Water-soluble high-dispersion nano-copper, preparation method thereof and PSCR application

By using water-soluble highly dispersed nano-copper as a catalyst during coal combustion, the generation of NOX is suppressed, the problem of difficult control of NOX emissions during coal combustion is solved, and low-cost, low-pollution combustion is achieved.

CN118772932APending Publication Date: 2024-10-15NANJING SHENGBOWEI CARBON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410716964.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing technologies are difficult to effectively control NOX emissions during coal combustion, especially in unorganized emission environments. Catalytic reduction methods are costly and unsuitable for industrial applications. Non-catalytic reduction methods are ineffective and difficult to reduce environmental pollution.

Method used

Water-soluble highly dispersed nano-copper is used as a catalyst. After being fully mixed with coal, it prevents the reaction of N2 and O2 during the combustion process, inhibits the generation of NOX, and realizes the process catalytic reduction (PSCR) method to reduce NOX emissions.

Benefits of technology

It effectively reduces NOX emissions during coal combustion, reduces environmental pollution, reduces costs, is suitable for industrial large-scale production, and improves the efficiency of coal combustion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772932A_ABST
    Figure CN118772932A_ABST
Patent Text Reader

Abstract

The invention provides water-soluble high-dispersion nano-copper and a preparation method and PSCR application thereof, the water-soluble high-dispersion nano-copper prepared by taking a compound shown as a formula I, ricinoleic acid amide or castor oil-based quaternary ammonium salt as a surface modifier is applied to a coal combustion process as a catalyst, so that coal can be combusted more sufficiently, the combustion efficiency is improved, and the service life of the water-soluble high-dispersion nano-copper is prolonged. The coal combustion efficiency is improved, meanwhile, emission of nitric oxide in the carbon combustion process can be effectively reduced, and the emission amount of the nitric oxide is smaller than 20 ppm. And for unorganized emission represented by steel production, the cost can be greatly reduced, the environmental pollution can be reduced, and the whole preparation method is safe and controllable and is suitable for industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of new energy materials, and specifically relates to a water-soluble highly dispersed nano copper, a preparation method of the highly dispersed nano copper, and a PSCR application as a catalyst in a coal combustion process, which can effectively reduce the emission of harmful gases in the carbon combustion process. Background Art

[0003] At present, during the coal combustion process, the coal combustion products flow with the wind and are directly discharged from the high-temperature furnace. Since the flue gas stays in the high-temperature area for a short time and the coal combustion products and excess air are mixed unevenly, on the one hand, the coal cannot be completely burned and a large amount of CO and soot are produced, and on the other hand, the NO produced by the combustion X Failure to restore will cause environmental pollution, making it extremely difficult to achieve standard management.

[0004] Currently on NO X Emissions are mainly controlled in NO X After it is generated, it is controlled by catalytic reduction (SCR) and non-catalytic reduction (NSCR) methods. For example, the installation of rare earth catalyst fillers in the chimney of a thermal power plant is a typical application of the SCR method. The basic principle is:

[0005]

[0006] Catalytic reduction can reduce NO X The final content is controlled within 20ppm, but the cost is high and it is not suitable for unorganized emissions.

[0007] Some coal chemical enterprises use ammonia water for denitration. For example, the use of urea liquid for denitration of diesel heavy trucks is a typical application of the NSCR method. The basic principle is:

[0008] NO X +NH3——→N2+H2O

[0009] Non-catalytic reduction methods are relatively low cost, but they are very sensitive to NO X The reduction effect is not as good as that of catalytic reduction (SCR), and it is also not suitable for fugitive emissions.

[0010] Both of the above treatment methods are NO X After the emission is generated, it is treated. For organized emission such as power plants and automobiles, the above method works well, but the disadvantage is that it is costly; it is too troublesome to replace the filler or three-way catalyst, and it cannot be used in an environment with unorganized emission. In particular, NSCR has high requirements for the use environment, the denitrification effect is not very ideal, and there is a risk of ammonia escape. Summary of the invention

[0011] The purpose of the present invention is to provide a method for preparing water-soluble highly dispersed nano copper.

[0012] The second object of the present invention is to provide water-soluble highly dispersed nano copper prepared by the above method as a catalyst for process catalytic reduction (PSCR) technology.

[0013] The third object of the present invention is to provide a water-soluble highly dispersed nano copper as a catalyst in the coal combustion process, which can effectively reduce NO in the carbon combustion process. X emissions.

