Cobalt-based high-temperature alloy powder for 3D printing as well as preparation method and application of cobalt-based high-temperature alloy powder
By optimizing the composition design and preparation process of cobalt-based superalloys, the problems of insufficient high-temperature mechanical properties, oxidation resistance, and hot corrosion resistance of cobalt-based superalloys have been solved, and the efficient application of cobalt-based superalloy powders in the aerospace field has been achieved. .
Patent Information
- Application Number
- CN202411280820.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-09-13
AI Technical Summary
It is difficult to develop cobalt-based high-temperature alloy powder suitable for large-scale industrial production and 3D printing processes with existing technology. Moreover, existing cobalt-based high-temperature alloys have deficiencies in high-temperature mechanical properties, oxidation resistance, and hot corrosion resistance, making it difficult to meet the needs of aerospace. high demands in the field.
By optimizing the composition design of cobalt-based high-temperature alloys, element ratios such as W(Ni): 8.5~12.5%, W(Cr): 22.5~27.5%, W(W): 6.0~8.0% are adopted, and vacuum melting and fogging are used. Cobalt-based high-temperature alloy powder is prepared through chemical milling, screening and drying processes, and combined with heat treatment technology, a uniformly distributed high-melting point compound is formed to improve the high-temperature temperature-bearing capacity and anti-oxidation performance of the alloy.
The high-temperature temperature-bearing capacity and high-temperature mechanical properties of the cobalt-based superalloy have been improved, while the oxidation resistance and high-temperature corrosion resistance have been improved, and the difficulty of smelting and the risk of stress cracking have been reduced. The high-temperature alloy specimens produced have good mechanical properties. and density.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to a cobalt-based high-temperature alloy powder for 3D printing, a preparation method and application thereof, and belongs to the technical field of metal materials. Background Art
[0002] At present, the high-temperature alloys widely used in aircraft engines and gas turbines are mainly nickel-based high-temperature alloys. However, the melting point of traditional nickel-based high-temperature alloys is limited, so the improvement of their temperature-bearing capacity is extremely limited. Therefore, the development of new high-temperature alloys with higher temperature-bearing capacity is an urgent need in this field.
[0003] Cobalt-based superalloys are a type of alloy that uses cobalt as the main element and adds a considerable amount of nickel, chromium, tungsten and a small amount of other elements to strengthen the matrix. Traditional cobalt-based superalloys rely on solid solution strengthening and carbide dispersion strengthening, lack strengthening phases similar to the γ′-Ni3Al phase (L12 structure) in nickel-based superalloys, have low high-temperature strength, and their applications are limited. In the early years, Japanese scholars discovered a new type of cobalt-based superalloy in the Co-Al-W series strengthened by an ordered γ′ phase, which has a significantly better strengthening effect than traditional cobalt-based superalloys and nickel-based alloys. However, the narrow γ / γ′ phase region, low high-temperature stability of the γ′ phase, and high alloy density limit the application of this alloy in the aerospace industry.
[0004] The organic combination of additive manufacturing technology and new cobalt-based high-temperature alloys can not only more conveniently manufacture more complex structural parts in aircraft engines, but also manufacture new cobalt-based high-temperature alloy parts with good heat resistance, wear resistance and corrosion resistance. At present, there are no public reports of cobalt-based high-temperature alloys for additive manufacturing with reasonable composition design, suitable for large-scale industrial preparation, and ideal high temperature bearing capacity, high temperature mechanical properties, high temperature oxidation resistance and hot corrosion resistance.
[0005] Therefore, based on the above research foundation and application status, it is urgently necessary to develop a new type of cobalt-based high-temperature alloy powder material suitable for large-scale industrial production and 3D printing process through reasonable composition design. This material can fully meet the requirements of high temperature bearing capacity, high temperature mechanical properties, high temperature oxidation resistance and thermal corrosion resistance in the aerospace field.
[0006] Existing technical solutions for high-temperature alloys mainly improve the high-temperature mechanical properties of alloys by controlling the composition. For example, Chinese patent application CN114032433A uses Ni, Ti, Al, Mo, rare earth metals and 3% to 6% of refractory metals Nb and Ta to replace the high-density element W, maintain the high high-temperature strength of the alloy, and achieve the purpose of lightweighting the alloy. However, the melting points of refractory metals niobium (melting point 2468°C) and tantalum (melting point 2996°C) are too high, and the melting points of the matrix elements Ni (melting point 1453°C) and Ti (melting point 1640°C) are too different, and the addition ratio is relatively high. Directly preparing the metal single material by the melting matching method is difficult to melt, which easily leads to the segregation of refractory metals in the powder. Chinese patent application CN117802387A discloses a high-chromium cobalt-nickel-based high-temperature alloy for additive manufacturing, involving 16 added elements, including: 0.005-0.5% of metal Hf. There are too many added elements, and the price of metal Hf is high, so the cost of industrial-scale preparation is high. In Chinese patent CN114015922B, the metal element powder is mixed to obtain alloy powder, and the final powder is obtained by screening and drying. The process is cumbersome, the production cost is high, and it is not conducive to large-scale industrial preparation. Similarly, there is also Chinese patent application CN117840417A, which prepares high-temperature alloy powder through multiple processes such as multi-element powder mixing, screening, and drying for nickel-based high-temperature alloy powder. The process is complicated, the cost is high, and it is not conducive to industrial production. In addition, its room temperature tensile strength is not less than 750Mpa, and the yield strength is not less than 450Mpa; at a high temperature of 800℃, the tensile strength is not less than 400Mpa, and this high-temperature mechanical property is low.
[0007] In addition, there are existing solutions for high-temperature alloys, such as: Chinese patent application CN115889808A, which uses three nickel-based high-temperature alloy powders, GH3536, GH3625, and GH4169, as raw materials. To address the problem of easy cracking during the printing and molding process of high-temperature alloys, the printing parameters are optimized and a second selective laser melting additive manufacturing molding process is added. The purpose of reducing the cracking of printed parts has been achieved, but the high-temperature mechanical properties of the alloy have not been significantly improved.
