Preparation method and feeding device of blast furnace charging material

By utilizing the low-temperature sensible heat and mixing technology of the intermediate bin in the blast furnace charge preparation method, the problem of incomplete screening of lump ore is solved, the screening efficiency and mixing effect are significantly improved, and the stability of blast furnace production is ensured.

CN118773387APending Publication Date: 2024-10-15SHANDONG IRON & STEEL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411104356.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the blast furnace smelting process, the lump ore is not completely screened due to moisture, causing the materials entering the furnace to be unqualified and affecting the production rhythm. The existing technical improvement measures are not effective.

Method used

By adding an intermediate bin to the blast furnace charging method, the low-temperature sensible heat of sinter and pellets is used to dry the wet sticky lumps, and the sinter, pellets and lumps are mixed in the intermediate bin to ensure full mixing and transfer. heat to improve screening efficiency.

Benefits of technology

It effectively solves the problem of difficult screening of wet and sticky lumps, improves the screening efficiency and mixing effect of lumps, and ensures the quality of the furnace materials and the stability of blast furnace production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773387A_ABST
    Figure CN118773387A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of blast furnace ironmaking, and particularly provides a blast furnace charging material preparation method and a feeding device, an intermediate bin is additionally arranged between a mineral aggregate sub-bin and a screening device, so that sintered ores, pellets and lump ores used by a blast furnace are knocked into the intermediate bin according to a preset proportion to be mixed, heat of sintering and the pellets is fully utilized, and the production efficiency is improved. The wet sticky lump ore is preheated, so that the mixed ore is convenient to screen when being discharged from the middle bin, and the lump ore adding amount and the feeding rhythm are prevented from being influenced; and the problem that sintered ore, pellets and lump ore are difficult to fully mix can also be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of blast furnace ironmaking, and in particular to a material preparation method and a material feeding device for blast furnace charging. Background Art

[0002] Sintered ore, pellets and lump ore are the main raw materials for wet blast furnace ironmaking. Lump ore is a natural ore that has not been artificially enriched and beneficiated, and generally contains about 60% iron. With the deepening of smelting cost reduction and efficiency improvement, the proportion of lump ore is getting higher and higher. In the blast furnace smelting process, the lump ore is conveyed to the blast furnace trough by a belt for screening. The screened material is the raw material that meets the furnace standard. Sintered ore, pellets, coke, solvents, etc. are added in proportion, and the screened material can be used as the raw material of sintered ore. However, the lump ore contains high powder and is moist. The moist and powdery lump ore is very easy to clog the sieve holes during the screening process. The screening is not thorough, resulting in unqualified materials entering the furnace, affecting the amount of lump ore added and the blast furnace production rhythm.

[0003] In the prior art, the screening device is usually improved to avoid the lump ore sticking to the screen. For example, Chinese patent CN111375541A provides a screening system for wet powder-containing lump ore. By installing an elastic component at the input end of the vibrating screen, when the vibrating screen stops running, the elastic component will be in a static state without external force, and the lump ore will stay on the diversion component, which can avoid the accumulation of the lump ore on the vibrating screen, thereby reducing the screening difficulty of the vibrating screen, but the improvement of the lump ore screening efficiency is not obvious.

[0004] In order to improve the screening efficiency of lump ore from the source, Chinese patent CN116571431A discloses a screening method for lump ore with high powder rate and high moisture content. By laying high-temperature pellets and lump ore on a conveyor belt, the evaporation of moisture in the lump ore is promoted and the screening efficiency of the lump ore is improved. However, the drying time of the pellets and lump ore on the conveyor belt is too short, and the drying effect on the lump ore is not obvious. Summary of the invention

[0005] In order to solve the problem of effective screening of wet and sticky lumps and avoid affecting the amount of lumps added, the present invention provides a method for preparing blast furnace feed and a feeding device. By adding an intermediate bin, the low-temperature sensible heat of sintered ore and pellets is fully utilized to dry the wet and sticky lumps, so that the lumps can be effectively screened.

[0006] A method for preparing a blast furnace charge comprises the following steps:

[0007] Step 1: Measure the theoretical screening index of sintered ore, pellets and lump ore respectively: S 烧 , S 球 , S 块 ;

[0008] Step 2: Determine the mass P of the ore batch into the blast furnace, as well as the mass percentage X of the sintered ore, pellets and lump ore into the furnace.烧 , X 球 and X 块 ;

[0009] Step 3: According to the mass ratio of sintered ore, pellets and lump ore, Feed the middle warehouse;

[0010] Step 4: Sintered ore, pellets and lump ore are mixed in the intermediate bin, screened and transported to the blast furnace for feeding.

[0011] In step 1, the theoretical screening index is expressed as the percentage of the sample amount smaller than the specified particle size to the total sample amount.

[0012] The theoretical screening index is measured by shaking the sample back and forth with a shaking sieve with a sieve hole of a specified particle size, and calculating the theoretical screening index based on the output of particles smaller than the specified particle size. The lump ore needs to be dried until it is no longer sticky before measuring the theoretical screening index.

