Sand inclusion side slope chemical curing material and construction process
By using chemical curing materials and processes on slopes in arid areas with little rainfall, the deficiencies in cost and environmental protection of existing technologies have been solved, efficient and stable management of sand-laden slopes has been achieved, adapted to the climate conditions in arid areas, and reduced Reduce construction costs and provide green and environmentally friendly solutions.
Patent Information
- Application Number
- CN202410763141.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
AI Technical Summary
In arid and rainless areas, existing slope stabilization management methods such as the net spraying method and the slope grass planting frame protection method have shortcomings in terms of cost and environmental protection, and are difficult to adapt to the specific needs of sandy slopes, especially the construction period. It is long, costly and poorly targeted.
A chemical curing material for sand-filled slopes and corresponding construction technology were developed, using components such as trimethylpentanediol monoisobutyrate, ethylene glycol/propylene glycol, and AMP-95 multifunctional amine additives, combined with soil Stabilizers, biological nitrogen-fixing bacteria and slow-release fertilizers are sprayed and grouted to form a stable membrane structure to enhance the soil's water-holding capacity and erosion resistance.
This method significantly improves the bearing capacity and stability of the sand layer, reduces the need for later maintenance, adapts to the climate conditions in arid areas, reduces construction costs, and provides a green and environmentally friendly solution.
Smart Images

Figure CN118772891A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of slope engineering construction, and more specifically to the technical field of slope engineering construction in arid and rainless areas. Background Art
[0002] When excavating a road cut, it is usually necessary to stabilize the slope after excavation. The current industry practices for slope instability are usually the mesh spraying method and the slope grass frame protection method; the mesh spraying method requires the hanging of steel mesh, and the mesh must have a reliable support point. The mesh anchor rod is driven into the hard geology. For the loose geology of the slope, it cannot provide a strong support point, and this method is costly, with a long construction and maintenance cycle, which is not conducive to environmental protection. The slope grass frame protection forms a stable frame through a concrete frame, and stabilizes the slope soil by planting grass to prevent loss, but this method is poorly targeted for sandy slopes, and has a long construction period, many processes, and high manual maintenance costs.
[0003] Many areas in China often have low precipitation, high evaporation, high temperature and dry climate. Figure 3 For example, due to the climate characteristics of little rain, large evaporation, and long overall route of highway projects, drip irrigation, sprinkler and other maintenance measures cannot be adopted. In many areas, the soil is clay, sand layer, silt, Gobi material, loess, soft saline soil and alkaline soil, etc. Class I soil and Class II soil and Class III soil with small particle size and poor weathering resistance. This type of soil combined with local climatic conditions cannot consider the widely used vegetation slope protection, ecological slope protection, and skeleton plant slope protection. The three types of construction methods for mild climate and suitable for plant growth areas. In view of this situation, it is necessary to develop chemical curing materials and construction processes suitable for sand-mixed slopes. Summary of the invention
[0004] The first object of the present invention is to provide a sand-containing slope chemical curing material to meet the needs of sand layer slope protection.
[0005] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:
[0006] A chemical curing material for sand-containing slopes, comprising the following raw material components in parts by weight: 50-100 parts of trimethylpentanediol monoisobutyrate, 50-100 parts of ethylene glycol / propylene glycol, 20-50 parts of AMP-95 multifunctional amine additive, 5-10 parts of defoaming agent, 200-350 parts of vinyl acetate-ethylene copolymer emulsion, 100-150 parts of soil stabilizer, 10-30 parts of biological nitrogen-fixing bacteria, 40-60 parts of slow-release fertilizer, 20-50 parts of anti-corrosion agent, 5-10 parts of mildew inhibitor, 10-30 parts of pH regulator, and 10-30 parts of salt-alkali resistance agent;
[0007] The soil stabilizer is one of polyacrylamide or cellulose derivatives;
[0008] The water retaining agent is one of sodium polyacrylate or carboxymethyl cellulose;
[0009] The anti-corrosion agent is a polymer film;
[0010] The preparation method of the chemical curing material for sand-included slope is as follows: the rotation speed is adjusted to 400-500 rpm in a stirring container, 50-100 parts of trimethylpentanediol monoisobutyrate and 50-100 parts of ethylene glycol / propylene glycol are mixed and stirred at a temperature of 35-80° for 10-15 minutes, 20-50 parts of AMP-95 multifunctional amine additive and 5-10 parts of defoamer are slowly added while stirring, the stirring speed is increased to 600-700 rpm, stirring is continued for 20 minutes to ensure uniform dispersion, and then vinegar is added. Add 200-350 parts of acid ethylene-ethylene copolymer emulsion, stir for 15 minutes, then add 100-150 parts of soil stabilizer, 10-30 parts of biological nitrogen-fixing bacteria, 40-60 parts of slow-release fertilizer, stir for 10 minutes, then add 20-50 parts of anti-corrosion agent, 5-10 parts of mildew inhibitor, 10-30 parts of pH adjuster, 10-30 parts of salt-alkali resistance agent in sequence. After each component is added, adjust the stirring speed to 800rpm, continue stirring for 5 minutes, adjust the solution to the required viscosity, form the finished curing agent and store it.
[0011] Through the above scheme, trimethylpentanediol monoisobutyrate and ethylene glycol / propylene glycol as solvents and plasticizers help adjust the viscosity and drying speed of the coating. Help improve the fluidity and coating properties of the coating. Help improve the fluidity and flexibility of the mixture for easy application. Multifunctional amine adjuvant AMP-95 as a curing accelerator can accelerate the curing process of the mixture in the soil. Defoamers are used to reduce the foam generated by the mixture during mixing or application. Vinyl acetate-ethylene copolymer emulsion as a binder helps the mixture form a stable film on the soil surface. Soil stabilizers and anti-erosion agents are key components in the formula to enhance soil structure and resist erosion. Water retainers and soil conditioners help improve the water holding capacity and structure of the soil. Biological nitrogen-fixing bacteria and slow-release fertilizers provide the nutrients needed for plant growth. Antifungal agents help plants grow healthily. pH adjusters and anti-salinity agents are used to adjust the chemical properties of the soil to make it more suitable for plant growth. This formula has good adhesion and film-forming properties. Excellent flexibility and durability. And can accelerate the drying and curing process. Improve water resistance, chemical resistance and weather resistance. Reduce foam during spraying and improve surface quality. It will be able to better adapt to the application of sandy soil surface, provide soil improvement, water retention, nutrient supply, anti-erosion and other multiple functions, thereby improving plant growth conditions and the overall quality of soil. After acting on the sand layer, the various effective ingredients in it interact with the corresponding gases in the air, and a series of complex physical and chemical changes occur, so that the originally loose soil particles form a tight structure as a whole, thereby improving the strength and density, and improving the bearing capacity of the sand layer. In addition, the solidified sand layer has good water repellency and freeze-thaw resistance, which will effectively improve the looseness of the slope, improve the stability of the slope, dry naturally, and do not require later maintenance. It is particularly suitable for sand layer slopes in areas with low precipitation, large evaporation, high temperature, and arid climate. It has strong adaptability and saves costs. It has good operability in terms of economy, technology, environment and construction methods.
