Hydrodesulfurization method for liquefied petroleum gas

Through the gas fractionation and hydrodesulfurization reaction of liquefied petroleum gas, the problems of olefin loss and environmental pollution in the existing technology are solved, efficient desulfurization of liquefied petroleum gas is achieved, and the sulfur content and energy consumption are reduced.

CN118772929AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310358750.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-15
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

Existing liquefied petroleum gas hydrodesulfurization methods inevitably cause olefin losses during the desulfurization process, and traditional processes have environmentally friendly pollutants that are difficult to handle and high energy consumption.

Method used

Through gas fractionation of liquefied petroleum gas, C3 and C4 fractions are obtained, and the liquid form is contacted with the hydrodesulfurization catalyst to perform the hydrodesulfurization reaction. The alcohol amine absorbs and removes hydrogen sulfide, and the liquefied petroleum gas product is refined, using matching reactions. Fraction composition and reaction conditions, control the reaction to reduce olefin loss and sulfur content.

Benefits of technology

It is possible to avoid olefin loss while reducing sulfur content, improve desulfurization efficiency, and reduce environmental pollution and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772929A_ABST
    Figure CN118772929A_ABST
Patent Text Reader

Abstract

The present invention discloses a liquefied petroleum gas hydrodesulfurization method, which comprises: (1) carrying out gas fractionation on a liquefied petroleum gas raw material to obtain a C3 fraction and a C4 fraction; (2) respectively contacting the C3 fraction and the C4 fraction with a hydrodesulfurization catalyst in a liquid form, carrying out hydrodesulfurization reaction, and hydrogenating sulfide in each fraction to generate hydrogen sulfide; wherein the C3 fraction is subjected to a high-temperature hydrodesulfurization reaction, and the C4 fraction is subjected to a low-temperature hydrodesulfurization reaction; and (3) carrying out alcohol amine absorption on hydrodesulfurization reaction effluents of the C3 fraction and the C4 fraction, and removing hydrogen sulfide to obtain a refined liquefied petroleum gas product. According to the method, the reaction fraction composition is matched with the reaction process, the reaction is accurately controlled, and the olefin loss is avoided while the liquefied petroleum gas is subjected to hydrodesulfurization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of liquefied petroleum gas desulfurization, and in particular relates to a liquefied petroleum gas hydrodesulfurization method. Background Art

[0002] The atmospheric and vacuum distillation, catalytic cracking, delayed coking, catalytic reforming, hydrocracking and other units of the refinery will produce a large amount of liquefied petroleum gas as a by-product. Traditionally, liquefied petroleum gas is mainly used as fuel; with the development of chemical technology, liquefied petroleum gas, especially catalytic cracking and other liquefied petroleum gas, contains a large amount of olefins and is increasingly used in the chemical industry, such as polypropylene production, MTBE production, alkylation process, etc. The main components of liquefied petroleum gas are propane, propylene, butane and butene, etc. Untreated liquefied petroleum gas also contains some sulfides. The molecular weight of the sulfides contained in liquefied petroleum gas is generally small and harmful, and its main components are hydrogen sulfide, carbonyl sulfide, mercaptan and sulfide.

[0003] Traditional double desulfurization processes for liquefied petroleum gas are mostly Merox deodorization (Sweeten) processes. One of the disadvantages of double desulfurization (de-H2S and de-sulfurization) is that mercaptans (RSH) are only oxidized and converted into disulfides (RSSR), which does not reduce the total sulfur content or only reduces the total sulfur content to a limited extent. The second disadvantage is that the regenerated organic waste gas and alkali residues produced by the desulfurization device are pollutants that are difficult to treat for environmental protection, and there are potential environmental or safety risks.

[0004] CN200910233505.1 introduces a highly efficient desulfurizer for highly acidic petroleum and natural gas. Its main feature is to add a water-soluble nitrogen-containing organic solvent (basic nitrogen content ≥ 100g / L) to a fiber membrane reactor for desulfurization. Its advantage is that the desulfurization rate is higher than that of the traditional alkanolamine method (such as N-methyldiethanolamine, MDEA); its disadvantage is that the nitrogen-containing organic solvent needs to be repeatedly regenerated and heat exchanged, the process is complicated, and the energy consumption is high.

[0005] CN104194833A introduces a deep desulfurization process for liquefied petroleum gas, which is characterized in that the liquefied petroleum gas is first extracted with amine liquid to remove H2S, and then washed with water to remove the carried amine liquid; then the sulfides in the liquefied petroleum gas are converted into high-boiling point sulfides by hydrogenation conversion on a sulfided Mo-Ni / γ-Al2O3 catalyst; the hydrogenation product enters a stabilization tower, and is distilled and separated using a low-sulfur carbon five or above fraction to obtain an ultra-low sulfur liquefied petroleum gas product, which can be used as a low-sulfur raw material for producing MTBE or alkylation.