[0014] The technical solution of the present invention is as follows:

[0015] A method for preparing water-soluble highly dispersed nano copper comprises the following steps: uniformly mixing a reducing agent, a surface modifier, a pH regulator and a solvent, adding a copper precursor aqueous solution to the obtained mixed solution, and performing a reduction reaction at 40-90° C. to obtain highly dispersed nano copper; the surface modifier is a compound shown in formula I, ricinoleic acid amide or castor oil-based quaternary ammonium salt, wherein the structural formula of the compound shown in formula I is as follows:

[0016]

[0017] For the present invention, the copper precursor is one or more of copper sulfate, copper chloride, copper nitrate or copper acetate. In a preferred embodiment, the concentration of the copper precursor aqueous solution is 0.1-1 mol / L.

[0018] For the present invention, the reducing agent is one or more of formaldehyde, sodium borohydride, sodium hypophosphite, hydrazine hydrate or ascorbic acid.

[0019] In the present invention, the reaction temperature is 40-90°C, and may be but not limited to 40°C, 50°C, 60°C, 70°C, 80°C or 90°C. In a preferred embodiment, the reaction temperature is 60-80°C.

[0020] In the present invention, the reducing agent, the surface modifier, the pH regulator and the solvent are mixed uniformly, wherein the solvent is water, anhydrous ethanol or ethanol aqueous solution. In the obtained mixed solution, the concentration of the reducing agent is 0.2-2 mol / L; the concentration of the reducing agent in the obtained mixed solution is 0.02-1 mol / L.

[0021] For the present invention, the molar ratio of the copper precursor, the reducing agent and the surface modifier is 1:1.5-3.5:0.1-1.5, preferably 1:2.0-3.0:0.4-0.8, and more preferably 1:2.5:0.5.

[0022] In the present invention, the pH regulator is one or more of sodium hydroxide, ammonia water, ethylenediamine, diethylamine or triethanolamine.

[0023] In view of the shortcomings or deficiencies of the SCR method and the NSCR method, the present invention provides a PSCR method, in which the water-soluble highly dispersed nano-copper is added to the fuel as a catalyst and mixed thoroughly to prevent the reaction of N2 and O2 during the combustion process, and no or less NO is generated. X The principle is that the catalyst helps NO X Towards a favorable decomposition direction:

[0024]

[0025] Nano-copper catalysis of NO in the environment and process of fuel combustion X The PSCR method can effectively inhibit the generation of NO under various emission conditions. X Emission control.

[0026] For the present invention, the preparation method of the compound shown in formula I comprises the following steps: adding N-oleyl-1,3-propylene diamine and ricinoleic acid into a reaction container, heating to 160-180°C under stirring conditions and reacting at a constant temperature for 1-3 hours, and when no water is produced in the reaction, cooling to 0-10°C in an ice water bath; then adding acrylonitrile dropwise, maintaining the reaction temperature at 0-10°C; after the addition of 2-hydroxyethyl acrylate is completed, heating to 60-80°C and reacting at a constant temperature for 1-3 hours; after the reaction is completed, the obtained reaction product is distilled under reduced pressure to obtain the compound shown in formula I.

[0027] For the present invention, ricinoleic acid amide is prepared by ester exchange reaction using ricinoleic acid as a raw material. For example, ricinoleic acid amide is prepared by ester exchange reaction using ricinoleic acid and N,N-dimethylethanolamine as raw materials under the condition of N-methylimidazole hydrogen sulfate ([Hmim]HSO4) as a catalyst.

[0028] Furthermore, the castor oil-based quaternary ammonium salt is prepared on the basis of the intermediate product ricinoleic acid amide by a quaternization reaction. For example, the ricinoleic acid amide is subjected to a quaternization reaction with epichlorohydrin to obtain the castor oil-based quaternary ammonium salt.

[0029] In the process of preparing highly dispersed nano copper, the present invention found that nano copper particles with a particle size of less than 30 nanometers can effectively reduce NO in the process of burning with gasoline and diesel. X No emissions, not even NO X This finding indicates that highly dispersed nano-copper can play a role in the combustion of NO during fossil fuel combustion. XIt can not only inhibit the production of pollutants, but also help the fuel to burn fully, inhibiting the production of toxic and harmful substances such as PM2.5, PM10, CO, and CH.

[0030] Coal is a large particle fragment, and it is difficult to directly apply the PSCR method. Due to the continuous improvement of combustion technology, large-scale coal-fired projects such as thermal power, steel, cement, and coal chemical industry now crush coal into powder and burn it in the furnace, which lays the foundation for the application of the PSCR method.