[0012] The second purpose of the present invention is to provide a sand-included slope chemical curing construction process, improve construction efficiency, prolong the slope protection stability, reduce later maintenance, and meet the needs of sand layer slope protection.
[0013] The construction process of chemical curing of sand-included slope by the curing material has the following steps:
[0014] Step S1: excavating and leveling the slope, excavating and trimming the slope;
[0015] Step S2: Sampling and testing of the geological layer of the slope, selecting a suitable amount of representative samples of different stratum structures and geological conditions in the excavation section for on-site sampling, and measuring and testing the looseness of the original slope;
[0016] Step S3: Chemical curing agent configuration and inspection, collect climate data and combine with the inspection results of the slope geological layer to determine the mixing ratio of the chemical curing agent and other additives and adjust the film-forming temperature, stability, soluble solid content, glass transition temperature, penetration depth, viscosity and other indicators to ensure curing, water repellency and freeze-thaw resistance;
[0017] Step S4: Select representative areas on site for control spraying to confirm the optimal number of spraying times of the curing agent;
[0018] Step S5: cleaning the loosened part of the slope to expose the construction surface;
[0019] Step S6: injecting curing agent into the completely loose part;
[0020] Step S7: spray the curing agent over a large area, and re-spray the missed parts;
[0021] Step S8: molding quality inspection.
[0022] Through the above scheme, the curing agent ratio is determined according to the specific soil type, climatic conditions and plant needs. The parts of the slope surface that are easy to peel off and easily eroded by rainwater are treated by surface spraying; for completely loose areas, the curing agent is injected into the loose layer through surface grouting, and a solidified film can be formed on the surface within 6-12 hours, which is conducive to the rapid improvement of the stability of the slope and achieve the overall stability. At the same time, the chemical curing agent is sprayed and infiltrated into the soil surface. The cross-linking degree between the polymers will form a network structure, which captures, adsorbs and agglomerates dust particles and locks them in the network structure, playing the role of wetting, bonding, condensation, dust prevention, erosion prevention and anti-scouring. And further form a colloidal film to reduce the expansion and contraction caused by the change of humidity on the sand layer and soil surface. The sand layer and soil are changed from hydrophilic to hydrophobic, forming a long-term solidification of the sand layer and soil layer, and at the same time it helps to reduce the evaporation inside the slope soil layer and maintain the moisture in the slope. The water retaining agent and soil conditioner help to improve the water holding capacity and structure of the soil. Biological nitrogen-fixing bacteria and slow-release fertilizers provide the nutrients needed for plant growth, facilitating the subsequent growth of slope vegetation and being more environmentally friendly.
[0023] Furthermore, in step S2, the measured and observed data of the sampled soil include the liquid limit, plastic limit, relative density, particle density, and moisture content of the soil.
[0024] Through the above scheme, the plastic limit is determined by the strip rubbing method, which is determined by observing the behavior of the soil. The liquid limit is determined by the Casagrande liquid limit test, which involves vibrating a certain amount of soil under specific conditions until a specific flow distance is formed. The plasticity index is the difference between the liquid limit and the plastic limit, which represents the plastic range of the soil. The calculation formula is: PI=LL-PL, the moisture content is the ratio of the mass of water in the soil to the mass of dry soil, the particle density is the ratio of the mass of soil particles to the volume, which is usually used for soil classification, and the relative density is the ratio of the density of soil particles to the maximum density. Through the above test method, the critical moisture content of sandy soil and fine-grained soil (such as clay) is determined, and the moisture content at which the inter-particle force begins to change significantly is determined. The engineering properties of the soil are judged by this critical moisture content, which is convenient for subsequent construction measurement.
[0025] Furthermore, in step S3, the climate data collected include the local average temperature, maximum temperature, minimum temperature, temperature difference between day and night, annual precipitation, number of precipitation days and average precipitation, annual evaporation, maximum wind speed and average wind speed. Specifically, control tests are carried out on the sampled geological layers, and after the samples are formed, extreme weather tests are carried out to simulate the basic conditions of the local climate to ensure that the stability of the materials meets the requirements.
[0026] Through the above plan, by collecting local climate data, it is convenient to conduct control experiments and simulation experiments, which is convenient for testing the durability of the curing material and its ability to cope with extreme climates, ensuring that the material's stability effect meets the requirements.
[0027] Furthermore, in step S4, in the process of selecting the site, 3 test sections need to be selected for each different geological condition, and the size of each area is 1 meter high and 3 meters long; each group of test areas is divided into 3 squares, and the curing agent is evenly sprayed without liquid gathering and flowing down. The number of spraying times is 1 time, 2 times, and 3 times, and each square is sprayed. The time interval between the first and second times is controlled within 3-15 minutes according to the penetration of the curing agent. After spraying and consolidation, the consolidation depth and surface uniformity, temperature difference resistance performance, anti-seepage performance, wind resistance performance, internal hollowing and surface cracking are tested, and the number of spraying times is comprehensively determined.