[0008] Oxidation resistance and thermal corrosion resistance are also important indicators for measuring the high-temperature performance of alloys. However, existing technologies mainly focus on improving the mechanical properties of cobalt-based high-temperature alloys and solving problems such as cracking during the printing process. There are few technologies for improving the high-temperature oxidation resistance and high-temperature corrosion resistance of cobalt-based high-temperature alloys. Summary of the invention
[0009] In view of the deficiencies in the prior art, the present invention provides a cobalt-based high-temperature alloy powder for 3D printing, a preparation method and an application thereof. The cobalt-based high-temperature alloy powder can improve the oxidation resistance and high-temperature corrosion resistance of the alloy while achieving alloy lightweighting, reducing smelting difficulty and reducing the risk of alloy stress cracking.
[0010] The technical solution of the present invention to solve the above technical problems is as follows: a cobalt-based high-temperature alloy powder for 3D printing, wherein the alloying elements in the cobalt-based high-temperature alloy powder are calculated by mass percentage as follows: W(Ni): 8.5-12.5%, W(Cr): 22.5-27.5%, W(W): 6.0-8.0%, W(C): 0-0.2%, W(Mo) + W(Ti) + W(Nb) + W(La) + W(Ta)+W(Al): 3.0-6.0%, W(Ti)+W(Al)<2.0%, wherein W(Mo): 0.5-1.0%, W(Al): 0.5-2.0%, W(Ti): 0.4-1.0%, W(Nb): 0.5-1.0%, W(La): 0.5-1.0%, W(Ta): 0.5-1.0%, and the remainder is Co.
[0011] Furthermore, the alloying elements in the cobalt-based high-temperature alloy powder are calculated by mass percentage as follows: W(Ni): 8.5~12.5%, W(Cr): 23~27%, W(W): 6.0~7.0%, W(C): 0-0.2%, W(Mo) + W(Ti) + W(Nb) + W(La) +W(Ta)+W(Al): 3.0~6.0%, W(Ti)+W(Al)<2.0%, wherein W(Mo): 0.5~1.0%, W(Al): 0.5~2.0%, W(Ti): 0.5~1.0%, W(Nb): 0.5~1.0%, W(La): 0.5~1.0%, W(Ta) 0.5~1.0%, and the balance is Co.
[0012] Further, W(Cr):W(Ni)=(2.4-2.6):1.
[0013] The present invention also discloses a method for preparing cobalt-based high-temperature alloy powder for 3D printing, the preparation method comprising: S1. Raw material smelting: heat and melt the pure metal and master alloy raw materials under vacuum conditions according to the formula; S2, atomization powder making: atomizing and powdering the smelted pre-alloyed metal using argon gas; S3, powder screening: the pre-alloyed metal powder prepared in step S2 is screened and graded under an inert gas protective atmosphere; S4, heat preservation and drying: drying the powder screened in step S3.
[0014] Furthermore, in step S1, Nb, Ta, Mo and W metal elements are fed in the form of raw materials of intermediate alloy.
[0015] Furthermore, in step S1, when the raw materials are smelted, a step-by-step power increase method is adopted, with a power span of 10-30Kw, each power stage is maintained for 10-30min, and sufficient stirring is maintained during the smelting process.
[0016] The smelting temperature is 1650-1700° C., and the smelting time is 10-40 minutes.
[0017] Furthermore, in step S2, the atomization gas pressure of atomization powder making is 4.0-5.0 MPa.
[0018] Furthermore, in step S3, the pressure of the inert gas protective atmosphere is 0.05-0.95 MPa, and the particle size range of the powder after screening is 15-53 μm.
[0019] The present invention also discloses an application of cobalt-based high-temperature alloy powder for 3D printing, and the cobalt-based high-temperature alloy powder is applied to 3D printing.
[0020] Furthermore, the 3D printed specimens were heat treated at a temperature of 300-400°C for 1-3 hours. After the heat treatment was completed, the temperature was further raised to 800-1000°C for 2-8 hours. The specimens were cooled in the furnace to obtain 3D printed specimens.
[0021] The beneficial effects of the present invention are: The cobalt-based high-temperature alloy powder for 3D printing of the present invention has good high-temperature bearing capacity and high-temperature mechanical properties, as well as good oxidation resistance and high-temperature corrosion resistance. This technology mainly adds three alloy elements of nickel, chromium and tungsten, supplemented by a small amount of alloy elements such as molybdenum, niobium, tantalum, titanium and rare earth metal lanthanum, and optimizes the composition to form a uniformly distributed high-melting point compound in the alloy, and increase the volume fraction of the γ′ phase in the alloy, thereby achieving the improvement of the temperature bearing capacity and high-temperature mechanical properties of the cobalt-based high-temperature alloy. And by adding a higher proportion of Cr and Ni elements, the two play a synergistic role. The Cr element forms a dense Cr2O3 oxide layer on the surface of the alloy to block the diffusion of O into the matrix, thereby improving the oxidation resistance of the alloy. The Ni element can promote the growth of Cr2O3 and delay the nodular oxidation of the alloy, thereby improving the oxidation resistance and high-temperature corrosion resistance of the alloy. At the same time, Cr and Ni elements can replace a considerable part of tungsten elements, which greatly reduces the addition of high-density tungsten elements relative to traditional cobalt-based alloys, and effectively plays the role of lightweighting the alloy. The addition of Ta has also been proven to improve the hot corrosion resistance of the alloy to a certain extent.
[0022] The present invention adopts the method of feeding low-melting-point intermediate alloys for high-melting-point insoluble metals such as niobium, tantalum and tungsten, thereby reducing the difficulty of metal melting, facilitating smelting and diffusion, and greatly reducing the difficulty of smelting the component alloys and the risk of component segregation in the final cobalt-based high-temperature alloy powder.
