere for 6 hours to obtain a Cs2NaYF6 luminescent material.

[0026] In some preferred embodiments, the preparation flow chart of the Cs2NaYF6 luminescent material is as follows: Figure 1 shown.

[0027] In some more specific embodiments, the method for preparing the Cs2NaYF6 luminescent material comprises:

[0028] (1) Raw material preparation

[0029] Cesium carbonate, sodium carbonate, yttrium oxide and ammonium fluoride were weighed in a molar ratio of 2.2:1:1:6. The weighed powders were mixed and placed in an agate mortar and ground in the same direction for 15-20 minutes until no blocky particles of ammonium fluoride were observed, mixed evenly and dried, and then placed in a crucible.

[0030] (2) High temperature furnace heating

[0031] Place the crucible in a high-temperature furnace and burn it at 700 degrees in air for 6 hours.

[0032] (3) Sample collection

[0033] After burning, the sample is cooled naturally to room temperature and then ground for 5-10 minutes until the blocky sintered material is fine powder.

[0034] The present invention discloses a simple preparation method of Cs2NaYF6 luminescent material, which adopts a high-temperature solid phase method to synthesize Cs2NaYF6 stably in one step, and can be divided into three processes: raw material preparation, high-temperature furnace heating, and sample collection. First, a certain amount of cesium carbonate, sodium carbonate, rare earth oxide and ammonium fluoride are fully ground, and the ground powder is placed in a crucible, and then placed in a high-temperature furnace and heated at a certain temperature to finally form Cs2NaYF6. Cs2NaYF6 doped with rare earth ions can be obtained by quantitatively mixing rare earth oxides in the reactants. 1-x Ln x F6, showing excellent luminous effect.

[0035] Another aspect of an embodiment of the present invention further provides a Cs2NaYF6 luminescent material prepared by the aforementioned preparation method.

[0036] Another aspect of the present invention provides the above-mentioned preparation method for preparing Cs2NaY doped with rare earth ions. 1-x Ln x F6 luminescent material, wherein Ln is selected from Yb and / or Er, 0 <x<1。

[0037] Another aspect of the embodiment of the present invention further provides a Cs2NaY doped with rare earth ions. 1-x Ln x The method for preparing F6 luminescent material comprises: causing a second mixed reaction system comprising a cesium source, a sodium source, yttrium oxide, a rare earth oxide and ammonium fluoride to undergo a solid phase reaction to obtain Cs2NaY doped with rare earth ions 1-x Ln x F6 luminescent material; wherein the molar ratio of the cesium source, the sodium source, the yttrium oxide, the rare earth oxide and the ammonium fluoride is 2.2:1:1-x:x:6, Ln is selected from Yb and / or Er, 0 <x<1。

[0038] In some preferred embodiments, the cesium source includes cesium carbonate, but is not limited thereto.

[0039] In some preferred embodiments, the sodium source includes sodium carbonate, but is not limited thereto.

[0040] In some preferred embodiments, the rare earth oxide includes Yb2O3 and / or Er2O3, but is not limited thereto.

[0041] In some preferred embodiments, the preparation method specifically comprises: placing a cesium source, a sodium source, yttrium oxide, a rare earth oxide and ammonium fluoride in a grinding device and grinding them in the same direction for 15-20 minutes, and then performing a high-temperature solid phase reaction at 700°C for 6 hours in an air atmosphere to obtain Cs2NaY doped with rare earth ions. 1-x Ln x F6 luminescent material.

[0042] In some more specific embodiments, Cs2NaY doped with rare earth ions 1-x Ln x The preparation method of F6 luminescent material comprises:

[0043] (1) Raw material preparation

[0044] Cesium carbonate, sodium carbonate, yttrium oxide, rare earth oxide and ammonium fluoride are weighed in a molar ratio of 2.2:1:1-x:x:6. The weighed powders are mixed and placed in an agate mortar and ground in the same direction for 15-20 minutes until no blocky particles of ammonium fluoride are observed, mixed evenly and dried, and then placed in a crucible.

[0045] (2) High temperature furnace heating

[0046] Place the crucible in a high-temperature furnace and burn it at 700 degrees in air for 6 hours.

[0047] (3) Sample collection

[0048] After burning, the sample is cooled naturally to room temperature and then ground for 5-10 minutes until the blocky sintered material is fine powder.

[0049] Another aspect of the embodiment of the present invention also provides Cs2NaY doped with rare earth ions prepared by the above preparation method. 1-x Ln x F6 luminescent material.

[0050] Another aspect of the embodiment of the present invention further provides the aforementioned Cs2NaYF6 luminescent material or Cs2NaYF6 doped with rare earth ions. 1-x Ln x The use of F6 luminescent materials in the fields of laser technology, bio-labeling or optoelectronic devices.