[0028] Through the above scheme, by selecting test sections under different geological conditions, this step can ensure that the application effect of the curing agent is widely representative and applicable. The characteristics of being suitable for a variety of geological conditions ensure the adaptability and effectiveness of the curing agent formula for different soil types. The uniform spraying of the curing agent without liquid aggregation and downflow is related to the uniformity and quality of the curing layer and improves the strength and density of the soil. The bearing capacity and stability of the sand-interlayer are improved. By controlling the number of spraying times and time intervals, the penetration capacity and curing speed of the curing agent can be effectively evaluated. The experiment also includes the detection of key indicators such as temperature difference resistance, anti-seepage performance, and wind resistance performance, which are challenges that sandy slopes need to face in natural environments. Through these tests, it can be ensured that the curing agent can provide long-term protection in actual applications and enhance the durability of the slope. Internal hollowing and surface cracking are part of the evaluation, which facilitates the discovery and resolution of problems in construction and ensures construction quality. The whole process provides a strong experimental basis and quality assurance to ensure the construction effect.
[0029] Furthermore, in step S5, air blowing is used to clean the loose parts of the surface until the surface of the slope is still stable when a portable fire-fighting hair dryer is used at a distance of 15 cm from the cleaning surface. The portable fire-fighting hair dryer has a power of 58.8KW, a horsepower of 79HP, and a rotation speed of 68000R. The cleaning process reduces the secondary disturbance to the stability of the slope during the cleaning process.
[0030] Through the above scheme, the loose soil and loose parts on the slope surface are cleaned to expose the construction surface and reduce the impact of loose soil and dust on the curing agent. At the same time, a fire-fighting portable blower is set for testing to form a unified and reliable testing standard.
[0031] Furthermore, in step S6, after the loose part of the slope is cleaned, for the geological situation that it is a discrete layer and there are holes on the surface, drilling and grouting construction is immediately carried out after the surface is cleaned to the designed slope. The depth and dosage of grouting are determined according to the geological conditions. The effective penetration range after drilling is 5.9-8.2cm in diameter at the center of the borehole. The spacing of drilling and grouting is controlled at 13cm-17cm. Local holes are filled with mortar formed by mixing original geological materials with a curing agent.
[0032] Through the above scheme, this step is specifically targeted at areas with loose geology or holes, ensuring that the curing agent can directly act on the parts that need reinforcement the most, improving the pertinence and effectiveness of the construction. Through drilling and grouting, the curing agent can penetrate into the soil to form an effective reinforcement layer, enhancing the stability and erosion resistance of the slope. By precisely controlling the depth and dosage of the drilling, as well as the effective penetration range of the grouting (5.9-8.2cm), the construction team can ensure the uniform distribution and optimal effect of the curing agent, avoiding material waste. The drilling and grouting construction not only improves the construction efficiency and quality of the chemical curing protection of the sandy slope, but also ensures the reinforcement effect by precisely controlling the construction parameters, meeting the requirements of the construction method for curing, water repellency and freeze-thaw resistance.
[0033] Furthermore, in step S6, the grouting equipment uses a cement mortar caulking gun and adds a hose connection at the end. A metal pipe is connected to the end of the hose as a grouting end. The grouting end is inserted into the soil to a depth of 3-7 cm. After insertion, uniform grouting is performed. It is required that the force is uniform and the insertion direction is perpendicular to the slope surface. While grouting, it is slowly pulled out perpendicular to the slope surface. The holes formed by drilling are filled with curing agent to allow the curing agent to fully penetrate.
[0034] Through the above scheme, by selecting a cement mortar caulking gun and transforming it into a grouting end, it is convenient to extract the curing agent and insert it into the soil for grouting. The whole process is uniform and smooth, ensuring the grouting effect of the collapsed porous area and facilitating the full penetration of the curing agent.
[0035] Furthermore, in step S1, excavation is carried out in layers, and the excavation depth of each layer shall not be greater than 3 meters. When excavating to the base layer, a width of 10-30 cm is reserved for manual cleaning of the slope foot. The slope is trimmed by replacing the bucket teeth on the surface of the excavator with strip scrapers for surface trimming.
[0036] Through the above scheme, the slope is excavated in layers to facilitate step-by-step slope maintenance, and width is reserved for manual cleaning of the slope foot. At the same time, strip scrapers are used for surface finishing to initially correct and level the slope surface for subsequent construction.
[0037] Furthermore, in step S8, the self-inspection standard for molding quality inspection is to randomly inspect 3 locations for every 100 square meters of complete curing depth, the effective curing depth is greater than 3.5 mm, the number of cracks larger than 3 mm shall not be greater than 1 location per 100 square meters, the spreading fullness is 100%, and the number of hollows and peelings shall not be greater than 1 square meter per 100 square meters.
[0038] Through the above scheme, the quality inspection standard is closely combined with the characteristics of the chemical curing protection method for sandy slopes, ensuring the high standard of construction and the reliability of the curing effect. The sampling inspection standard requires that the curing depth meets the standard, the number of cracks is strictly controlled, and the hollowing and peeling phenomena are minimized. These are all to verify the penetration and curing effect of the curing agent and ensure the stability and durability of the slope. The requirement of 100% spreading fullness ensures the uniform distribution of the curing agent and avoids the potential risks caused by uneven curing.