[0023] The present invention rationally designs the content of alloying elements by applying the grain boundary segregation engineering theory, and adds an appropriate amount of aluminum element W (Al): 0.5-2.0%. During the solidification process of the alloy, the solubility of aluminum decreases as the temperature decreases, causing the aluminum element to be enriched at the branch grain boundaries and grain boundaries, thereby promoting the formation of a continuous liquid phase film. At the same time, the continuous shrinkage of the matrix will generate large residual stresses at the branch grain boundaries and grain boundaries. As the temperature further decreases, the B2 phase gradually precipitates at the branch grain boundaries and grain boundaries, and gradually undergoes spinodal decomposition, decomposing into island B2 phases and Cr-rich BCC phases. The phase change behavior caused by spinodal decomposition will promote molar volume expansion, and the asymmetric distribution of the intermetallic compound phase will introduce more geometric dislocations. The stress fields generated by the two aspects can jointly offset part of the residual tensile stress, change the residual stress distribution state at the dendrite boundaries and grain boundaries, and even change from a tensile stress state to a compressive stress state, thereby effectively inhibiting the cracking behavior of the alloy.
[0024] At the same time, please note that the Al and Ti contents should satisfy W(Ti): 0.5~1.0%, W(Ti)+W(Al)<2.0%. Prevent excessive Al and Ti contents from causing alloy strength to decrease.
[0025] In addition, combined with the optimization of the smelting process, the uniform distribution of the γ′ strengthening phase in the cobalt-based high-temperature alloy is achieved, and the uniform distribution of the fine dispersed MoC strengthening phase in the cobalt-based high-temperature alloy is achieved, which has a uniform dispersion effect on the internal stress generated in the printing process, thereby reducing the risk of stress cracking. The high-temperature alloy specimens made from the cobalt-based high-temperature alloy powder of the present invention have no cracks and the density is over 99%.
[0026] The high-temperature alloy specimens made from the cobalt-based high-temperature alloy powder of the present invention have excellent mechanical properties: room temperature tensile strength ≥1650 MPa, elongation after fracture ≥10%; tensile strength at 820°C ≥580 MPa, elongation after fracture ≥20%; initial stress at 820°C is 205 MPa, high-temperature creep rupture time is greater than 60h, and high-temperature creep elongation after fracture is <3%. DETAILED DESCRIPTION
[0027] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0029] A cobalt-based high-temperature alloy powder for 3D printing, wherein the alloy elements in the cobalt-based high-temperature alloy powder are calculated by mass percentage as follows: W(Ni): 8.5-12.5%, W(Cr): 22.5-27.5%, W(W): 6.0-8.0%, W(C): 0-0.2%, W(Mo) + W(Ti) + W(Nb) + W(La) + W(Ta)+W(Al): 3.0-6.0%, W(Ti)+W(Al)<2.0%, wherein W(Mo): 0.5-1.0%, W(Al): 0.5-2.0%, W(Ti): 0.4-1.0%, W(Nb): 0.5-1.0%, W(La): 0.5-1.0%, W(Ta): 0.5-1.0%, and the balance is Co.
[0030] Specifically, the alloying elements in the cobalt-based high-temperature alloy powder are calculated by mass percentage as follows: W(Ni): 8.5~12.5%, W(Cr): 23~27%, W(W): 6.0~7.0%, W(C): 0-0.2%, W(Mo) + W(Ti) + W(Nb) + W(La) +W(Ta)+W(Al): 3.0~6.0%, W(Ti)+W(Al)<2.0%, wherein W(Mo): 0.5~1.0%, W(Al): 0.5~2.0%, W(Ti): 0.5~1.0%, W(Nb): 0.5~1.0%, W(La): 0.5~1.0%, W(Ta) 0.5~1.0%, and the balance is Co.
[0031] Specifically, W(Cr):W(Ni)=(2.4-2.6):1. Under this ratio, the 3D printed alloy has the best high-temperature oxidation resistance. In the atmospheric environment, a dense and thin oxide film will be formed on the surface during high-temperature use (600~800℃) to prevent further oxidation, and the alloy can maintain good high-temperature mechanical properties.
[0032] Specifically, W(Al): 0.5~2.0%, W(Ti): 0.5~1.0%, W(Ti)+W(Al)<2.0%. Within this range, the 3D printed alloy has the best anti-cracking effect, and the possibility of cracking of the printed parts can be minimized from the printing deposition forming process to the subsequent heat treatment and mechanical processing process. It can also effectively balance the internal stress of the printed parts and greatly reduce the degree of deformation caused by the heat treatment process.
[0033] A method for preparing cobalt-based high-temperature alloy powder for 3D printing, the preparation method comprising: S1. Raw material smelting: heat and melt the pure metal and master alloy raw materials under vacuum conditions according to the formula; S2, atomization powder making: atomizing and powdering the smelted pre-alloyed metal using argon gas; S3, powder screening: the pre-alloyed metal powder prepared in step S2 is screened and graded under an inert gas protective atmosphere; S4, heat preservation and drying: drying the powder screened in step S3.
[0034] Specifically, in step S1, Nb, Ta, Mo and W metal elements are fed in the form of raw materials of master alloy.