[0006] CN103965984A introduces a method for catalytic desulfurization of liquefied petroleum gas, which is characterized in that liquefied petroleum gas is mixed with hydrogen and then enters a fixed bed reactor, and undergoes a thioetherification reaction with a Ni-Mo / γ-Al2O3 catalyst or a Ni-W / γ-Al2O3 catalyst loaded therein to convert low-boiling-point mercaptans into high-boiling-point sulfide compounds; then the thioetherification reaction product is distilled in a distillation tower to obtain a liquefied petroleum gas product free of mercaptans. The disadvantage is that it can only process liquefied petroleum gas that has been treated to remove hydrogen sulfide and carbonyl sulfide, and the distillation tower requires a reboiler, which has high energy consumption. Liquefied petroleum gas contains a large amount of propylene and butene, and the existing hydrodesulfurization method inevitably causes a certain amount of olefin loss while desulfurizing. Summary of the invention

[0007] In view of the deficiencies in the prior art, the present invention provides a method for hydrodesulfurization of liquefied petroleum gas, which matches the composition of the reaction fraction with the reaction process, accurately controls the reaction, and avoids olefin loss during hydrodesulfurization of the liquefied petroleum gas.

[0008] The liquefied petroleum gas hydrodesulfurization method of the present invention comprises the following contents:

[0009] (1) fractionating the liquefied petroleum gas raw material to obtain a C3 fraction and a C4 fraction;

[0010] (2) the C3 fraction and the C4 fraction are contacted with a hydrodesulfurization catalyst in liquid form to perform a hydrodesulfurization reaction, whereby the sulfides in the respective fractions are hydrogenated to generate hydrogen sulfide; wherein the C3 fraction is subjected to a first hydrodesulfurization reaction, and the C4 fraction is subjected to a second hydrodesulfurization reaction;

[0011] (3) The effluent from the hydrodesulfurization reaction of the C3 fraction and the C4 fraction is subjected to alcohol amine absorption to remove hydrogen sulfide and obtain a refined liquefied petroleum gas product.

[0012] In the method of the present invention, the liquefied petroleum gas raw material in step (1) is catalytic cracking (FCC) liquefied petroleum gas, coking liquefied petroleum gas, natural liquefied petroleum gas, etc. Among them, catalytic cracking (FCC) liquefied petroleum gas is preferred, and the typical composition is propylene content of 20.0v% to 40.0v%, butene content of 10.0v% to 30.0v%; total sulfur content of 100 to 5000mg / m 3 , of which the hydrogen sulfide content is 50~5000mg / m 3 , carbonyl sulfide content is 10~50mg / m 3 , methyl mercaptan sulfur content is 50~500mg / m 3 , ethanethiol sulfur content is 50~500mg / m 3 .

[0013] In the method of the present invention, the gas fractionation operation described in step (1) is well known to those skilled in the art and is generally carried out in a gas fractionation device.

[0014] In the method of the present invention, the C3 fraction described in step (2) mainly includes hydrogen sulfide, propane, propylene, and carbonyl sulfide, wherein the propylene content is 50.0v% to 80.0v%, and the hydrogen sulfide content is 50 to 5000mg / m 3 , carbonyl sulfide content is 10~100mg / m 3 .

[0015] In the method of the present invention, the first hydrodesulfurization reaction conditions described in step (2) are: reaction pressure of 0.5-1.6 MPa, reaction temperature of 150-250°C, liquefied petroleum gas feed volume space velocity of 0.2-20.0 h -1 The volume ratio of hydrogen and hydrocarbon (hydrogen and C3 fraction) is 0.1 to 20:1; the preferred operating conditions are as follows: reaction pressure is 0.5 to 1.0 MPa, reaction temperature is 150 to 200°C, and LPG feed volume space velocity is 0.2 to 10.0 h -1 The volume ratio of hydrogen to hydrocarbon is 0.1 to 10:1.

[0016] In the method of the present invention, the first hydrodesulfurization catalyst used in the first hydrodesulfurization reaction described in step (2) is a catalyst that can hydrodesulfurize carbonyl sulfide; for example, a Ni-Mo / γ-Al2O3 or Ni-W / γ-Al2O3 supported hydrodesulfurization catalyst is used, and the content of NiO is 5.0wt% to 20.0wt%, preferably 5.0wt% to 10.0wt%, based on the weight of the catalyst; the content of MoO3 or WO3 is 3.0wt% to 14.0wt%, preferably 3.0wt% to 10.0wt%.

[0017] In the method of the present invention, the first hydrodesulfurization catalyst described in step (2) needs to be pre-sulfurized by a conventional sulfurization method before use, so that the metal oxide active precursor is converted into a catalytically active sulfide active phase; the pre-sulfurization of the catalyst can be carried out by two methods: in-situ sulfurization and ex-situ sulfurization, and the sulfurizing agent can be selected from sulfides such as dimethyl disulfide, hydrogen sulfide, and carbon disulfide.