[0039] The beneficial effects of the present invention are as follows:
[0040] 1. The chemical curing material for sand-containing slopes provided by the present invention, after being applied to the sand-containing layer, various effective ingredients therein interact with corresponding gases in the air, and a series of complex physical and chemical changes occur, so that the originally loose soil particles form a tightly structured whole, thereby improving the strength and density, and improving the bearing capacity of the sand-containing layer. In addition, the solidified sand-containing layer has good water repellency and freeze-thaw resistance, which will effectively improve the looseness of the slope, improve the stability of the slope, dry naturally, and do not require later maintenance. It is particularly suitable for sand layer slopes in areas with low precipitation, large evaporation, high temperature, and arid climates, and has strong adaptability and cost savings. The curing agent reacts with soil particles to form a tightly structured whole, significantly improving the strength and density of the soil, and effectively resisting erosion and water damage. The liquid form of the curing agent is easy to spray, non-corrosive, harmless, safe and environmentally friendly to construction. The solidified soil surface has good water repellency and freeze-thaw resistance, adapts to changing climate conditions, and ensures the long-term stability of the slope. These advantages together ensure the efficiency, economy and environmental friendliness of the construction;
[0041] 2. The chemical curing construction process for sand-mixed slopes provided by the present invention uses a polymer chemical curing agent that can work closely with soil particles, significantly improving the strength and density of the slope, thereby enhancing the stability of the slope. The curing agent ratio is determined according to the specific soil type, climatic conditions and plant needs, and the parts of the slope surface that are easy to peel off and easily eroded by rainwater are treated by surface spraying; for completely loose areas, the curing agent is injected into the loose layer through surface grouting, and a solidified film can be formed on the surface within 6-12 hours, which is conducive to the rapid improvement of the stability of the slope and achieves an overall stable effect. At the same time, the chemical curing agent is sprayed and infiltrated into the soil surface, and the cross-linking degree between the polymers will form a mesh structure, which captures, adsorbs and agglomerates dust particles and locks them in the mesh structure, playing the role of wetting, bonding, condensation, dust prevention, erosion prevention and anti-scouring. And further form a colloidal film to reduce the expansion and contraction caused by changes in the humidity of the sand-mixed layer and the soil surface. The sand-interlayer and soil are changed from hydrophilic to hydrophobic, forming a long-term solidification of the sand-interlayer and soil layer, while helping to reduce evaporation inside the slope soil layer and retain moisture in the slope. Water retaining agents and soil conditioners help improve the soil's water holding capacity and structure. Biological nitrogen-fixing bacteria and slow-release fertilizers provide the nutrients needed for plant growth, facilitating the growth of slope vegetation in the later stage. It is more green and environmentally friendly, with significant economic benefits, less material usage, and lower labor and machinery costs, providing an economical and efficient solution for slope management;
[0042] 3. By selecting test sections under different geological conditions, this step can ensure that the application effect of the curing agent is widely representative and applicable. The characteristics of being suitable for a variety of geological conditions ensure the adaptability and effectiveness of the curing agent formula for different soil types. By controlling the number of spraying times and time intervals, the penetration ability and curing speed of the curing agent can be effectively evaluated. The experiment also includes the detection of key indicators such as resistance to temperature difference, anti-seepage performance, and resistance to wind performance. These are the challenges that sandy slopes need to face in the natural environment. Through these tests, it can be ensured that the curing agent can provide long-term protection in actual applications and enhance the durability of the slope. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a schematic diagram of the construction process flow of the present invention;
[0044] Figure 2 It is a schematic diagram of the film-forming process of the post-construction curing material of the present invention;
[0045] Figure 3 Here are photos of existing slope protection in arid areas;
[0046] Figure 4 This is a slope effect diagram after construction using the curing agent and construction process of the present invention;
[0047] Figure 5 This is a picture of the experiment simulating the local environment after spraying the curing agent. DETAILED DESCRIPTION
[0048] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0049] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] Example 1
[0051] like Figure 1 As shown, this embodiment provides a chemical curing material for sand-containing slopes, including the following raw material components in parts by weight: 50-100 parts of trimethylpentanediol monoisobutyrate, 50-100 parts of ethylene glycol / propylene glycol, 20-50 parts of AMP-95 multifunctional amine additive, 5-10 parts of defoaming agent, 200-350 parts of vinyl acetate-ethylene copolymer emulsion, 100-150 parts of soil stabilizer, 10-30 parts of biological nitrogen-fixing bacteria, 40-60 parts of slow-release fertilizer, 20-50 parts of anti-corrosion agent, 5-10 parts of mildew inhibitor, 10-30 parts of pH regulator, and 10-30 parts of salt-alkali resistance agent;
[0052] The soil stabilizer is one of polyacrylamide or cellulose derivatives;
[0053] The water retaining agent is one of sodium polyacrylate or carboxymethyl cellulose;
[0054] The anti-corrosion agent is a polymer film;
[0055] The preparation method of the chemical curing material for sand-included slope is as follows: the rotation speed is adjusted to 400-500 rpm in a stirring container, 50-100 parts of trimethylpentanediol monoisobutyrate and 50-100 parts of ethylene glycol / propylene glycol are mixed and stirred at a temperature of 35-80° for 10-15 minutes, 20-50 parts of AMP-95 multifunctional amine additive and 5-10 parts of defoamer are slowly added while stirring, the stirring speed is increased to 600-700 rpm, stirring is continued for 20 minutes to ensure uniform dispersion, and then vinegar is added. Add 200-350 parts of acid ethylene-ethylene copolymer emulsion, stir for 15 minutes, then add 100-150 parts of soil stabilizer, 10-30 parts of biological nitrogen-fixing bacteria, 40-60 parts of slow-release fertilizer, stir for 10 minutes, then add 20-50 parts of anti-corrosion agent, 5-10 parts of mildew inhibitor, 10-30 parts of pH adjuster, 10-30 parts of salt-alkali resistance agent in sequence. After each component is added, adjust the stirring speed to 800rpm, continue stirring for 5 minutes, adjust the solution to the required viscosity, form the finished curing agent and store it.
[0056] Trimethylpentanediol monoisobutyrate and ethylene glycol / propylene glycol act as solvents and plasticizers to help adjust the viscosity and drying speed of the coating. Help improve the fluidity and coating properties of the coating. Help improve the fluidity and flexibility of the mixture for easy application.
[0057] Multifunctional amine additive AMP-95 acts as a curing accelerator to accelerate the curing process of the mixture in the soil. Defoamers are used to reduce the foam generated by the mixture during mixing or application. Vinyl acetate-ethylene copolymer emulsion acts as a binder to help the mixture form a stable film on the soil surface.
[0058] Soil stabilizers and anti-erosion agents are key ingredients in the formulation to strengthen soil structure and resist erosion. Water retainers and soil conditioners help improve the soil's water holding capacity and structure. Biological nitrogen fixers and slow-release fertilizers provide the nutrients plants need to grow. Mold inhibitors help plants grow healthily. pH adjusters and salt and alkali inhibitors are used to adjust the chemical properties of the soil to make it more suitable for plant growth.