[0051] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0052] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0053] Example 1

[0054] Preparation of 1 mmol Cs2NaYF6:

[0055] (1) Raw material preparation

[0056] Weigh 0.3584g of cesium carbonate, 0.0530g of sodium carbonate, 0.1129g of yttrium oxide and 0.2222g of ammonium fluoride, mix the weighed powders in an agate mortar and grind them in the same direction for 15-20 minutes, mix them evenly and dry them, and then put them in a crucible.

[0057] (2) High temperature furnace heating

[0058] Place the crucible in a high-temperature furnace and burn it at 700 degrees in air for 6 hours.

[0059] (3) Sample collection

[0060] After burning, the sample is naturally cooled to room temperature and then ground for 5-10 minutes until the blocky sintered material becomes fine powder to obtain Cs2NaYF6.

[0061] The XRD patterns of Cs2NaYF6 and Cs2NaYF6 standard cards prepared in this example are as follows: Figure 2 As shown, the SEM (scanning electron microscope) image of the prepared Cs2NaYF6 is as follows Figure 3a-Figure 3b shown.

[0062] Example 2

[0063] Preparation of 1 mmol Cs2NaYF6 doped with 6% Er:

[0064] (1) Raw material preparation

[0065] Weigh 0.3584g of cesium carbonate, 0.0530g of sodium carbonate, 0.1061g of yttrium oxide, 0.0115g of erbium oxide and 0.2222g of ammonium fluoride, mix the weighed powders in an agate mortar and grind them in the same direction for 15-20 minutes, mix them evenly, dry them, and then put them in a crucible.

[0066] (2) High temperature furnace heating

[0067] Place the crucible in a high-temperature furnace and burn it at 700 degrees in air for 6 hours.

[0068] (3) Sample collection

[0069] After burning, the sample is naturally cooled to room temperature and then ground for 5-10 minutes until the block sintered material is fine powder, so that Cs2NaY 1-x Ln x F6 is Cs2NaYF6 doped with 6% Er.

[0070] Example 3

[0071] Preparation of 1 mmol Cs2NaYF6 doped with 4% Yb and 6% Er:

[0072] (1) Raw material preparation

[0073] Weigh 0.3584g of cesium carbonate, 0.0530g of sodium carbonate, 0.1016g of yttrium oxide, 0.0115g of erbium oxide, 0.0079g of ytterbium oxide and 0.2222g of ammonium fluoride. Mix the weighed powders in an agate mortar and grind them in the same direction for 15-20 minutes, mix them evenly, dry them, and then put them in a crucible.

[0074] (2) High temperature furnace heating

[0075] Place the crucible in a high-temperature furnace and burn it at 700 degrees in air for 6 hours.

[0076] (3) Sample collection

[0077] After burning, the sample is naturally cooled to room temperature and then ground for 5-10 minutes until the block sintered material is fine powder, so that Cs2NaY 1-x Ln x F6 is Cs2NaYF6 doped with 4% Yb and 6% Er.

[0078] Figure 5 It is the emission spectrum of Cs2NaYF6 doped with 6% Er and 4% Yb, 6% Er prepared in Examples 2 and 3 of the present invention in the visible light region (the excitation light source is a 980nm laser); Figure 6 This is the emission spectrum of Cs2NaYF6 doped with 6% Er and 4% Yb, 6% Er prepared in Examples 2 and 3 of the present invention in the near-infrared region (the excitation light source is a 980nm laser).

[0079] Comparative Example 1

[0080] (1) Raw material preparation

[0081] Weigh 0.3584g of cesium carbonate, 0.0530g of sodium carbonate, 0.1129g of yttrium oxide and 0.2222g of ammonium fluoride, mix the weighed powders in an agate mortar and grind them in the same direction for 15-20 minutes, mix them evenly and dry them, and then put them in a crucible.

[0082] (2) High temperature furnace heating

[0083] Place the crucible in a high-temperature furnace and burn it at 600 degrees in air for 6 hours.

[0084] (3) Sample collection

[0085] After burning, the sample is naturally cooled to room temperature and then ground for 5-10 minutes until the blocky sintered material is fine powder.

[0086] The XRD patterns of the samples prepared in this comparative example and the standard cards of NaF, YF3, Cs3YF6, and Cs2NaYF6 are shown in Figure 4As shown in the comparative example 1 fired at 600 degrees for 6 hours, although Cs2NaYF6 exists, the main phase is Cs3YF6.

[0087] Comparative Example 2

[0088] 0.3258g of cesium carbonate, 0.0530g of sodium carbonate, 0.1129g of yttrium oxide and 0.2222g of ammonium fluoride were weighed. The molar ratio of cesium carbonate, sodium carbonate, yttrium oxide and ammonium fluoride was 2:1:1:6 (normal molar ratio). The weighed powders were mixed and placed in an agate mortar and ground in the same direction for 15-20 minutes, mixed evenly and dried, and then placed in a crucible.