[0031] The key to the successful application of the PSCR method is to uniformly mix nano-copper with coal.

[0032] Since the amount of nano copper needed is very small relative to coal, it is impossible to mix it evenly directly. Dissolving nano copper in water and then mixing it with coal in a corresponding proportion is an effective way. Therefore, selecting a specific hydrophilic modifier to modify nano copper so that nano copper can be stably dispersed in water and fully mixed with coal is a breakthrough in applying the PSCR method to coal emission reduction.

[0033] The use of the water-soluble highly dispersed nano copper provided by the present invention as a catalyst in the coal combustion process can effectively reduce the emission of harmful gases in the carbon combustion process.

[0034] In a preferred embodiment, the water-soluble highly dispersed nano copper stock solution is further dispersed in a water pool and added to the crushed coal. For example, the concentration of highly dispersed nano copper dispersed in water is 0.14-1.4%, which can be but not limited to 0.14%, 0.28%, 0.42%, 0.56% or 0.7%, etc.

[0035] According to the present invention, the addition amount of highly dispersed nano-copper per ton of coal is 50-500ppm; preferably 100-400ppm.

[0036] Adopt the technical scheme of the present invention, the advantages are as follows:

[0037] The nano copper prepared by the compound shown in Formula I, ricinoleic acid amide or castor oil-based quaternary ammonium salt as a surface modifier is used as a catalyst in the coal combustion process, which can make the coal combustion more complete, improve the coal combustion efficiency, and effectively reduce the emission of nitrogen oxides in the carbon combustion process, and the nitrogen oxide emission is less than 20ppm. For steel enterprises, it can greatly reduce costs and reduce environmental pollution, and the whole preparation method is simple and suitable for industrial large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 is a TEM image of highly dispersed nano-copper in Example 4;

[0039] Figure 2is a TEM image of highly dispersed nano-copper in Example 5;

[0040] Figure 3 is a TEM image of highly dispersed nano-copper in Example 6;

[0041] Figure 4 This is a TEM image of highly dispersed nano-copper in Comparative Example 1;

[0042] Figure 5 The invention is a synthetic route of obtaining castor oil-based quaternary ammonium salt by quaternizing ricinoleic acid amide with epichlorohydrin. DETAILED DESCRIPTION

[0043] The present invention can be better understood according to the following examples. However, it is easy for those skilled in the art to understand that the contents described in the examples are only used to illustrate the present invention, and should not and will not limit the present invention described in detail in the claims.

[0044] Example 1 Preparation of the compound represented by formula I:

[0045] In a 1L three-necked flask equipped with a mechanical stirrer, a thermometer and a water removal separator, 324.6g (1mol) of N-oleyl-1,3-propylene diamine and 298.5 (1mol) of ricinoleic acid were added, and the temperature was slowly raised to 160°C under stirring conditions and the reaction was kept at a constant temperature for 3 hours. When no water was produced in the reaction, the temperature was slowly lowered to 0°C using an ice water bath; then the water removal separator was removed and a constant pressure dropping funnel was installed, and 53.1g (1mol) of acrylonitrile was slowly added dropwise, and the reaction temperature was maintained at 0-10°C; after the addition of acrylonitrile was completed, the temperature was slowly raised to 60°C and the reaction was kept at a constant temperature for 3 hours; after the reaction was completed, the obtained reaction product was distilled under reduced pressure to obtain a light yellow oily transparent liquid, which was the compound shown in the formula.

[0046] Example 2 Preparation of ricinoleic acid amide:

[0047] A certain amount of N-methylimidazole was added to a three-necked flask with a stirring device, cooled to 0-5°C, stirred vigorously under ice bath conditions, and sulfuric acid aqueous solution was added dropwise for 30 minutes. After the addition was completed, it was stirred at room temperature for 12 hours, and the crude product was distilled under reduced pressure to remove excess water, and vacuum dried to obtain a colorless and transparent ionic liquid N-methylimidazole hydrogen sulfate ([Hmim]HSO4).

[0048] Weigh a certain amount of castor oil (1 mol) and place it in a three-necked flask with a liquid separator, add 8% of the above catalyst, pass nitrogen for 5 minutes, and drop N,N-dimethylethanolamine (6 mol) at room temperature while stirring. After the dropwise addition is completed, heat to 80°C and react for 8 hours. The reaction product is allowed to stand for stratification, the upper layer is washed with deionized water, and the excess water is removed by vacuum distillation at 50°C and 2.67 kPa to obtain the product ricinoleic acid amide.