[0018] In the method of the present invention, the C4 fraction described in step (2) mainly includes butane, butene, methyl mercaptan, ethyl mercaptan, etc., wherein the butene content is 40.0v% to 60.0v%, and the methyl mercaptan content is 50 to 500mg / m 3 , ethanethiol content is 50~500mg / m 3 .

[0019] In the method of the present invention, the second hydrodesulfurization reaction conditions described in step (2) are: reaction pressure of 0.5-2.5 MPa, reaction temperature of 20-100°C, liquefied gas feed volume space velocity of 0.1-20.0 h -1 , hydrogen hydrocarbon (hydrogen and C4 fraction) volume ratio 0.1-20:1; the preferred operating conditions are as follows: reaction pressure 1.0-2.5 MPa, reaction temperature 20-80°C, feed volume space velocity 0.1-10.0 h -1 , the volume ratio of hydrogen to hydrocarbon (hydrogen and C4 fraction) is 0.1 to 10:1.

[0020] In the method of the present invention, the second hydrodesulfurization catalyst used in the second hydrodesulfurization reaction described in step (2) comprises a composite oxide carrier and an active metal component, wherein the composite oxide carrier is graphene oxide-ZnO-Al2O3, wherein the graphene oxide is distributed on the surface of zinc oxide and aluminum oxide; the weight ratio of zinc oxide is 20.0% to 90.0%, preferably 50.0% to 70.0%, the content of graphene oxide is 0.1wt% to 10.0wt%, preferably 0.5wt% to 8.0wt%, and the balance is aluminum oxide; the active metal component is CuO and / or NiO; based on the weight of the catalyst, the content of CuO and / or NiO is 5.0wt% to 20.0wt%, preferably 5.0wt% to 10.0wt%, and the balance is the composite oxide carrier; the specific surface area of ​​the catalyst is 200 to 300m 2 / g, pore size 6.5~7.5nm.

[0021] Wherein, the preparation method of the second hydrodesulfurization catalyst comprises the following contents:

[0022] (a) mixing zinc oxide and aluminum oxide, adding water and a molding aid, kneading, extruding, drying, and calcining to obtain a strip-shaped carrier;

[0023] (b) mixing graphene oxide and a strip-shaped carrier, subjecting the mixture to a first microwave treatment, adding an alkaline solution and subjecting the mixture to a second microwave treatment, filtering the mixture, and drying the mixture to obtain a ZnO-Al2O3 carrier having a surface covered with graphene oxide;

[0024] (c) Spraying an impregnation solution containing Cu and / or Ni onto a ZnO-Al2O3 carrier having a surface covered with graphene oxide to prepare a liquefied petroleum gas desulfurization catalyst.

[0025] The molding aid described in step (a) includes one or more of a peptizing agent and an extrusion aid. The peptizing agent is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc. The extrusion aid refers to a substance that is conducive to extrusion molding, such as one or more of sesbania powder, carbon black, graphite powder, citric acid, etc. The amount of the molding aid is 1.0wt% to 10.0wt% of the carrier.

[0026] The drying method and conditions are recognized by those skilled in the art. For example, the drying method may be air-drying, oven-drying, or forced air drying. Preferably, the drying temperature may be room temperature to 400°C, preferably 100 to 350°C; the drying time may be more than 0.5h, preferably 0.5 to 100h, and more preferably 2 to 20h. The roasting conditions are as follows: the roasting temperature may be 400 to 700°C, preferably 450 to 650°C, and the roasting time may be 0.5 to 100 hours, and more preferably 0.5 to 10 hours.

[0027] The conditions of the first microwave treatment in step (b) are as follows: microwave power is 500-900 W and treatment time is 0.5-3.0 h. The conditions of the second microwave treatment are as follows: microwave power is 500-800 W and treatment time is 1.0-4.0 h.

[0028] The alkaline solution in step (b) can be potassium hydroxide and / or sodium hydroxide aqueous solution, and the mass concentration of the alkaline solution is 5.0% to 40.0%. The ratio of the alkaline solution to the total volume of the graphene oxide and the strip-shaped carrier is 1.5:1 to 2.5:1.

[0029] The impregnation solution containing Cu and / or Ni is an aqueous solution prepared from soluble copper salt and / or nickel salt, and the soluble copper salt and / or nickel salt is one or more of chloride, sulfate, acetate and nitrate.

[0030] The second hydrodesulfurization catalyst needs to be reduced before use. The reduction condition is that the active metal oxide is converted into a metal element under a hydrogen-containing atmosphere, while the metal oxide in the carrier will not be converted. The reduction condition is: pressure of 0.5-2.0 MPa, temperature of 100-550°C, liquefied petroleum gas feed volume space velocity of 0.1-20.0 h -1 The volume ratio of hydrogen agent is 10:1 to 100:1; the preferred reduction conditions are as follows: pressure is 1.0 to 2.0 MPa, temperature is 200 to 450 ° C, feed volume space velocity is 0.1 to 10.0 h -1 The volume ratio of hydrogen agent is 50:1 to 100:1.