[0035] More specifically, this technology adopts the method of adding low melting point intermediate alloys to high melting point insoluble metals such as Nb (melting point 2477℃), Ta (melting point 2996℃), Mo (melting point 2620℃) and W (melting point 3410℃), such as: adding Nb element, using NiNb 65 Master alloy (melting point 1320℃); W element added, using CoW 20 Master alloy (melting point 1680℃); Ta element added, using NiTa 30 Master alloy (melting point about 1400℃); Mo element added, using NiMo 28 Intermediate alloy (melting point is about 1380℃). The above 4 intermediate alloys are all mature metal products, which are easy to purchase in the market. Compared with the single metals of Nb, Ta, Mo and W, their melting points are greatly reduced to about 50% and are relatively close, which greatly reduces the difficulty of smelting the component alloys. Combined with the equal power maintenance smelting process-a step-by-step power increase method is adopted, with a power span of 10-30Kw, and each power stage is maintained for 10-30min to ensure that the molten metal is fully electromagnetically stirred. According to the actual situation, mechanical stirring is added when necessary, which is conducive to the control of the smelting process and the diffusion of alloy elements, and ultimately greatly reduces the risk of component segregation in the final high-temperature alloy powder. In the end, the alloy powder has a uniform composition, and there are no refractory metal particles or high melting point intermediate phase particles.
[0036] Specifically, in step S1, the smelting temperature is 1650-1700° C., and the smelting time is 10-40 minutes.
[0037] Specifically, in step S2, the atomization gas pressure of atomization powder making is 4.0-5.0 MPa.
[0038] Specifically, in step S3, the pressure of the inert gas protective atmosphere is 0.05-0.95 MPa, and the particle size range of the powder after screening is 15-53 μm.
[0039] An application of cobalt-based high-temperature alloy powder for 3D printing, wherein the cobalt-based high-temperature alloy powder is applied to 3D printing.
[0040] Specifically, the 3D printed specimen is heat treated at a temperature of 300-400° C. for 1-3 hours. After the heat treatment is completed, the temperature is further raised to 800-1000° C. for 2-8 hours, and the specimen is cooled in the furnace to obtain a 3D printed specimen.
[0041] Example 1 The chemical composition (mass fraction) of a cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10%, W(Cr): 25%, W(W): 7.5%, W(C): 0.2%, W(Mo): 0.5%, W(Al): 0.5%, W(Ti): 0.5%, W(Nb): 1.0%, W(La): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0042] The preparation method of the cobalt-based high-temperature alloy powder for 3D printing is: S1. Raw material smelting: Heat and melt the pure metal and intermediate alloy raw materials under vacuum conditions according to the formula.
[0043] Adding Nb element, using NiNb 65 Master alloy; W element added, using CoW 20 Master alloy; Ta element added, using NiTa 30 Master alloy; Mo element added, using NiMo 28 Master alloy.
[0044] Mechanical stirring is used during the smelting process, and a step-by-step power increase method (power span is 10-30Kw) is adopted: maintain the power at 10Kw for 10 minutes; maintain the power at 20Kw for 20 minutes; and finally melt at 1680℃ for 30 minutes.
[0045] S2. Atomization powder making: The smelted pre-alloyed metal is atomized and powdered using argon gas; the atomization gas pressure of the atomization powder making is 4.5 MPa.
[0046] S3, powder screening: the pre-alloyed metal powder prepared in step S2 is screened and graded under a nitrogen protective atmosphere; the pressure of the nitrogen protective atmosphere is 0.6 MPa, and the particle size range of the powder after screening is 15 to 53 μm.
[0047] S4, heat preservation and drying: drying the powder screened in step S3 at a drying temperature of 120° C. for 4 hours to obtain a cobalt-based high-temperature alloy powder.
[0048] Cobalt-based high-temperature alloy powder was used for 3D printing, where the 3D printing conditions were: scanning power 250 W, scanning speed 950 mm / s, scanning spacing 0.09 mm, and layer thickness 0.03 mm.
[0049] The 3D printed alloy specimen was heat treated at 350°C for 2 hours. After the insulation was completed, the temperature was continued to rise to 900°C for 5 hours and cooled with the furnace to obtain a 3D printed specimen.
[0050] Example 2 The chemical composition (mass fraction) of a cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10.5%, W(Cr): 26%, W(W): 7%, W(C): 0.15%, W(Mo): 1.0%, W(Al): 0.5%, W(Ti): 1.0%, W(Nb): 1.0%, W(La): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0051] The preparation method of the cobalt-based high-temperature alloy powder for 3D printing is: S1. Raw material smelting: Heat and melt the pure metal and intermediate alloy raw materials under vacuum conditions according to the formula.
[0052] Adding Nb element, using NiNb 65 Master alloy; W element added, using CoW 20 Master alloy; Ta element added, using NiTa 30 Master alloy; Mo element added, using NiMo 28 Master alloy.
[0053] Mechanical stirring is used during the smelting process, and a step-by-step power increase method (power span is 10-30Kw) is adopted: maintain the power at 10Kw for 10 minutes; maintain the power at 20Kw for 10 minutes; maintain the power at 30Kw for 10 minutes; and finally melt at 1700℃ for 10 minutes.
[0054] S2. Atomization powder making: The smelted pre-alloyed metal is atomized and powdered using argon gas; the atomization gas pressure of the atomization powder making is 5 MPa.
[0055] S3, powder screening: the pre-alloyed metal powder prepared in step S2 is screened and graded under a nitrogen protective atmosphere; the pressure of the nitrogen protective atmosphere is 0.05 MPa, and the powder particle size range after screening is 15 to 53 μm.
[0056] S4, heat preservation and drying: drying the powder screened in step S3 at a drying temperature of 120° C. for 4 hours to obtain a cobalt-based high-temperature alloy powder.
[0057] Cobalt-based high-temperature alloy powder was used for 3D printing, where the 3D printing conditions were: scanning power 250 W, scanning speed 950 mm / s, scanning spacing 0.09 mm, and layer thickness 0.03 mm.
[0058] The 3D printed alloy specimen was heat treated at 300°C for 3 hours. After the insulation was completed, the temperature was continued to rise to 800°C for 8 hours and cooled with the furnace to obtain the 3D printed specimen.
[0059] Example 3 The chemical composition (mass fraction) of a cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 11.0%, W(Cr): 27.5%, W(W): 8.0%, W(C): 0.1%, W(Mo): 0.5%, W(Al): 1.0%, W(Ti): 0.5%, W(Nb): 0.5%, W(La): 0.5%, W(Ta): 1.0%, and the balance is Co.