[0049] Example 3 Preparation of castor oil-based quaternary ammonium salt:

[0050] The ricinoleic acid amide prepared in Example 2 was weighed and placed in a four-necked bottle with a reflux device, nitrogen was passed for 5 minutes, and epichlorohydrin was added dropwise for 30 minutes while stirring, and the temperature was controlled at 48°C. After the addition was completed, the temperature was raised to 50°C and kept for reaction for 1 hour. Excess epichlorohydrin was removed with n-hexane, and the mixture was dried in vacuum to obtain a castor oil-based quaternary ammonium salt.

[0051] Example 4

[0052] Into a 500mL three-necked flask, add 80mL of distilled water, 18mL of NH3·H2O, 0.016mol of the compound of formula I prepared in Example 1, and 5mL of 80% (mass concentration, the same below) hydrazine hydrate, and stir until completely dissolved to obtain a mixed solution; add 0.032mol of CuSO4·5H2O to a beaker, and then add 100mL of distilled water and stir until completely dissolved to prepare a copper precursor aqueous solution; add the obtained copper precursor aqueous solution to the above mixed solution, heat to 80°C and react for 2h to obtain a dark red-brown nano copper dispersion, which can be stably dispersed in water for a long time without coagulation. The obtained nano copper dispersion is centrifuged, washed, and dried to obtain highly dispersed nano copper. The specific morphology is as follows Figure 1 As shown by Figure 1 It can be seen that the nano copper particles are similar to spherical particles with uniform particle size, and the particle size is between 10-13nm.

[0053] Example 5

[0054] Into a 500mL three-necked flask, add 80mL of distilled water, 18mL of NH3·H2O, 0.016mol of ricinoleic acid amide prepared in Example 2, and 5mL of 80% (mass concentration, the same below) hydrazine hydrate in sequence, and stir until completely dissolved to obtain a mixed solution; add 0.032mol of CuSO4·5H2O to a beaker, and then add 100mL of distilled water and stir until completely dissolved to prepare a copper precursor aqueous solution; add the obtained copper precursor aqueous solution to the above mixed solution, heat to 60°C and react for 2h to obtain a dark red-brown nano-copper dispersion, which can be stably dispersed in water for a long time without coagulation. The obtained nano-copper dispersion is centrifuged, washed, and dried to obtain highly dispersed nano-copper. The specific morphology is as follows Figure 2 As shown by Figure 2 It can be seen that the nano copper particles are similar to spherical particles with uniform particle size, and the particle size is between 10-20nm.

[0055] Example 6

[0056] Into a 500mL three-necked flask, add 80mL of distilled water, 18mL of NH3·H2O, 0.016mol of castor oil-based quaternary ammonium salt prepared in Example 3, and 5mL of 80% (mass concentration, the same below) hydrazine hydrate in sequence, and stir until completely dissolved to obtain a mixed solution; add 0.032mol of CuSO4·5H2O to a beaker, and then add 100mL of distilled water and stir until completely dissolved to prepare a copper precursor aqueous solution; add the obtained copper precursor aqueous solution to the above mixed solution, heat to 70°C and react for 2h to obtain a dark red-brown nano-copper dispersion, which can be stably dispersed in water for a long time without coagulation. The obtained nano-copper dispersion is centrifuged, washed, and dried to obtain highly dispersed nano-copper. The specific morphology is as follows Figure 3 As shown by Figure 3 It can be seen that the nano copper particles are similar to spherical particles with uniform particle size, and the particle size is between 20-30nm.

[0057] Comparative Example 1

[0058] Add 80mL of distilled water, 18mL of NH3·H2O, 0.016mol of adipic acid, and 5mL of 80% (mass concentration, the same below) hydrazine hydrate to a 500mL three-necked flask in sequence, and stir until completely dissolved to obtain a mixed solution; add 0.032mol of CuSO4·5H2O to a beaker, and then add 100mL of distilled water and stir until completely dissolved to prepare a copper precursor aqueous solution; add the obtained copper precursor aqueous solution to the above mixed solution, heat to 80°C and react for 2h to obtain a dark red-brown nano-copper dispersion, which can be stably dispersed in water for a long time without coagulation. The obtained nano-copper dispersion is centrifuged, washed, and dried to obtain nano-copper. The specific morphology is as follows Figure 4 As shown by Figure 4 It can be seen that the nano copper particles are similar to spherical particles, and the particle size is not uniform, and the particle size is between 5-30nm.