[0031] In the method of the present invention, the hydrodesulfurization reaction process described in step (2) can be carried out in a fixed bed reactor, a fluidized bed reactor or an ebullating bed reactor, preferably a fixed bed reactor.

[0032] In the method of the present invention, the alcoholamine absorption in step (3) adopts a commonly used and mature process in industry. The alcoholamine liquid includes at least one of monoethanolamine, diethanolamine and diisopropanolamine.

[0033] Compared with the prior art, the method of the present invention has the following characteristics:

[0034] The present invention matches the composition of the reaction fraction with the reaction process to accurately control the reaction process; first, the liquefied petroleum gas is divided into C3 and C4 fractions, and then hydrodesulfurization is performed respectively; there are a large number of carbonyl sulfide compounds and propylene in the C3 fraction. According to the characteristics of the hydrodesulfurization reaction of carbonyl sulfide compounds and propylene, by controlling a certain reaction temperature and pressure, and coordinating with a first hydrodesulfurization catalyst, the carbonyl sulfide content is reduced while the olefin saturation rate is controlled at a low level; the C4 fraction mainly contains butene and mercaptan compounds. According to the characteristics of the hydrodesulfurization reaction of butene and mercaptan, by controlling the second hydrodesulfurization reaction conditions, and coordinating with a second hydrodesulfurization catalyst, the mercaptan sulfur content is reduced while the olefin saturation rate is controlled at a low level. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic diagram of a process of hydrodesulfurization of liquefied petroleum gas according to the present invention

[0036] Figure 2 This is the TEM image of the zinc oxide-alumina support with graphene oxide coated on the surface of Example 2.

[0037] Figure 3 This is the active metal distribution diagram of the catalyst in Example 2. DETAILED DESCRIPTION

[0038] The method and effects of the present invention are further described below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited thereby.

[0039] The hydrodesulfurization of liquefied petroleum gas of the present invention is carried out as follows: wherein the liquefied petroleum gas raw material 1 enters a gas separation tower to separate a C3 fraction 3 and a C4 fraction 4. The C3 fraction 3 is mixed with hydrogen 5 and enters a hydrodesulfurization reactor 6, and a hydrodesulfurization reaction is carried out under appropriate reaction conditions. The C4 fraction 4 is mixed with hydrogen 5 and enters a hydrodesulfurization reactor 8, and a hydrodesulfurization reaction is carried out under appropriate reaction conditions. The hydrodesulfurization reaction product 7 of the C3 fraction 3 and the hydrodesulfurization product 9 of the C4 fraction 4 are mixed and enter an alcohol amine absorption tower 10 together with a lean amine liquid 11 to remove hydrogen sulfide from the liquefied petroleum gas. A refined liquefied petroleum gas product 12 is obtained from the upper end of the absorption tower 10, and the rich amine liquid 13 obtained from the lower end of the absorption tower 10 is regenerated.

[0040] In the present invention, the specific surface area and pore volume of the catalyst are measured by low-temperature liquid nitrogen adsorption BET method.

[0041] Example 1

[0042] This example prepares a C3 fraction hydrodesulfurization catalyst.

[0043] Weigh 100.0g of pseudo-boehmite powder (Al2O3 dry basis content is 70wt%), add 3.5g of sesbania powder additive accounting for 5wt% of Al2O3 dry basis, 80g of 5wt% nitric acid aqueous solution, mix and roll the mixture into a plastic powder, use an extruder to prepare cylindrical bars with a diameter of 1.5mm, dry at 120℃ for 6 hours, and calcine at 500℃ for 4 hours to prepare a γ-Al2O3 carrier.

[0044] 9.27g of nickel nitrate and 0.88g of ammonium molybdate were weighed, 13.27g of deionized water was added to prepare a solution, and then the solution was impregnated with 20g of the above-mentioned γ-Al2O3 carrier in equal volumes at 30°C for 8h, dried at 120°C for 6h, and calcined at 500°C for 4h to prepare a catalyst numbered C3-1. The physical properties of the C3-1 catalyst are listed in Table 1.

[0045] Example 2

[0046] This example prepares a C4 fraction hydrodesulfurization catalyst.

[0047] Weigh 50.0 g of zinc oxide powder, 71.4 g of aluminum oxide powder (dry basis content 70%), 6.0 g of sesbania powder and an appropriate amount of deionized water, mix and knead, extrude into strips, dry and calcine to obtain a strip-shaped carrier.

[0048] Weigh 0.8 g of graphene oxide (GO) and 60 g of ZnO-Al2O3 carrier into a beaker, put it into a microwave and treat it at 700 W for 1.0 h, then add 94 mL of 10 wt% potassium hydroxide solution and continue to treat it at 600 W for 2.0 h, take it out and filter it, and dry it at 120°C for 8.0 h to obtain a graphene-ZnO-Al2O3 carrier with graphene oxide covered on the surface. Figure 2 TEM image of an alumina-based support with graphene oxide coated on its surface. Figure 2 The network flocs in the graphite are graphene components.