[0060] The preparation method of the cobalt-based high-temperature alloy powder for 3D printing is: S1. Raw material smelting: Heat and melt the pure metal and intermediate alloy raw materials under vacuum conditions according to the formula.
[0061] Adding Nb element, using NiNb 65 Master alloy; W element added, using CoW 20 Master alloy; Ta element added, using NiTa 30 Master alloy; Mo element added, using NiMo 28 Master alloy.
[0062] During the smelting process, sufficient electromagnetic stirring is used, and a step-by-step power increase method (power span is 10-30Kw) is adopted: keep the power at 10 Kw for 10 minutes; keep the power at 20 Kw for 10 minutes; keep the power at 30 Kw for 10 minutes; finally, melt at 1650℃ for 40 minutes.
[0063] S2. Atomization powder making: The smelted pre-alloyed metal is atomized and powdered using argon gas; the atomization gas pressure of the atomization powder making is 4Mpa.
[0064] S3, powder screening: the pre-alloyed metal powder prepared in step S2 is screened and graded under a nitrogen protective atmosphere; the pressure of the nitrogen protective atmosphere is 0.95 MPa, and the particle size range of the powder after screening is 15 to 53 μm.
[0065] S4, heat preservation and drying: drying the powder screened in step S3 at a drying temperature of 120° C. for 4 hours to obtain a cobalt-based high-temperature alloy powder.
[0066] Cobalt-based high-temperature alloy powder was used for 3D printing, where the 3D printing conditions were: scanning power 250 W, scanning speed 950 mm / s, scanning spacing 0.09 mm, and layer thickness 0.03 mm.
[0067] The 3D printed alloy specimen was heat treated at 400°C for 1 hour. After the insulation was completed, the temperature was continued to rise to 1000°C for 2 hours and cooled with the furnace to obtain a 3D printed specimen.
[0068] Example 4 The chemical composition (mass fraction) of a cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 9.5%, W(Cr): 24.5%, W(W): 7.0%, W(C): 0.1%, W(Mo): 0.5%, W(Al): 1.5%, W(Ti): 0.4%, W(Nb): 1.0%, W(La): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0069] The preparation method of the cobalt-based high-temperature alloy powder for 3D printing is: S1. Raw material smelting: Heat and melt the pure metal and intermediate alloy raw materials under vacuum conditions according to the formula.
[0070] Adding Nb element, using NiNb 65 Master alloy; W element added, using CoW 20 Master alloy; Ta element added, using NiTa 30 Master alloy; Mo element added, using NiMo 28 Master alloy.
[0071] Mechanical stirring is used during the smelting process, and a step-by-step power increase method (power span is 10-30Kw) is adopted: maintain the power at 10Kw for 10 minutes; maintain the power at 20Kw for 10 minutes; maintain the power at 30Kw for 10 minutes; and finally melt at 1700℃ for 20 minutes.
[0072] S2. Atomization powder making: The smelted pre-alloyed metal is atomized and powdered using argon gas; the atomization gas pressure of the atomization powder making is 5 MPa.
[0073] S3, powder screening: the pre-alloyed metal powder prepared in step S2 is screened and graded under a nitrogen protective atmosphere; the pressure of the nitrogen protective atmosphere is 0.6 MPa, and the particle size range of the powder after screening is 15 to 53 μm.
[0074] S4, heat preservation and drying: drying the powder screened in step S3 at a drying temperature of 120° C. for 4 hours to obtain a cobalt-based high-temperature alloy powder.
[0075] Cobalt-based high-temperature alloy powder was used for 3D printing, where the 3D printing conditions were: scanning power 250 W, scanning speed 950 mm / s, scanning spacing 0.09 mm, and layer thickness 0.03 mm.
[0076] The 3D printed alloy specimen was heat treated at 350°C for 2 hours. After the insulation was completed, the temperature was continued to rise to 900°C for 4 hours and cooled with the furnace to obtain a 3D printed specimen.
[0077] Comparative Example 1 The cobalt-based high-temperature alloy powder for 3D printing is prepared by the same method as in Example 1, except that the amount of Cr element is reduced.
[0078] In this comparative example 1, the chemical composition (mass fraction) of the cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10%, W(Cr): 20%, W(W): 7.5%, W(C): 0.2%, W(Mo): 0.5%, W(Al): 0.5%, W(Ti): 0.5%, W(Nb): 1.0%, W(La): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0079] The other preparation processes are the same as those in Example 1.
[0080] Comparative Example 2 The cobalt-based high-temperature alloy powder for 3D printing is prepared by the same method as in Example 1, except that the amount of Cr element is increased.
[0081] In this comparative example 2, the chemical composition (mass fraction) of the cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10%, W(Cr): 30%, W(W): 7.5%, W(C): 0.2%, W(Mo): 0.5%, W(Al): 0.5%, W(Ti): 0.5%, W(Nb): 1.0%, W(La): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0082] The other preparation processes are the same as those in Example 1.
[0083] Comparative Example 3 The cobalt-based high-temperature alloy powder for 3D printing was prepared by the same method as in Example 2, except that La was not added.
[0084] In this comparative example 3, the chemical composition (mass fraction) of the cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10.5%, W(Cr): 26%, W(W): 7%, W(C): 0.15%, W(Mo): 1.0%, W(Al): 0.5%, W(Ti): 1.0%, W(Nb): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0085] The other preparation processes are the same as those in Example 2.
[0086] Comparative Example 4 The same method as in Example 2 was adopted to prepare cobalt-based high-temperature alloy powder for 3D printing, except that the amount of La was increased so that W(Mo) +W(Al)+W(Ti) + W(Nb) + W(La) +W(Ta)>6.0%.