[0059] Example 7

[0060] The nano copper in Examples 4-6 and Comparative Example 1 can be mixed with water, and completely dissolved after mixing, with good dispersibility. The nano copper prepared in Examples 4-6 and Comparative Example 1 were dispersed in water to prepare nano copper dispersions with a concentration of 4% nano copper, which were added to a coal combustion furnace in sequence, and then crushed coal was added to conduct a furnace test. Under the coal combustion furnace, the nitrogen oxide emissions are as follows.

[0061] Table 1 Nitrogen oxide emissions of different types of nano copper and added amounts

[0062]

[0063] As shown in Table 1, when the nano copper in Example 4 is added to the coal combustion furnace, compared with before the addition, the nitrogen oxide emissions are less than 10ppm, which can effectively reduce the emission of nitrogen oxides in the carbon combustion process; under the same nano copper situation, with the increase of the amount of nano copper added, the nitrogen oxide emissions show a trend of first decreasing and then increasing, and the emission reduction effect is best when the nano copper concentration is 20-30ppm. In addition, when the nano copper in Examples 5 and 6 is added to the coal combustion furnace, when the nano copper concentration is 20-30ppm, it also has a good emission reduction effect. When the nano copper in Comparative Example 1 is added, the nitrogen oxide emissions are greater than 45ppm, and the emission reduction effect is obviously not good. It can be seen from this that the nano copper prepared by the compound shown in Formula I, ricinoleic acid amide or castor oil-based quaternary ammonium salt as a surface modifier in the present invention is used as a catalyst in the coal combustion process, which can make the coal combustion more complete, improve the coal combustion efficiency, and effectively reduce the emission of nitrogen oxides in the carbon combustion process, and the nitrogen oxide emissions are less than 10ppm.

[0064] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that it is still possible to modify the technical solutions described in the aforementioned embodiments, or to perform equivalent replacements on some of the technical features therein. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing water-soluble highly dispersed nano copper, characterized in that: The method comprises the following steps: uniformly mixing a reducing agent, a surface modifier, a pH regulator and a solvent, adding a copper precursor aqueous solution to the obtained mixed solution, and performing a reduction reaction at 40-90° C. to obtain water-soluble highly dispersed nano copper; the surface modifier is a compound shown in formula I, ricinoleic acid amide or castor oil-based quaternary ammonium salt, wherein the structural formula of the compound shown in formula I is as follows:

2. The method for preparing water-soluble highly dispersed nano copper according to claim 1, characterized in that: The copper precursor is one or more of copper sulfate, copper chloride, copper nitrate or copper acetate; the concentration of the copper precursor aqueous solution is 0.1-1 mol / L.

3. The method for preparing water-soluble highly dispersed nano copper according to claim 1, characterized in that: The reducing agent is one or more of formaldehyde, sodium borohydride, sodium hypophosphite, hydrazine hydrate or ascorbic acid; and the reaction temperature is 60-80°C.

4. The method for preparing water-soluble highly dispersed nano copper according to claim 1, characterized in that: The molar ratio of the copper precursor, the reducing agent and the surface modifier is 1:1.5-3.5:0.1-1.5, preferably 1:2.0-3.0:0.4-0.8, and more preferably 1:2.5:0.5; the concentration of the reducing agent in the obtained mixed solution is 0.2-2 mol / L; the concentration of the reducing agent in the obtained mixed solution is 0.02-1 mol / L.

5. The method for preparing water-soluble highly dispersed nano copper according to claim 1, characterized in that: The pH regulator is one or more of sodium hydroxide, ammonia water, ethylenediamine, diethylamine or triethanolamine; the solvent is water, anhydrous ethanol or ethanol aqueous solution.

6. The water-soluble highly dispersed nano copper obtained by the preparation method according to any one of claims 1 to 5 has a concentration of not less than 10%.

7. Use of the water-soluble highly dispersed nano copper described in claim 1 as a catalyst in the process of coal combustion.

8. The use according to claim 1, characterized in that: The water-soluble highly dispersed nano copper stock solution is dissolved in a water pool and added into the crushed coal.

9. The use according to claim 1, characterized in that: The concentration control range of the water-soluble highly dispersed nano copper dispersed in the water pool is: 0.14-1.4%.