[0049] 37.6 g of nickel nitrate was weighed to prepare 100 mL of impregnation solution, and 85 mL of the impregnation solution was sprayed onto the catalyst support. After drying at room temperature, it was dried at 120° C. for 6 hours and calcined at 470° C. for 4 hours to prepare a catalyst, which was numbered as C4-1 catalyst. The physical properties of the C4-1 catalyst are listed in Table 1.

[0050] Example 3

[0051] This example prepares a C3 fraction hydrodesulfurization catalyst.

[0052] In this example, the γ-Al2O3 carrier is prepared according to the method of Example 1.

[0053] 9.27g of nickel nitrate, 0.78g of ammonium tungstate, and 13.27g of deionized water were weighed to prepare a solution, and then impregnated with 20g of the above-mentioned γ-Al2O3 carrier in equal volumes at 30°C for 8h, dried at 120°C for 6h, and calcined at 500°C for 4h to prepare a catalyst numbered C3-2. The physical properties of the C3-2 catalyst are listed in Table 1.

[0054] Example 4

[0055] This example prepares a C4 fraction hydrodesulfurization catalyst.

[0056] Weigh 60.0 g of zinc oxide powder, 57.0 g of aluminum oxide powder (dry basis content 70%), 6.0 g of sesbania powder and an appropriate amount of deionized water, mix and knead, extrude into strips, dry and calcine to obtain a strip-shaped carrier.

[0057] Weigh 0.5 g of graphene oxide (GO) and 60 g of ZnO-Al2O3 carrier into a beaker, put it into a microwave and treat it at 700 W for 1.0 h, then add 94 mL of 10 wt% potassium hydroxide solution and continue to treat it at 600 W for 2.0 h, take it out and filter it, and dry it at 120°C for 8.0 h to obtain a graphene-ZnO-Al2O3 carrier with graphene oxide covered on the surface.

[0058] 18.9 g of copper nitrate was weighed to prepare 100 mL of impregnation solution, and 85 mL of the impregnation solution was sprayed onto the catalyst support. After drying at room temperature, it was dried at 120° C. for 6 hours and calcined at 470° C. for 4 hours to prepare a catalyst, which was numbered as C4-2 catalyst. The physical properties of the C4-2 catalyst are listed in Table 1. Figure 3 is the active metal distribution diagram of Example 2. Figure 3 It can be seen that the active metals of the catalyst in this embodiment are mainly distributed on the outer surface of the catalyst.

[0059] Example 5

[0060] This embodiment treats a liquefied petroleum gas according to the method of the present invention.

[0061] First, the C3-1 catalyst of Example 1 was subjected to conventional ex-situ pre-sulfurization treatment, that is, the selected sulfiding agent was loaded onto the oxidized catalyst by impregnation, and then subjected to low-temperature drying treatment.

[0062] 10 mL of presulfurized C3-1 catalyst was loaded into Figure 1 In the hydrodesulfurization reactor 6, 10 mL of the C4-1 catalyst in Example 2 was loaded into Figure 1 In the hydrodesulfurization reactor 8. First, the liquefied petroleum gas raw material enters the gas separation tower to separate the C3 fraction and the C4 fraction. The properties of the liquefied petroleum gas raw material and the C3 fraction and the C4 fraction are listed in Table 2.

[0063] The C3 fraction is mixed with hydrogen and enters the hydrodesulfurization reactor 6, where it is reacted for 2 hours at a hydrogen pressure of 1.0 MPa, a temperature of 320°C, and a hydrogen-to-hydrogen volume ratio of 100:1, so that the C3-1 catalyst is completely converted into a sulfurized state; then, the reaction pressure is maintained at 1.0 MPa, the hydrogen-to-hydrocarbon volume ratio is 10:1, the temperature is lowered to 160°C, and the volume space velocity is 10.0 h -1 The properties of the C3 fraction hydrodesulfurization product are listed in Table 2.

[0064] The C4 fraction is mixed with hydrogen and enters the hydrodesulfurization reactor 8, where it is reduced for 2 h at a hydrogen pressure of 1.6 MPa, a temperature of 400°C, and a hydrogen volume ratio of 100:1 to reduce NiO in the C4-1 catalyst to Ni. Then, the reaction pressure is maintained at 1.6 MPa, the hydrogen volume ratio is 10:1, the temperature is lowered to 80°C, and the volume space velocity is 10.0 h / min. -1 The properties of the C4 fraction hydrodesulfurization product are listed in Table 2.

[0065] The hydrodesulfurization reaction product of the C3 fraction is mixed with the hydrodesulfurization product of the C4 fraction, and after hydrogen is separated by a separator, it enters the alcohol amine absorption tower together with the lean amine liquid to remove hydrogen sulfide in the liquefied petroleum gas. The rich amine liquid obtained from the lower end of the absorption tower is regenerated, and the refined liquefied petroleum gas product is obtained from the upper end of the absorption tower. The product properties are listed in Table 2.

[0066] Example 6

[0067] This embodiment treats a liquefied petroleum gas according to the method of the present invention.