[0089] (2) High temperature furnace heating

[0090] Place the crucible in a high-temperature furnace and burn it at 700 degrees in air for 6 hours.

[0091] (3) Sample collection

[0092] After burning, the sample is cooled naturally to room temperature and then ground for 5-10 minutes until the blocky sintered material is fine powder.

[0093] The XRD patterns of the samples prepared in this comparative example and the standard cards of NaF, YF3, Cs3YF6, and Cs2NaYF6 are shown in Figure 4 As shown in the figure, when the molar ratio of cesium carbonate, sodium carbonate, yttrium oxide and ammonium fluoride is 2:1:1:6, that is, the normal molar ratio, although the main phase is Cs2NaYF6, there is a YF3 impurity phase.

[0094] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0095] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.

Claims

1. A method for preparing a Cs2NaYF6 luminescent material, characterized in that: include: A first mixed reaction system comprising a cesium source, a sodium source, yttrium oxide and ammonium fluoride is subjected to a solid phase reaction to obtain a Cs2NaYF6 luminescent material; wherein the molar ratio of the cesium source, the sodium source, the yttrium oxide and the ammonium fluoride is 2.2:1:1:

6.

2. The preparation method according to claim 1, characterized in that: The cesium source includes cesium carbonate; And / or, the sodium source comprises sodium carbonate.

3. The preparation method according to claim 1, characterized in that: Specifically include: The cesium source, sodium source, yttrium oxide and ammonium fluoride were placed in a grinding device and ground in the same direction for 15-20 minutes, and then subjected to a high-temperature solid phase reaction at 700°C for 6 hours in an air atmosphere to obtain a Cs2NaYF6 luminescent material.

4. The Cs2NaYF6 luminescent material prepared by the preparation method described in any one of claims 1 to 3.

5. The method according to any one of claims 1 to 3 is used to prepare Cs2NaY doped with rare earth ions 1-x Use of LnxF6 luminescent materials, wherein Ln is selected from Yb and / or Er, 0 <x<1。 6. A rare earth ion doped Cs2NaY 1-x Ln x The preparation method of F6 luminescent material is characterized in that: include: A second mixed reaction system comprising a cesium source, a sodium source, yttrium oxide, a rare earth oxide and ammonium fluoride is subjected to a solid phase reaction to obtain Cs2NaY doped with rare earth ions. 1-x LnxF6 luminescent material; wherein the molar ratio of the cesium source, the sodium source, the yttrium oxide, the rare earth oxide and the ammonium fluoride is 2.2:1:1-x:x:6, Ln is selected from Yb and / or Er, 0 <x<1。 7. The preparation method according to claim 6, characterized in that: The cesium source includes cesium carbonate; and / or, the sodium source comprises sodium carbonate; And / or, the rare earth oxide includes Yb2O3 and / or Er2O3.

8. The preparation method according to claim 6, characterized in that: Specifically include: The cesium source, sodium source, yttrium oxide, rare earth oxide and ammonium fluoride were placed in a grinding device and ground in the same direction for 15-20 minutes, and then subjected to high-temperature solid-phase reaction at 700°C for 6 hours in an air atmosphere to obtain Cs2NaY doped with rare earth ions. 1-x Ln x F6 luminescent material.

9. Cs2NaY doped with rare earth ions prepared by the preparation method according to any one of claims 6 to 8 1-x Ln x F6 luminescent material.

10. The Cs2NaYF6 luminescent material according to claim 4 or the Cs2NaYF6 doped with rare earth ions according to claim 9 1- x Ln x The use of F6 luminescent materials in the fields of laser technology, bio-labeling or optoelectronic devices.

Citation Information

Patent Citations

  • Method for preventing severe volatilization during growth process of cesium triborate

    CN102108550A

  • Industrialized preparation method of tantalum-aluminum-codoped lithium-lanthanum zirconate solid-state electrolyte

    CN109052473A

  • NiO-doped CsPbCl1.5Br1.5 quantum dot microcrystalline glass and application thereof

    CN111217530A

  • Rare earth doped potassium cryolite nano luminescent material and preparation method thereof

    CN112625687A

  • Near-ultraviolet-excited wide-spectrum warm white light fluorescent material as well as preparation and application thereof

    CN118026245A

Cited By

  • Cs2KYF6 luminescent material, rare earth element-doped Cs2KYF6 luminescent material as well as preparation method and application of Cs2KYF6 luminescent material

    CN122146297A

  • A Cs2KYF6 luminescent material, a rare earth-doped Cs2KYF6 luminescent material, its preparation method and application

    CN122146297B