[0013] Preferably, the specified particle size is 4-6 mm.

[0014] In step 2, X 烧 +X 球 +X 块 =1.

[0015] In step 3, the sintered ore and pellets are produced in the factory to retain the waste heat of the sintered ore and pellets, and the temperature is controlled at 70-150°C when entering the intermediate warehouse.

[0016] In step 4, the residence time of the sintered ore, pellets and lump ore in the intermediate bin is greater than 30 minutes.

[0017] The sintered ore, pellets and lump ore are added into the intermediate bin at the same time to ensure the sufficient mixing and heat transfer of the sintered ore, pellets and lump ore.

[0018] The present invention also provides a feeding device for blast furnace charge, comprising a ore storage bin, an intermediate bin, and a screening device;

[0019] The ore storage bins include: sintering bin, pelletizing bin and lump ore bin, which are used to store sintered ore, pellets and lump ore respectively;

[0020] The intermediate bin is used for mixing mineral materials.

[0021] The intermediate bin body is evenly provided with exhaust holes for exhausting water vapor in the intermediate bin.

[0022] The size of the intermediate bin must meet the requirement that the residence time of the mixed material is greater than 30 minutes. That is, if the batch distribution cycle time of the blast furnace is Tmin, the size of the intermediate bin must accommodate more than Ore volume;

[0023] The p is the batch capacity of the mine, m 3 .

[0024] The screening device is a vibrating screen;

[0025] Preferably, the screening method is a bar screen with high throughput; more preferably, the spacing of the screening bars is 4-6 mm.

[0026] The advantages of the present invention are:

[0027] By adding an intermediate bin before loading, mixing sintered ore, pellets and lump ore, not only can the low-temperature sensible heat of sintered ore and pellets be effectively utilized in a confined space to solve the problem of difficulty in screening wet and sticky lump ore, but also the problem of difficulty in fully mixing sintered ore, pellets and lump ore can be solved by mixing them in advance before entering the furnace. In addition, the present invention fully considers the screening index of sintered ore, pellets and lump ore themselves, and can adjust the addition amount of each component in real time according to the change of blast furnace batching. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of a method for preparing charging materials into a blast furnace in an embodiment of the present invention. DETAILED DESCRIPTION

[0029] The present invention will be further described below with reference to the accompanying drawings and embodiments, but is not limited thereto.

[0030] Embodiment 1:

[0031] A feeding device for blast furnace charging includes a ore storage bin, an intermediate bin, and a screening device; wherein the ore storage bins include a sintering bin, a pellet bin, and a lump bin, which are respectively used to store sintered ore, pellets, and lump ore; and the intermediate bin is used to mix ore.

[0032] The intermediate warehouse is evenly provided with exhaust holes, and the ore batch capacity is 36m 3 , the batch loading cycle is 10min, and the size of the intermediate bin is 150m 3 .

[0033] The screening device is a bar screen; the spacing between the screening bars is 5 mm.

[0034] 1880m 3 Taking the actual production of blast furnace as an example, when entering the intermediate bin, the temperature of sintered ore in the blast furnace bin is controlled at 80℃, and the temperature of pellets is controlled at 85℃. The blast furnace ore batch is 67 tons, the theoretical screening index of sintered ore is 4%, the theoretical screening index of pellets is 3.5%, and the theoretical screening index of lump ore is 10%. The mass ratio of sintered ore, pellets and lump ore entering the furnace is determined to be 7:1:2, and the mass ratio of sintered ore, pellets and lump ore entering the intermediate bin is controlled to be 49:7:15 for charging.

[0035] The screening index is measured as follows: after drying the lump ore at 105°C, the sintered ore, pellets and lump ore are reciprocated 10 times using a shaking sieve with a sieve hole of 5mm×5mm, and the screening index is calculated based on the output of less than 5mm.

[0036] like Figure 1 As shown, sintered ore, pellets, and lump ore are charged to the intermediate bin at a mass ratio of 49:7:15 from the sintering bin, pellet bin, and lump bin, respectively, and then screened with bars, with a bar spacing of 5 mm. After screening, the ore with a particle size smaller than 5 mm is returned to the sintering, and the ore with a particle size larger than 5 mm is fed into the blast furnace with the feeding belt.

[0037] When the material is discharged from the intermediate bin for screening, the material temperature is about 50°C, the mixing effect is good, there is no sticking, and the screening effect is good. As shown in Table 1, the screening efficiency of sintered ore, pellets, lump ore and their mixtures before and after passing through the intermediate bin. By comparing before and after, it can be seen that due to the wet stickiness of the lump ore, the screen is blocked, the screening effect is extremely poor, and the screening efficiency is only 20%. Through mixing, using the waste heat of sintered ore and pellets, the wet sticky lump ore is dried, and the screening efficiency of the mixture is 91.1%, and the mixing effect is good.