[0068] First, the C3-2 catalyst of Example 3 was subjected to conventional ex-situ pre-sulfurization treatment, that is, the selected sulfiding agent was loaded onto the oxidized catalyst by impregnation method, and then subjected to low-temperature drying treatment.

[0069] 10 mL of the presulfurized C3-2 catalyst in Example 3 was loaded into Figure 1 In the hydrodesulfurization reactor 6, 10 mL of the C4-2 catalyst in Example 4 was loaded into Figure 1 In the hydrodesulfurization reactor 8. First, the liquefied petroleum gas raw material enters the gas separation tower to separate the C3 fraction and the C4 fraction. The properties of the liquefied petroleum gas raw material and the C3 fraction and the C4 fraction are listed in Table 2.

[0070] The C3 fraction is mixed with hydrogen and enters the hydrodesulfurization reactor 6, where it is reacted for 2 hours at a hydrogen pressure of 1.0 MPa, a temperature of 320°C, and a hydrogen-to-hydrogen volume ratio of 100:1, so that the L-1 catalyst is completely converted into a sulfurized state; then, the reaction pressure is maintained at 1.0 MPa, the hydrogen-to-hydrocarbon volume ratio is 5:1, the temperature is lowered to 180°C, and the volume space velocity is 5.0 h-1 The properties of the C3 fraction hydrodesulfurization product are listed in Table 2.

[0071] The C4 fraction is mixed with hydrogen and enters the hydrodesulfurization reactor 8, where it is reduced for 2 hours at a hydrogen pressure of 1.0 MPa, a temperature of 220°C, and a hydrogen-to-hydrogen volume ratio of 80:1, so that the CuO in the C4-2 catalyst is reduced to Cu. Then, the reaction pressure is maintained at 1.0 MPa, the hydrogen-to-hydrocarbon volume ratio is 5:1, the temperature is lowered to 50°C, and the volume space velocity is 8.0 h -1 The properties of the C4 fraction hydrodesulfurization product are listed in Table 2.

[0072] The hydrodesulfurization reaction product of the C3 fraction is mixed with the hydrodesulfurization product of the C4 fraction, and after hydrogen is separated by a separator, it enters the alcohol amine absorption tower together with the lean amine liquid to remove hydrogen sulfide in the liquefied petroleum gas. The rich amine liquid obtained from the lower end of the absorption tower is regenerated, and the refined liquefied petroleum gas product is obtained from the upper end of the absorption tower. The product properties are listed in Table 2.

[0073] Comparative Example 1

[0074] This comparative example investigates the hydrodesulfurization effect of the whole fraction of liquefied petroleum gas using the catalyst of Example 1.

[0075] The catalyst of Example 1 is first subjected to conventional ex-situ pre-sulfidation treatment, that is, the selected sulfiding agent is loaded onto the oxidized catalyst by an impregnation method, and then subjected to low-temperature drying treatment.

[0076] 10mL of pre-sulfurized C3-1 catalyst was loaded into the hydrodesulfurization reaction device. First, hydrogen was introduced to increase the pressure. The C3-1 catalyst was reacted for 2 hours under the conditions of hydrogen pressure of 1.0MPa, temperature of 320℃, and hydrogen agent volume ratio of 100:1, so that the C3-1 catalyst was completely converted into a sulfurized state; then, the reaction pressure was maintained at 1.0MPa,

[0077] The volume ratio of hydrogen to hydrocarbon is 10:1. The temperature is lowered to 160°C. At a volume space velocity of 10.0 h -1 The whole fraction liquefied petroleum gas raw material is subjected to a hydrodesulfurization reaction. After the hydrogen is separated from the reaction product by a separator, it enters the alcohol amine absorption tower together with the lean amine liquid to remove the hydrogen sulfide in the liquefied petroleum gas. The rich amine liquid obtained from the lower end of the absorption tower is regenerated, and the refined liquefied petroleum gas product is obtained from the upper end of the absorption tower. The product properties are listed in Table 3.

[0078] Comparative Example 2

[0079] This comparative example investigates the hydrodesulfurization effect of the whole fraction of liquefied petroleum gas using the catalyst of Example 2.

[0080] 10 mL of the C4-1 catalyst of Example 2 was loaded into the hydrodesulfurization reactor. First, hydrogen was introduced to increase the pressure, and the C4-1 catalyst was reduced for 2 h under the conditions of a hydrogen pressure of 1.6 MPa, a temperature of 400°C, and a hydrogen agent volume ratio of 100:1, so that the NiO in the C4-1 catalyst was reduced to Ni; then the reaction pressure was maintained at 1.6 MPa, a hydrogen hydrocarbon volume ratio of 10:1, the temperature was lowered to 80°C, and the volume space velocity was 10.0 h -1 The whole fraction liquefied petroleum gas raw material is subjected to hydrodesulfurization reaction; the reaction product is separated into hydrogen by a separator, and then enters the alcohol amine absorption tower together with the lean amine liquid to remove hydrogen sulfide in the liquefied petroleum gas. The rich amine liquid obtained from the lower end of the absorption tower is regenerated, and the refined liquefied petroleum gas product is obtained from the upper end of the absorption tower. The product properties are listed in Table 3.