[0087] In this comparative example 4, the chemical composition (mass fraction) of the cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10.5%, W(Cr): 26%, W(W): 7%, W(C): 0.15%, W(Mo): 1.0%, W(Al): 0.5%, W(Ti): 1.0%, W(Nb): 1.0%, W(La): 2.5%, W(Ta): 1.0%, and the balance is Co.
[0088] The other preparation processes are the same as those in Example 2.
[0089] Comparative Example 5 The cobalt-based high-temperature alloy powder for 3D printing was prepared by the same method as in Example 2, except that Mo was not added.
[0090] In this comparative example 5, the chemical composition (mass fraction) of the cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10.5%, W(Cr): 26%, W(W): 7%, W(C): 0.15%, W(Al): 0.5%, W(Ti): 1.0%, W(Nb): 1.0%, W(La): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0091] The other preparation processes are the same as those in Example 2.
[0092] Comparative Example 6 The cobalt-based high-temperature alloy powder for 3D printing is prepared by the same method as in Example 2, except that the amount of Mo is increased and W(Mo) + W(Al) + W(Ti) + W(Nb) + W(La) + W(Ta)>6.0%.
[0093] In this comparative example 6, the chemical composition (mass fraction) of the cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10.5%, W(Cr): 26%, W(W): 7%, W(C): 0.15%, W(Mo): 2.0%, W(Al): 0.5%, W(Ti): 1.0%, W(Nb): 1.0%, W(La): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0094] The other preparation processes are the same as those in Example 2.
[0095] Comparative Example 7 The cobalt-based high-temperature alloy powder for 3D printing was prepared by the same method as in Example 2, except that no Al was added.
[0096] In this comparative example 7, the chemical composition (mass fraction) of the cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10.5%, W(Cr): 26%, W(W): 7%, W(Mo): 1.0%, W(C): 0.15%, W(Ti): 1.0%, W(Nb): 1.0%, W(La): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0097] The other preparation processes are the same as those in Example 2.
[0098] Comparative Example 8 The cobalt-based high-temperature alloy powder for 3D printing was prepared by the same method as in Example 2, except that the amount of Al added was increased.
[0099] In this comparative example 8, the chemical composition (mass fraction) of the cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10.5%, W(Cr): 26%, W(W): 7%, W(C): 0.15%, W(Mo): 1.0%, W(Al): 5.0%, W(Ti): 1.0%, W(Nb): 1.0%, W(La): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0100] The other preparation processes are the same as those in Example 2.
[0101] Comparative Example 9 The cobalt-based high-temperature alloy powder for 3D printing is prepared by the same method as in Example 2, except that the amount of Al added is increased so that W(Ti)+W(Al)>2.0.
[0102] In this comparative example 9, the chemical composition (mass fraction) of the cobalt-based high-temperature alloy powder for 3D printing is: W(Ni): 10.5%, W(Cr): 26%, W(W): 7%, W(C): 0.15%, W(Mo): 1.0%, W(Al): 2.0%, W(Ti): 1.0%, W(Nb): 1.0%, W(La): 1.0%, W(Ta): 1.0%, and the balance is Co.
[0103] Comparative Example 10 The cobalt-based high-temperature alloy powder for 3D printing is prepared by the same method as in Example 1, except that: during the raw material smelting process, the pure metal is heated and smelted under vacuum conditions according to the formula, that is, all metal elements use elemental single substances as raw materials, and the smelting temperature is increased. The smelting temperature in this comparative example 10 is 3450°C.
[0104] Comparative Example 11 The cobalt-based high-temperature alloy powder for 3D printing was prepared by the same method as in Example 1, except that when the 3D printed alloy specimen was heat treated, it was directly kept at 900°C for 7 hours and then cooled with the furnace to obtain a 3D printed specimen.
[0105] The 3D printed specimens prepared in the above embodiments and comparative examples were subjected to performance tests. The specific test methods are as follows: room temperature mechanical properties test refers to GB / T 228.1; high temperature mechanical properties test refers to GB / T 228.2; high temperature creep properties test refers to GB / T 2039-2012; antioxidant properties test refers to HB5258-83; hot corrosion test refers to GB / T38231-2019. The test results are shown in Tables 1 and 2.
[0106] Table 1 Mechanical properties and high temperature performance test results of 3D printed specimens
[0107] Table 2 Anti-oxidation properties and high temperature corrosion resistance of 3D printed specimens
[0108] From the above table data, it can be seen that the alloy powders prepared by the method of the present invention in Examples 1 to 4 have good mechanical properties and high temperature properties, as well as good oxidation resistance and high temperature corrosion resistance. This technology mainly adds three alloy elements of Ni, Cr, and W, supplemented by a small amount of alloy elements such as C, Mo, Nb, Ta, Ti, and rare earth metal La, and forms a uniformly distributed high melting point compound in the alloy through component optimization and adjustment, and increases the volume fraction and melting temperature of the γ′ phase-Co3M (M=Ni, Ti, Cr, Nb, Mo, Ta, and W, etc.) in the alloy, thereby achieving the improvement of the high temperature performance of the cobalt-based high temperature alloy. Among them, the Ni element tends to be distributed in the γ′ phase, which increases the dissolution temperature of the γ′ phase, and also expands the stable γ / γ′ two-phase region of the Co-W-Ni-Cr new cobalt-based high temperature alloy at high temperature. Similarly, refractory alloy elements such as Mo, Ti, Ta, and Nb can also significantly increase the dissolution temperature of the γ′ phase, thereby improving the high temperature bearing capacity of the alloy, so that the high temperature range of the long-term extreme load parts of this material can reach (600~1000℃). Cr element is mainly matched with Ni element, and the two play a synergistic role. Cr element forms a dense Cr2O3 oxide layer on the alloy surface to block the diffusion of O into the matrix, thereby improving the high-temperature oxidation resistance of the alloy. Ni element can promote the growth of Cr2O3 and delay the nodular oxidation of the alloy, thereby improving the oxidation resistance and high-temperature corrosion resistance of the alloy. At the same time, Cr (density 7.19 g / cm 3 )、Ni(density 8.90 g / cm 3 ) elements can replace a considerable part of about 10% of W (density 19.35 g / cm 3 ) element, relative to traditional cobalt-based alloys, the W content is about 17-18%, and the weight reduction effect of equal volume is 30%-50%, which effectively achieves the effect of lightweighting the alloy. And the reduction of W content is conducive to reducing the precipitation of harmful secondary phases such as χ-Co3W and μ-Co7W6 and other hard and brittle phases in the matrix, which has a significant positive effect on the performance of the alloy. In addition, the addition of appropriate amounts of refractory alloying elements such as Mo, W, La, Ti, Nb and Ta not only ensures the generation of sufficient high-melting point compounds, but also acts as a strong γ′ phase-forming element, significantly increasing the volume fraction of the γ′ phase, and avoiding excessive elements, which leads to accelerated coarsening and increased density of the γ′ phase, and better achieves the strengthening effect of the alloy.