[0038] Table 1 Screening efficiency of sintered ore, pellets, lump ore and their mixtures before and after passing through the intermediate bin

[0039]

[0040] Embodiment 2:

[0041] A feeding device for blast furnace charging includes a ore storage bin, an intermediate bin, and a screening device; wherein the ore storage bins include a sintering bin, a pellet bin, and a lump bin, which are respectively used to store sintered ore, pellets, and lump ore; and the intermediate bin is used to mix ore.

[0042] The intermediate warehouse is evenly provided with exhaust holes, and the ore batch capacity is 33m 3 , the batch loading cycle is 10min, and the size of the intermediate bin is 150m 3 .

[0043] The screening device is a bar screen; the spacing between the screening bars is 5 mm.

[0044] 1880m 3 Taking the actual production of blast furnace as an example, when entering the intermediate bin, the temperature of sintered ore in the blast furnace bin is controlled at 90℃, and the temperature of pellets is controlled at 80℃. The blast furnace ore batch is 60 tons, the theoretical screening index of sintered ore is 4%, the theoretical screening index of pellets is 3.5%, and the theoretical screening index of lump ore is 11%. The mass ratio of sintered ore, pellets and lump ore entering the furnace is determined to be 7:1:2, and the mass ratio of sintered ore, pellets and lump ore entering the intermediate bin is controlled to be 44:6:13 for charging.

[0045] The screening index is measured as follows: after drying the lump ore at 105°C, the sintered ore, pellets and lump ore are reciprocated 10 times using a shaking sieve with a sieve hole of 5mm×5mm, and the screening index is calculated based on the output of less than 5mm.

[0046] When the material is discharged from the intermediate bin for screening, the material temperature is about 60°C, the mixing effect is good, there is no sticking, and the screening effect is good. Table 2 shows the screening efficiency of sintered ore, pellets, lump ore and their mixtures before and after passing through the intermediate bin. By comparing before and after, it can be seen that due to the wet stickiness of the lump ore, the screen is blocked, the screening effect is extremely poor, and the screening efficiency is only 18.2%. Through mixing, using the waste heat of sintered ore and pellets, the wet sticky lump ore is dried, and the screening efficiency of the mixture is 91.3%, and the mixing effect is good.

[0047] Table 2 Screening efficiency of sintered ore, pellets, lump ore and their mixtures before and after passing through the intermediate bin

[0048]

[0049] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the embodiments, it should be understood by those skilled in the art that any modification or equivalent replacement of the technical solutions of the present invention does not depart from the spirit and scope of the technical solutions of the present invention and should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing blast furnace charge, characterized in that: The steps include: Step 1: Measure the theoretical screening index of sintered ore, pellets and lump ore respectively: S 烧 , S 球 , S 块 ; Step 2: Determine the mass P of the ore batch into the blast furnace, as well as the mass percentage X of the sintered ore, pellets and lump ore into the furnace. 烧 , X 球 and X 块 ; Step 3: Sintered ore, pellets and lump ore flow The mass ratio is the same as that of the intermediate bin at the same time; Step 4: Sintered ore, pellets and lump ore are mixed in the intermediate bin, screened and transported to the blast furnace for feeding.

2. The method for preparing blast furnace charge according to claim 1, characterized in that: The theoretical screening index is expressed as the percentage of the sample volume smaller than the specified particle size to the total sample volume; Preferably, the specified particle size is 4-6 mm.

3. The method for preparing blast furnace charge according to claim 1, characterized in that: X 烧 +X 球 +X 块 =1。 4. The method for preparing blast furnace charge according to claim 1, characterized in that: The temperature of the sintered ore and pellets is controlled at 70-150°C when entering the intermediate bin.

5. The method for preparing blast furnace charge according to claim 1, characterized in that: The residence time of the sintered ore, pellets and lump ore in the intermediate bin is greater than 30 minutes.

6. A feeding device for blast furnace charge, characterized in that: It includes mineral material storage bins, intermediate bins, and screening devices; The ore storage bins include: sintering bin, pelletizing bin and lump ore bin, which are used to store sintered ore, pellets and lump ore respectively; The intermediate bin is used for mixing mineral materials.

7. The feeding device for blast furnace charge according to claim 6, characterized in that: The middle warehouse body is provided with an exhaust hole.

8. The feeding device for blast furnace charge according to claim 6, characterized in that: The size of the intermediate warehouse needs to accommodate more than Mineral volume, Where T is the blast furnace batch distribution cycle time, min; p is the batch capacity, m 3 .

9. The feeding device for blast furnace charge according to claim 6, characterized in that: The screening device is a vibrating screen; Preferably, the screening method is a bar screen.

10. The feeding device for blast furnace charge according to claim 9, characterized in that: The rods of the rod screen are spaced 4-6 mm apart.

Citation Information

Patent Citations

  • Charging method for blast furnace burden

    CN101275172A

  • Screening treatment method for imported lump ores for iron smelting

    CN102658263A

  • Device and method for hot loading of metallized pellets of rotary hearth furnace into blast furnace

    CN102839244A

  • Material preparation and material charging method of blast furnace feeding materials

    CN108085441A

  • Integrated method and system for drying and screening lump ore through sintering waste heat

    CN113720167A