[0081] Comparative Example 3

[0082] This comparative example investigates the hydrodesulfurization effect of liquefied petroleum gas under conventional reaction conditions after fractionation.

[0083] In this comparative example, the C3 fraction and the C4 fraction were separated from the liquefied petroleum gas according to the catalyst loading method and process flow of Example 5. The properties of the liquefied petroleum gas raw material and the C3 fraction and the C4 fraction raw material are shown in Table 2.

[0084] The reaction conditions of the C3 fraction were the same as those in Example 5, except that the reaction temperature was adjusted to 120° C. The properties of the C3 fraction hydrodesulfurization product are listed in Table 3.

[0085] The reaction conditions of the C4 fraction were the same as those in Example 5, and the properties of the hydrodesulfurization products are listed in Table 3.

[0086] The hydrodesulfurization reaction product of the C3 fraction is mixed with the hydrodesulfurization product of the C4 fraction, and after hydrogen is separated by a separator, it enters the alcohol amine absorption tower together with the lean amine liquid to remove hydrogen sulfide in the liquefied petroleum gas. The rich amine liquid obtained from the lower end of the absorption tower is regenerated, and the refined liquefied petroleum gas product is obtained from the upper end of the absorption tower. The product properties are listed in Table 3.

[0087] Comparative Example 4

[0088] This comparative example investigates the hydrodesulfurization effect of liquefied petroleum gas under conventional reaction conditions after fractionation.

[0089] In this comparative example, the C3 fraction and the C4 fraction are separated from the liquefied petroleum gas according to the catalyst loading method and process flow of Example 6. The properties of the liquefied petroleum gas raw material and the C3 fraction and the C4 fraction raw material are shown in Table 2.

[0090] The reaction conditions of the C3 fraction were the same as those in Example 6, except that the reaction pressure was adjusted to 2.0 MPa. The properties of the hydrodesulfurization product of the C3 fraction are listed in Table 3.

[0091] The reaction conditions of the C4 fraction were the same as those in Example 6, and the properties of the hydrodesulfurization products are listed in Table 3.

[0092] The hydrodesulfurization reaction product of the C3 fraction is mixed with the hydrodesulfurization product of the C4 fraction, and after hydrogen is separated by a separator, it enters the alcohol amine absorption tower together with the lean amine liquid to remove hydrogen sulfide in the liquefied petroleum gas. The rich amine liquid obtained from the lower end of the absorption tower is regenerated, and the refined liquefied petroleum gas product is obtained from the upper end of the absorption tower. The product properties are listed in Table 3.

[0093] Table 1 Catalyst properties

[0094] project Example 1 Example 2 Example 3 Example 4 Catalyst No. C3-1 C4-1 C3-2 C4-2 <![CDATA[Specific surface area, m 2 ·g -1 > 200.1 240.2 194.7 235.3 Pore ​​diameter, nm 7.1 6.8 8.3 7.0 ZnO, wt% - 50 - 60 Graphene oxide, wt% - 1.32 - 0.83 NiO, wt% 10.0 5 10.0 - CuO, wt% - - - 5 <![CDATA[MoO3,wt%]]> 3.0 - - - <![CDATA[WO3,wt%]]> - - 3.0 -

[0095] Table 2 Properties of LPG feedstock and hydrodesulfurization products

[0096]

[0097] Table 3 Properties of LPG feedstock and hydrodesulfurization products As can be seen from Tables 2 and 3, by using the method of the present invention to treat a liquefied petroleum gas, by controlling a certain reaction temperature and pressure, and by using the first hydrodesulfurization catalyst, a total sulfur content of ≯2.0 mg / m can be produced under the condition of olefin saturation ≯2.0%. 3 Refined liquefied petroleum gas products.

Claims

1. A method for hydrodesulfurization of liquefied petroleum gas, characterized in that The method comprises the following contents: (1) fractionating the liquefied petroleum gas raw material to obtain a C3 fraction and a C4 fraction; (2) contacting the C3 fraction and the C4 fraction with a hydrodesulfurization catalyst in liquid form to perform a hydrodesulfurization reaction, thereby hydrogenating the sulfide in each fraction to generate hydrogen sulfide; The C3 fraction is subjected to a high-temperature hydrodesulfurization reaction, and the C4 fraction is subjected to a low-temperature hydrodesulfurization reaction; (3) the effluents of the hydrodesulfurization reactions of the C3 fraction and the C4 fraction are subjected to alcohol amine absorption to remove hydrogen sulfide and obtain a refined liquefied petroleum gas product.

2. The method according to claim 1, characterized in that: The liquefied petroleum gas raw material in step (1) is one or more of catalytic cracking liquefied petroleum gas, coking liquefied petroleum gas, and natural liquefied petroleum gas.