[0109] It can be seen from the data results of Comparative Examples 1-2 and Example 1 that if the amount of Cr element is too much or too little, the mechanical properties, high temperature properties, oxidation resistance and heat corrosion resistance of the alloy will decrease. Because the Cr element is mainly matched with the Ni element, the two play a synergistic role. The Cr element forms a dense Cr2O3 oxide layer on the surface of the alloy to block the diffusion of O into the matrix, thereby improving the high temperature oxidation resistance of the alloy. The Ni element can promote the growth of Cr2O3 and delay the nodular oxidation of the alloy, thereby improving the oxidation resistance and high temperature corrosion resistance of the alloy. Moreover, when the element content W (Cr): W (Ni) = (2.4-2.6): 1, the alloy has the best high temperature oxidation resistance. In the atmospheric environment, a dense and thin oxide film will be formed on the surface during high temperature use (600~800℃) to prevent further oxidation, and the alloy can maintain good high temperature mechanical properties.
[0110] It can be seen from the data results of Comparative Examples 3-4 and Example 2 that if La is not added to the alloy powder, or if too much La is added, the mechanical properties and high-temperature mechanical properties of the test piece will decrease.
[0111] From the data results of Comparative Examples 5-6 and Example 2, it can be seen that if Mo is not added to the alloy powder, or if too much Mo is added, the mechanical properties and high-temperature mechanical properties of the alloy test piece will decrease. It can be seen that the addition of appropriate amounts of refractory alloying elements such as Mo, W, La, Ti, Nb and Ta not only ensures that sufficient high-melting point compounds can be generated, but also significantly increases the volume fraction of the γ' phase as a strong γ' phase-forming element, and avoids the accelerated coarsening and density increase of the γ' phase caused by excessive elements, thereby achieving a better strengthening effect on the alloy.
[0112] It can be seen from the data results of Comparative Examples 7-8 and Example 2 that an inappropriate amount of Al added will also lead to a decrease in the mechanical properties and high-temperature mechanical properties of the alloy specimens, and cracking will occur. The technical solution of the present invention uses the grain boundary segregation engineering theory to rationally design the content of alloying elements and add an appropriate amount of A aluminum element W (Al): 0.5~2.0%. During the solidification of the alloy, the solubility of aluminum will decrease with decreasing temperature, causing aluminum to be enriched at the branch grain boundaries and grain boundaries, thereby promoting the formation of a continuous liquid phase film. At the same time, the continuous contraction of the matrix will produce large residual stresses at the branch grain boundaries and grain boundaries. As the temperature further decreases, the B2 phase gradually precipitates at the branch grain boundaries and grain boundaries, and gradually undergoes spinodal decomposition, decomposing into island B2 phases and Cr-rich BCC phases. The phase change behavior caused by spinodal decomposition will promote the expansion of molar volume, and the asymmetric distribution of the intermetallic compound phase will introduce more geometric dislocations. The stress fields generated by the two aspects can jointly offset part of the residual tensile stress, change the residual stress distribution state at the dendrite boundary and grain boundary position, and even change from a tensile stress state to a compressive stress state, thereby effectively inhibiting the cracking behavior of the alloy. In addition, combined with the optimization of the smelting process, the uniform distribution of the γ′ strengthening phase in the cobalt-based high-temperature alloy is achieved, and the uniform distribution of the fine and dispersed MoC strengthening phase in the cobalt-based high-temperature alloy is achieved, which has a uniform dispersion effect on the internal stress generated during the printing process, further reducing the risk of stress cracking. The high-temperature alloy specimens made of the cobalt-based high-temperature alloy powder of the present invention have no cracks and the density is more than 99%. Finally, no cracks occurred in the alloy structure prepared by the SLM process, and the density was more than 99%.
[0113] From the data comparison between Comparative Example 9 and Example 1, it can be seen that when W(Ti)+W(Al)<2.0%, the 3D printed alloy has the best anti-cracking effect and does not reduce the mechanical properties of the alloy. From the printing deposition forming process to the subsequent heat treatment and mechanical processing process, the possibility of cracking of the printed part can be minimized. It can also effectively balance the internal stress of the printed part and greatly reduce the degree of deformation caused by the heat treatment process.
[0114] From the data comparison of comparative example 10 and embodiment 1, it can be seen that if the raw materials are all metal single substances, a very high melting temperature is required, the melting difficulty is extremely high, and the production energy consumption is high; in addition, the mechanical properties and high-temperature mechanical properties of the alloy specimens finally prepared will be reduced. The preparation method of the present invention adopts the method of feeding low-melting-point intermediate alloys for high-melting-point intolerant metals such as Nb (melting point 2477°C), Ta (melting point 2996°C), Mo (melting point 2620°C) and W (melting point 3410°C), which greatly reduces the difficulty of melting the component alloys, and combines the equal power maintenance melting process: adopts a step-by-step power increase method, with a power span of 10-30Kw, and each power is maintained for 10-30min to ensure that the metal liquid is fully electromagnetically stirred. According to the actual situation, mechanical stirring is added when necessary, which is conducive to the control of the melting process and the diffusion of alloy elements, and finally greatly reduces the risk of component segregation in the final high-temperature alloy powder. Finally, the alloy powder has a uniform composition and does not contain refractory metal particles or high-melting-point intermediate phase particles, thereby improving the mechanical properties and high-temperature mechanical properties of the alloy specimens without causing cracks.