[0059] The test data of this formula curing agent is as follows
[0060]
[0061] This formula has good adhesion and film-forming properties. Excellent flexibility and durability. It can also accelerate the drying and curing process. It improves water resistance, chemical resistance and weather resistance. It reduces foam during spraying and improves surface quality. It will be better adapted to the application of sandy soil surface, providing multiple functions such as soil improvement, water retention, nutrient supply, and anti-erosion, thereby improving plant growth conditions and the overall quality of the soil. After acting on the sand layer, the various active ingredients in it interact with the corresponding gases in the air, and a series of complex physical and chemical changes occur, so that the originally loose soil particles form a tightly structured whole, thereby improving the strength and density, and improving the bearing capacity of the sand layer. In addition, the solidified sand layer has good water repellency and freeze-thaw resistance, which will effectively improve the looseness of the slope, improve the stability of the slope, dry naturally, and do not require later maintenance. It is particularly suitable for sand layer slopes in areas with low precipitation, large evaporation, high temperature, and arid climate. It has strong adaptability and saves costs. It has good operability in terms of economy, technology, environment and construction methods.
[0062] Embodiment 2
[0063] According to the formula ratio, weigh 50-100 parts of trimethylpentanediol monoisobutyrate, 50-100 parts of ethylene glycol / propylene glycol, 20-50 parts of AMP-95 multifunctional amine additive, 5-10 parts of defoamer, 200-350 parts of vinyl acetate-ethylene copolymer emulsion, 100-150 parts of soil stabilizer, 10-30 parts of biological nitrogen-fixing bacteria, 40-60 parts of slow-release fertilizer, 20-50 parts of anti-corrosion agent, 5-10 parts of mildew inhibitor, 10-30 parts of pH regulator, and 10-30 parts of salt-alkali resistance agent. Prepare according to the following steps.
[0064] S1In a large mixing container, first add trimethylpentanediol monoisobutyrate and ethylene glycol / propylene glycol, turn on the agitator, set to medium speed, and ensure that the two solvents are fully mixed. S2Slowly add AMP-95 multifunctional amine additive and continue to stir until it is completely dissolved. Then add the defoamer and adjust the stirring speed to ensure that the defoamer is evenly dispersed. S3Add the adhesive and add the vinyl acetate-ethylene copolymer emulsion to the mixture, increase the stirring speed until the emulsion is completely mixed and uniform. S4Add soil stabilizer and biological nitrogen-fixing bacteria to the mixture, adjust the stirring speed to ensure uniform dispersion, and complete the mixing of soil stabilizer and biological nitrogen-fixing bacteria. S5Continue to add slow-release fertilizer and anti-erosion agent, keep stirring until the components are completely mixed, and add slow-release fertilizer and anti-erosion agent. S6During the stirring process, carefully add mildew inhibitor, pH adjuster and anti-salinity agent until the mixture is evenly mixed. S7During the mixing process, take samples regularly and use a viscometer and pH meter to test the viscosity and pH value of the mixture to ensure that the product meets the construction requirements. S8Filter the mixture through a filter to remove possible undissolved particles or impurities. Place the filtered mixture into a pre-cleaned and dried storage container to form a finished curing agent and seal it for storage. Store the product in a cool and dry environment, away from direct sunlight and high temperatures. During transportation, ensure that the container is sealed to prevent leakage and contamination.
[0065] Embodiment 3
[0066] This embodiment provides a chemical curing construction process for sand-containing slopes, which improves construction efficiency, prolongs the stability of slope protection, reduces later maintenance, and meets the needs of sand layer slope protection.
[0067] Reference Figure 1 and Figure 2 and Figure 4 The construction process of chemical curing of sand-included slope by the curing material has the following steps:
[0068] Step S1: excavating and leveling the slope, excavating and trimming the slope;
[0069] Step S2: Sampling and testing of the geological layer of the slope, selecting a suitable amount of representative samples of different stratum structures and geological conditions in the excavation section for on-site sampling, and measuring and testing the looseness of the original slope;
[0070] Step S3: Chemical curing agent configuration and inspection, collect climate data and combine with the inspection results of the slope geological layer to determine the mixing ratio of the chemical curing agent and other additives and adjust the film-forming temperature, stability, soluble solid content, glass transition temperature, penetration depth, viscosity and other indicators to ensure curing, water repellency and freeze-thaw resistance;
[0071] Step S4: Select representative areas on site for control spraying to confirm the optimal number of spraying times of the curing agent;
[0072] Step S5: cleaning the loosened part of the slope to expose the construction surface;
[0073] Step S6: injecting curing agent into the completely loose part;
[0074] Step S7: spray the curing agent over a large area, and re-spray the missed parts;
[0075] Step S8: molding quality inspection.
[0076] Through the above scheme, the curing agent ratio is determined according to the specific soil type, climatic conditions and plant needs. The parts of the slope surface that are easy to peel off and easily eroded by rainwater are treated by surface spraying; for completely loose areas, the curing agent is injected into the loose layer through surface grouting, and a solidified film can be formed on the surface within 6-12 hours, which is conducive to the rapid improvement of the stability of the slope and achieve the overall stability. At the same time, the chemical curing agent is sprayed and infiltrated into the soil surface. The cross-linking degree between the polymers will form a network structure, which captures, adsorbs and agglomerates dust particles and locks them in the network structure, playing the role of wetting, bonding, condensation, dust prevention, erosion prevention and anti-scouring. And further form a colloidal film to reduce the expansion and contraction caused by the change of humidity on the sand layer and soil surface. The sand layer and soil are changed from hydrophilic to hydrophobic, forming a long-term solidification of the sand layer and soil layer, and at the same time it helps to reduce the evaporation inside the slope soil layer and maintain the moisture in the slope. The water retaining agent and soil conditioner help to improve the water holding capacity and structure of the soil. Biological nitrogen-fixing bacteria and slow-release fertilizers provide the nutrients needed for plant growth, facilitating the subsequent growth of slope vegetation and being more environmentally friendly.
[0077] In step S1, excavation is carried out in layers, and the excavation depth of each layer shall not exceed 3 meters. When excavating to the base layer, a 10-30cm width is reserved for manual cleaning of the slope foot. The slope trimming work uses the bucket teeth on the surface of the excavator to replace the strip scraper for surface trimming. By excavating the slope in layers, it is convenient to carry out slope maintenance step by step, and a width is reserved for manual cleaning of the slope foot. At the same time, a strip scraper is used for surface trimming, and the slope surface is initially corrected and leveled to facilitate subsequent construction.