3. The method according to claim 1, characterized in that: The liquefied petroleum gas raw material in step (1) has a propylene content of 20.0v%~40.0v%, a butene content of 10.0v%~30.0v%; and a total sulfur content of 100~5000mg / m 3 ; The preferred hydrogen sulfide content is 50~5000mg / m 3 , carbonyl sulfide content is 10~50 mg / m 3 , methyl mercaptan sulfur content is 50~500mg / m 3 , ethanethiol sulfur content is 50~500mg / m 3 .

4. The method according to claim 1, characterized in that: The propylene content in the C3 fraction of step (2) is 50.0v%~80.0v%, and the hydrogen sulfide content is 50~5000mg / m 3 , carbonyl sulfide content is 10~100mg / m 3 .

5. The method according to claim 1, characterized in that: The high temperature hydrodesulfurization reaction conditions in step (2) are: reaction pressure of 0.5-1.6 MPa, reaction temperature of 150-250°C, LPG feed volume space velocity of 0.2-20.0 h -1 The volume ratio of hydrogen to hydrocarbon is 0.1 to 20:1; the preferred operating conditions are as follows: reaction pressure is 0.5 to 1.0 MPa, reaction temperature is 150 to 200°C, and the volume space velocity of liquefied petroleum gas feed is 0.2 to 10.0 h -1 The volume ratio of hydrogen to hydrocarbon is 0.1 to 10:

1.

6. The method according to claim 1, characterized in that: The first hydrodesulfurization catalyst used in the high-temperature hydrodesulfurization reaction of step (2) is a Ni-Mo / γ-Al2O3 or Ni-W / γ-Al2O3 supported hydrodesulfurization catalyst, wherein the content of NiO is 5.0wt%~20.0wt%, preferably 5.0wt%~10.0wt%, based on the weight of the catalyst; the content of MoO3 or WO3 is 3.0wt%~14.0wt%, preferably 3.0wt%~10.0wt%.

7. The method according to claim 1, characterized in that: The first hydrodesulfurization catalyst in step (2) is pre-sulfurized before use to convert the metal oxide active precursor into a catalytically active sulfide active phase.

8. The method according to claim 1, characterized in that: The butene content in the C4 fraction of step (2) is 40.0v%~60.0v%, and the methyl mercaptan content is 50~500mg / m 3 , ethanethiol content is 50~500 mg / m 3 .

9. The method according to claim 1, characterized in that: The low-temperature hydrodesulfurization reaction conditions in step (2) are: reaction pressure of 0.5-2.5 MPa, reaction temperature of 20-100°C, liquefied gas feed volume space velocity of 0.1-20.0 h -1 , hydrogen-to-hydrocarbon volume ratio of 0.1 to 20:1; the preferred operating conditions are as follows: reaction pressure of 1.0 to 2.5 MPa, reaction temperature of 20 to 80°C, feed volume space velocity of 0.1 to 10.0 h -1 , hydrogen to hydrocarbon volume ratio 0.1 to 10:

1.

10. The method according to claim 1, characterized in that: The second hydrodesulfurization catalyst used in the low-temperature hydrodesulfurization reaction of step (2) comprises a composite oxide carrier and an active metal component; the composite oxide carrier is graphene oxide-ZnO-Al2O3, wherein the graphene oxide is distributed on the surface of zinc oxide and aluminum oxide; the weight ratio of zinc oxide is 20.0% to 90.0%, the content of graphene oxide is 0.1wt% to 10.0wt%, and the balance is aluminum oxide; the active metal component is CuO and / or NiO; based on the weight of the catalyst, the content of CuO and / or NiO is 5.0wt% to 20.0wt%, and the balance is the composite oxide carrier; the specific surface area of ​​the catalyst is 200 to 300m 2 / g, pore size 6.5~7.5nm.

11. The method according to claim 1, characterized in that: The second hydrodesulfurization catalyst needs to be reduced before use; the reduction conditions are that the active metal oxide is converted into a metal element under a hydrogen-containing atmosphere, while the metal oxide in the carrier is not converted; the reduction conditions are: pressure of 0.5-2.0MPa, temperature of 100-550°C, liquefied petroleum gas feed volume space velocity of 0.1-20.0h -1 The volume ratio of hydrogen agent is 10:1 to 100:

1.

12. The method according to claim 1, characterized in that: The hydrodesulfurization reaction process described in step (2) is carried out in a fixed bed reactor, a fluidized bed reactor or an ebullating bed reactor.

Citation Information

Patent Citations

  • Method for producing ethylene cracking material through hydrogenation of liquefied petroleum gas

    CN102452879A

  • Method for deep desulfurization of liquefied petroleum gas

    CN104789290A

  • Refining method for reducing alkadiene by deeply desulfurizing liquefied petroleum gas in presence of hydrogen

    CN115029158A

  • C4 fraction hydrogenation method

    CN115678604A

  • Process for removal of sulfur and other impurities from olefinic liquefied petroleum gas

    EP3882329A1