[0115] From the data comparison of Comparative Example 11 and Example 1, it can be seen that if the heat treatment process of the alloy specimen is directly carried out under high temperature conditions, the mechanical properties and high-temperature mechanical properties of the alloy specimen will decrease, and cracks will occur. The heat treatment process of the present invention, by gradually increasing the temperature in stages, better controls the thermal stress changes of the material during the heating process, ensures that the material / parts are heated uniformly, and avoids damage to the material / parts due to too fast temperature changes; in addition, by gradually increasing the temperature, any abnormal conditions that may cause overheating or combustion can be discovered and handled in time, thereby protecting the safety of equipment and materials; and, by adopting staged heating, the accuracy of the temperature can be precisely controlled, and the accuracy and repeatability of the heat treatment process can be ensured by precisely controlling the temperature changes.
[0116] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0117] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A cobalt-based high-temperature alloy powder for 3D printing, characterized in that: The alloy elements in the cobalt-based high-temperature alloy powder are calculated by mass percentage as follows: W(Ni): 8.5-12.5%, W(Cr): 22.5-27.5%, W(W): 6.0-8.0%, W(C): 0-0.2%, W(Mo) + W(Ti) + W(Nb) + W(La) + W(Ta) + W(Al): 3.0-6.0%, W(Ti)+W(Al)<2.0%, wherein W(Mo): 0.5-1.0%, W(Al): 0.5-2.0%, W(Ti): 0.4-1.0%, W(Nb): 0.5-1.0%, W(La): 0.5-1.0%, W(Ta): 0.5-1.0%, and the balance is Co.
2. The cobalt-based high-temperature alloy powder for 3D printing according to claim 1, characterized in that: The alloy elements in the cobalt-based high-temperature alloy powder are calculated by mass percentage as follows: W(Ni): 8.5-12.5%, W(Cr): 23-27%, W(W): 6.0-7.0%, W(C): 0-0.2%, W(Mo) + W(Ti) + W(Nb) + W(La) + W(Ta)+W(Al): 3.0-6.0%, W(Ti)+W(Al)<2.0%, wherein W(Mo): 0.5-1.0%, W(Al): 0.5-2.0%, W(Ti): 0.5-1.0%, W(Nb): 0.5-1.0%, W(La): 0.5-1.0%, W(Ta) 0.5-1.0%, and the balance is Co.
3. A cobalt-based high-temperature alloy powder for 3D printing according to claim 1 or 2, characterized in that: W (Cr): W (Ni) = (2.4-2.6):
1.
4. A method for preparing a cobalt-based high-temperature alloy powder for 3D printing according to any one of claims 1 to 3, characterized in that: The preparation method is: S1. Raw material smelting: heat and melt the pure metal and master alloy raw materials under vacuum conditions according to the formula; S2, atomization powder making: atomizing and powdering the smelted pre-alloyed metal using argon gas; S3, powder screening: the pre-alloyed metal powder prepared in step S2 is screened and graded under an inert gas protective atmosphere; S4, heat preservation and drying: drying the powder screened in step S3.
5. The method for preparing a cobalt-based high-temperature alloy powder for 3D printing according to claim 4, characterized in that: In step S1, Nb, Ta, Mo and W metal elements are fed in the form of raw materials of master alloy.
6. The method for preparing a cobalt-based high-temperature alloy powder for 3D printing according to claim 4, characterized in that: In step S1, when the raw materials are smelted, a step-by-step power increase method is adopted, with a power span of 10-30Kw, each power stage is maintained for 10-30min, and sufficient stirring is maintained during the smelting process; The smelting temperature is 1650-1700° C., and the smelting time is 10-40 minutes.
7. The method for preparing a cobalt-based high-temperature alloy powder for 3D printing according to claim 4, characterized in that: In step S2, the atomization gas pressure of atomization powder making is 4.0-5.0 MPa.
8. The method for preparing a cobalt-based high-temperature alloy powder for 3D printing according to claim 4, characterized in that: In step S3, the pressure of the inert gas protective atmosphere is 0.05-0.95 MPa, and the particle size range of the powder after screening is 15-53 μm.
9. An application of a cobalt-based high-temperature alloy powder for 3D printing according to any one of claims 1 to 3, characterized in that: The cobalt-based high-temperature alloy powder is applied to 3D printing.
10. The use of a cobalt-based high-temperature alloy powder for 3D printing according to claim 9, characterized in that: The 3D printed specimens were heat treated at a temperature of 300-400°C for 1-3 hours. After the heat treatment, the temperature was raised to 800-1000°C for 2-8 hours. The specimens were cooled in the furnace to obtain 3D printed specimens.
Citation Information
Patent Citations
Cobalt-based high temperature alloy
CN104046850A
3D printing based method for preparing antibacterial cobalt based dental crown
CN105838926A
Cobalt-based spray powder used for aero-engine abrasion-resistant parts and preparation method thereof
CN106975742A
ECY768 cobalt-based alloy powder and preparation method and application thereof
CN110184501A
Powder consisting of nickel-cobalt alloy, and method for producing powder
CN113891950A
Cited By
Gamma '-phase reinforced cobalt-based high-temperature alloy for LPBF process and preparation method of gamma'-phase reinforced cobalt-based high-temperature alloy
CN119640098A
High-temperature alloy powder applied to 3D printing, preparation method and molded product of high-temperature alloy powder
CN119927236A