[0078] In step S2, the sampled soil is measured and observed for data including the liquid limit, plastic limit, relative density, particle density, and moisture content of the soil. Through the above scheme, the plastic limit is determined by the rubbing method, which is determined by observing the behavior of the soil, and the liquid limit is determined by the Casagrande liquid limit test, which involves vibrating a certain amount of soil under specific conditions until a specific flow distance is formed. The plasticity index is the difference between the liquid limit and the plastic limit, which represents the plastic range of the soil, and the calculation formula is: PI = LL-PL, the moisture content is the ratio of the mass of water in the soil to the mass of dry soil, the particle density is the ratio of the mass of soil particles to the volume, which is usually used for soil classification, and the relative density is the ratio of the density of soil particles to the maximum density. Through the above test method, the critical moisture content of sandy soil and fine-grained soil (such as clay) is determined, and the moisture content at which the inter-particle force begins to change significantly is determined. The engineering properties of the soil are judged by this critical moisture content, which is convenient for subsequent construction measurement.
[0079] Reference Figure 5 In step S3, the climate data collected include the local average temperature, maximum temperature, minimum temperature, temperature difference between day and night, annual precipitation, number of precipitation days and average precipitation, annual evaporation, maximum wind speed and average wind speed. Specifically, a control test is carried out on the sampled geological layer, and after the sample is formed, an extreme weather test is carried out to simulate the basic conditions of the local climate to ensure that the stability of the material meets the requirements.
[0080] By collecting local climate data, it is convenient to conduct control experiments and simulation experiments, which can help test the durability of curing materials and their ability to cope with extreme climates, and ensure that the material's stability meets the requirements.
[0081] In step S4, during the selection of the site, 3 test sections need to be selected for each different geological condition, and the size of each area is 1 meter high and 3 meters long; each group of test areas is divided into 3 squares, and the curing agent is evenly sprayed, and there is no liquid gathering and flowing down. The number of spraying times is 1 time, 2 times, and 3 times, and each square is sprayed. The time interval between the first and second times is controlled within 3-15 minutes according to the penetration of the curing agent. After spraying and consolidation, the depth of consolidation and the uniform state of the surface, the performance against temperature difference, the anti-seepage performance, the performance against wind force, the internal hollowing and the surface cracking are checked, and the number of spraying times is comprehensively determined. Refer to the table below, which is a table of curing agent control test samples under different geological conditions collected in the early stage and during the construction process (the following figure is the experimental data of the sand layer and clay layer and the adjacent material layer) and different spraying times.
[0082] Table 2.1 Adaptability analysis of existing slope management practices (sand layer)
[0083]
[0084] Table 2.2 Adaptability analysis of existing slope management practices (clay layer)
[0085]
[0086] Table 2.3 Adaptability analysis of existing slope management practices (Gobi material layer)
[0087]
[0088] By selecting test sections under different geological conditions, this step can ensure that the application effect of the curing agent is widely representative and applicable. The characteristics of being suitable for a variety of geological conditions ensure the adaptability and effectiveness of the curing agent formula for different soil types. The uniform spraying of the curing agent without liquid aggregation and downflow is related to the uniformity and quality of the curing layer and improves the strength and density of the soil. The bearing capacity and stability of the sand-interlayer are improved. By controlling the number of spraying times and time intervals, the penetration capacity and curing speed of the curing agent can be effectively evaluated. The experiment also includes the detection of key indicators such as temperature difference resistance, anti-seepage performance, and wind resistance performance, which are challenges that sandy slopes need to face in natural environments. Through these tests, it can be ensured that the curing agent can provide long-term protection in actual applications and enhance the durability of the slope. Internal hollowing and surface cracking are part of the evaluation, which makes it easy to discover and solve problems in construction and ensure construction quality. The whole process provides a strong experimental basis and quality assurance to ensure the construction effect.
[0089] At the same time, in order to prove the best curing agent spraying concentration, refer to the following table, which is a 75% concentration sand layer spraying analysis table.
[0090] Table 2.5 Adaptability analysis of existing slope management practices (sand layer) Concentration 75%
[0091]
[0092] It can be seen from the above table that in this embodiment, the curing agent spraying concentration is more appropriately 100%, and the number of spraying times is 3 times.
[0093] In step S5, the loose parts of the surface are cleaned by blasting until the slope surface is stable at a distance of 15 cm from the cleaning surface using a portable fire-fighting hair dryer. The power of the portable fire-fighting hair dryer is 58.8KW, the horsepower is 79HP, and the speed is 68000R. The cleaning process reduces the secondary disturbance of the stability of the slope during the cleaning process. The loose soil and loose parts on the slope surface are cleaned to expose the construction surface and reduce the influence of loose soil and dust on the curing agent. At the same time, the portable fire-fighting hair dryer is set for testing to form a unified and reliable testing standard.
[0094] In step S6, after the loose part of the slope is cleaned, for the geological situation that it is a discrete layer and there are holes on the surface, drilling and grouting construction is immediately carried out after the surface is cleaned to the designed slope. The depth and dosage of grouting are determined according to the geological conditions. The effective penetration range after drilling is 5.9-8.2cm in diameter at the center of the borehole. The spacing of drilling and grouting is controlled at 13cm-17cm. Local holes are filled with mortar formed by mixing original geological materials with a curing agent.
[0095] This step is specifically targeted at areas with loose geology or holes, ensuring that the curing agent can directly act on the parts that need reinforcement the most, improving the pertinence and effectiveness of the construction. Through drilling and grouting, the curing agent can penetrate deep into the soil to form an effective reinforcement layer, enhancing the stability and erosion resistance of the slope. By precisely controlling the depth and dosage of the drill holes, as well as the effective penetration range of the grouting (5.9-8.2cm), the construction team can ensure the uniform distribution and optimal effect of the curing agent, avoiding material waste. The drilling and grouting construction not only improves the construction efficiency and quality of the chemical curing protection of the sandy slope, but also ensures the reinforcement effect by precisely controlling the construction parameters, meeting the requirements of the construction method for curing, water repellency and freeze-thaw resistance.
[0096] In step S6, the grouting equipment uses a cement mortar caulking gun and adds a hose connection at the end. A metal pipe is connected to the end of the hose as the grouting end. The grouting end is inserted into the soil to a depth of 3-7 cm. After insertion, uniform grouting is performed. It is required that the force is uniform and the insertion direction is perpendicular to the slope surface. While grouting, it is slowly pulled out perpendicular to the slope surface. The holes formed by drilling are filled with curing agent to allow the curing agent to fully penetrate. Construction method for local hole repair: For the parts that have been hollowed out and have slope appearance requirements, the original geological materials can be used to mix and fully blend with the curing agent to form a state similar to mortar and then fill the holes manually, and at the same time, the surface is polished.
[0097] By selecting a cement mortar caulking gun and transforming it into a grouting end, it is convenient to extract the curing agent and insert it into the soil for grouting. The whole process is uniform and smooth, ensuring the grouting effect of the collapsed porous area and facilitating full penetration of the curing agent.
[0098] In step S7, the curing agent is sprayed over a large area. For small areas, it is recommended to use a backpack lithium battery high-pressure pump single-nozzle sprayer for manual spraying. The volume is 20 liters and it is continuous in pieces. Each continuous area is more than 1,000 square meters. A portable quad-core pump electric sprayer intelligent high-pressure water pump can be used, adjusted to the atomization mode to increase work efficiency, and equipped with a 100-meter water outlet hose for continuous spraying.
[0099] The following table can be used as the acceptance standard table for curing agent spraying
[0100] Table of requirements for curing agent index for chemical curing protection construction method of sand-containing slope
[0101]
[0102] Attached below are three engineering examples carried out on site by the applicant as auxiliary verifications of the present invention.
[0103] Project Example 1
[0104] Project Overview
[0105] Reference Figure 3 and Figure 4 This method was implemented in a highway construction project in Kashgar Economic Development Zone, involving the treatment of sandy layers on 10 sections of road cutting slopes. A total of 4,133.5 square meters of sandy layers on the road cutting slopes were treated, and 2,650 kg of polymer soil solidifier was used.
[0106] Construction status
[0107] A highway construction project in Kashgar Economic Development Zone completed the treatment of 4133.5 square meters of sand-interlayered layers on the road cutting slope in four days from June 25 to June 28, 2023. The on-site treatment of the sand-interlayered layers only requires no rainfall on the construction day and the following three days, and the daily minimum temperature is greater than 10 degrees Celsius. Four workers and one aerial work vehicle can complete the work of spraying 1200m2-1600m2 of the treatment layer twice a day according to the actual terrain conditions if there is enough working surface.
[0108] Project Evaluation
[0109] The completed curing agent treatment area was inspected again on September 25, 2023. No peeling, flaking, hollowing, etc. occurred on site. The overall surface was flat and could withstand the influence of extreme temperature, extreme rainfall, and extreme windy weather in Kashgar. The construction quality was controllable. The implementation effect of this construction method was recognized and praised by both the supervisor and the owner.
[0110] Project Example 2
[0111] Project Overview
[0112] This method was implemented in the deep foundation pit slope of a pump station in a certain infrastructure construction and supporting project in Kashgar, involving a sand-interlayer slope management area of 6,000 square meters and using 3,846 kg of polymer soil solidifier.
[0113] Construction status
[0114] An infrastructure construction and supporting project in Kashgar Economic Development Zone completed the treatment of 6,000 square meters of sand-interlayered layers on the road cutting slope in five days from July 15, 2023 to July 19, 2023. The on-site operation of the sand-interlayered layer treatment only requires no rainfall on the construction day and the following three days, and the daily minimum temperature is greater than 10 degrees Celsius. Four workers and one aerial work vehicle can complete the work of spraying 1,200m2-1,600m2 of the treatment layer twice a day according to the actual terrain conditions if there is enough working surface.
[0115] 12.3 Project Evaluation
[0116] The completed curing agent treatment area was inspected again on September 27, 2023. No peeling, flaking, hollowing, etc. occurred on site. The overall surface was flat and could withstand the influence of extreme temperature, extreme rainfall, and extreme windy weather in Kashgar. The construction quality was controllable. The implementation effect of this construction method was recognized and praised by both the supervisor and the owner.
[0117] 13. Engineering Example 3
[0118] 13.1 Project Overview
[0119] This method was implemented in the drainage foundation pit of the first section of a government road reconstruction project in Atushi City, Kezhou, involving 5,340 square meters of sand-intercalated layer slope and using 3,423 kg of polymer soil solidifier.
[0120] 13.2 Construction Status
[0121] The first section of a municipal road reconstruction project in Atushi City, Kezhou, completed the treatment of 5,340 square meters of sand-interlayered layers on the road cutting slope in four days from July 22, 2023 to July 25, 2023. The on-site operation of the sand-interlayered layer treatment only requires no rainfall on the construction day and the following three days, and the daily minimum temperature is greater than 10 degrees Celsius. Four workers and one aerial work vehicle can complete the work of spraying 1,200m2-1,600m2 of the treatment layer twice a day if the working surface is sufficient, depending on the actual terrain conditions.
[0122] 13.3 Project Evaluation
[0123] The completed curing agent treatment area was inspected again on September 29, 2023. No peeling, flaking, hollowing, etc. occurred on site. The overall surface was flat and could withstand the influence of extreme temperature, extreme rainfall, and extreme windy weather in Kezhou. The construction quality was controllable. The implementation effect of this construction method was recognized and praised by both the supervisor and the owner.
Claims
1. A chemical curing material for sand-included slope, characterized in that: The invention comprises the following raw material components in parts by weight: 50-100 parts of trimethylpentanediol monoisobutyrate, 50-100 parts of ethylene glycol / propylene glycol, 20-50 parts of AMP-95 multifunctional amine adjuvant, 5-10 parts of defoaming agent, 200-350 parts of vinyl acetate-ethylene copolymer emulsion, 100-150 parts of soil stabilizer, 10-30 parts of biological nitrogen-fixing bacteria, 40-60 parts of slow-release fertilizer, 20-50 parts of anti-corrosion agent, 5-10 parts of mildew inhibitor, 10-30 parts of pH regulator, and 10-30 parts of salt-alkali resistance agent. The soil stabilizer is one of polyacrylamide or cellulose derivatives; The water-retaining agent is one of sodium polyacrylate or carboxymethyl cellulose; The anti-corrosion agent is a polymer film; The preparation method of the chemical curing material for sand-included slope is as follows: in a stirring container, the rotation speed is adjusted to 400-500 rpm, 50-100 parts of trimethylpentanediol monoisobutyrate and 50-100 parts of ethylene glycol / propylene glycol are mixed and stirred at a temperature of 35-80° for 10-15 minutes, 20-50 parts of AMP-95 multifunctional amine additive and 5-10 parts of defoamer are slowly added while stirring, the stirring speed is increased to 600-700 rpm, and stirring is continued for 20 minutes to ensure uniform dispersion, and then vinegar is added. Add 200-350 parts of ethylene glycol-vinyl copolymer emulsion and stir for 15 minutes. Then add 100-150 parts of soil stabilizer, 10-30 parts of biological nitrogen-fixing bacteria, and 40-60 parts of slow-release fertilizer and stir for 10 minutes. Then add 20-50 parts of anti-corrosion agent, 5-10 parts of mildew inhibitor, 10-30 parts of pH regulator, and 10-30 parts of salt-alkali resistance agent in sequence. After each component is added, adjust the stirring speed to 800 rpm and continue stirring for 5 minutes. Adjust the solution to the required viscosity to form a finished curing agent and store it.
2. The chemical curing material for sand-included slope according to claim 1, characterized in that: The construction process of chemical curing of sand-included slope using this curing material has the following steps: Step S1: excavation and leveling of the slope, excavation and trimming of the slope; Step S2: Sampling and testing of the geological layer of the slope: selecting a suitable amount of representative samples of different stratum structures and geological conditions in the excavation section for on-site sampling, and measuring and testing the looseness of the original slope; Step S3: Chemical curing agent preparation and testing: collect climate data and combine it with the test results of the slope geological layer to determine the mixing ratio of the chemical curing agent and other additives, and adjust the film forming temperature, stability, soluble solid content, glass transition temperature, permeability depth, viscosity and other indicators to ensure curing, water repellency and freeze-thaw resistance; Step S4: Select a representative area on site for control spraying to confirm the optimal number of spraying times of the curing agent; Step S5: cleaning the loose part of the slope to expose the construction surface; Step S6: injecting curing agent into the completely loose part; Step S7: spray the curing agent over a large area, and re-spray any missed areas; Step S8: Molding quality inspection.
3. The chemical curing construction process for sand-included slope according to claim 2, characterized in that: In step S2, the sampled soil is measured and observed for data including the liquid limit, plastic limit, relative density, particle density, and moisture content of the soil.
4. The chemical curing construction process for sand-included slope according to claim 2, characterized in that: In step S3, the climate data collected include the local average temperature, maximum temperature, minimum temperature, temperature difference between day and night, annual precipitation, number of precipitation days and average precipitation, annual evaporation, maximum wind speed and average wind speed. Specifically, a control test is conducted on the sampled geological layer, and after the sample is formed, an extreme weather test is conducted to simulate the basic conditions of the local climate to ensure that the stability of the material meets the requirements.
5. The chemical curing construction process for sand-included slope according to claim 4, characterized in that: In step S4, during the site selection process, 3 test sections need to be selected for each different geological condition, and the size of each area is 1 meter high and 3 meters long; each group of test areas is divided into 3 squares, and the curing agent is evenly sprayed without liquid accumulation and flow down. The number of spraying times is 1 time, 2 times, and 3 times, and one square is sprayed each time. The time interval between the first and second times is controlled within 3-15 minutes according to the penetration of the curing agent. After spraying and consolidation, the consolidation depth and surface uniformity, temperature difference resistance, anti-seepage performance, wind resistance performance, internal hollowing and surface cracking are tested to determine the number of spraying times.
6. The chemical curing construction process for sand-included slope according to claim 5, characterized in that: In step S5, air blowing is used to clean the loose parts of the surface until the slope surface is stable when a fire portable blower is used at a distance of 15 cm from the cleaning surface. The fire portable blower has a power of 58.8KW, a horsepower of 79HP, and a speed of 68000R. The cleaning process reduces the secondary disturbance to the stability of the slope during the cleaning process.
7. The chemical curing construction process for sand-included slope according to claim 6, characterized in that: In step S6, after the loose part of the slope is cleaned, for the geological situation that it is a discrete layer and there are holes on the surface, drilling and grouting construction is immediately carried out after the surface is cleaned to the designed slope. The depth and dosage of grouting are determined according to the geological conditions. The effective penetration range after drilling is 5.9-8.2cm in diameter at the center of the borehole. The spacing of drilling and grouting is controlled at 13cm-17cm. Local holes are filled with mortar formed by mixing original geological materials with a curing agent.
8. The chemical curing construction process for sand-included slope according to claim 7, characterized in that: In step S6, the grouting equipment uses a cement mortar caulking gun and adds a hose connection at the end. A metal pipe is connected to the end of the hose as a grouting end. The grouting end is inserted into the soil to a depth of 3-7 cm. After insertion, uniform grouting is performed. It is required that the force is uniform and the insertion direction is perpendicular to the slope surface. While grouting, it is slowly pulled out perpendicular to the slope surface. The holes formed by drilling are filled with curing agent to allow the curing agent to fully penetrate.
9. The chemical curing construction process for sand-included slope according to claim 2, characterized in that: In step S1, excavation is carried out in layers, and the excavation depth of each layer shall not exceed 3 meters. When excavating to the base layer, a width of 10-30 cm is reserved for manual cleaning of the slope foot. The slope is trimmed by replacing the bucket teeth on the surface of the excavator with strip scrapers for surface trimming.
10. The chemical curing construction process for sand-included slope according to claim 2, characterized in that: In step S8, the self-inspection standard for molding quality inspection is to randomly inspect 3 places for every 100 square meters of complete curing depth, the effective curing depth is greater than 3.5mm, the number of cracks larger than 3mm shall not be greater than 1 place per 100 square meters, the spreading fullness is 100%, and the number of hollows and peelings shall not be greater than 1 square meter per 100 square meters.