High-thermal-conductivity and high-strength wrought magnesium alloy containing high-abundance rare earth and preparation method thereof
By adding high-abundance rare earth elements La, Zn and Mn to magnesium alloys, simplifying the element composition and optimizing the proportions, the inversion problem of thermal conductivity and strength properties of magnesium alloys is solved, deformed magnesium alloys with high thermal conductivity and high strength are realized, and simplified The process flow is simplified and suitable for industrial production.
Patent Information
- Application Number
- CN202410776241.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-15
AI Technical Summary
The thermal conductivity and strength properties of magnesium alloys are in an inverted relationship, which limits their application fields. Especially in deformed magnesium alloys, the complex element composition leads to increased process complexity and cost, making it difficult to effectively optimize thermal conductivity and strength.
By adding high-abundance rare earth elements La, Zn and Mn to magnesium alloys, the element composition is simplified, the element ratio is optimized, the thermal conductivity and mechanical properties are improved, and a simplified preparation method is used to reduce production costs and process complexity.
A deformed magnesium alloy with high thermal conductivity and high strength has been achieved, which simplifies the process flow, reduces production costs, and is suitable for industrial mass production.
Smart Images

Figure CN118773497A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermally conductive magnesium alloys, and in particular to a high-thermal conductive and high-strength deformable magnesium alloy containing high-abundance rare earths and a preparation method thereof. Background Art
[0002] Magnesium is the lightest metal structural material currently used. Its density is only 2 / 3 of aluminum and 1 / 5 of steel. Its specific strength and specific stiffness are higher than those of aluminum and steel. It also has electromagnetic shielding and excellent damping performance. It is widely used in aerospace, new energy vehicles, 3C and other fields. Among them, the development of lightweight automotive structural materials is increasingly achieved through lightweight structural materials such as magnesium alloys, such as dashboard brackets, wheels, steering armatures, etc. However, the thermal conductivity and strength properties of magnesium alloys are inversely related, which greatly limits the application of magnesium alloys. For example, the tensile strength of commercial AZ91D and AS21 magnesium alloys can reach more than 230MPa, but the room temperature thermal conductivity is only 51.2W / (m·K) and 68W / (m·K), respectively. Therefore, how to balance the improvement of the thermal conductivity and strength properties of magnesium alloys is still the key and difficult point of current research.
[0003] According to different processing techniques and application fields, magnesium alloys can be divided into cast magnesium alloys and deformed magnesium alloys. Compared with cast magnesium alloys, deformed magnesium alloys have higher mechanical properties, so the potential of deformed magnesium alloys with both thermal conductivity and strength is even greater. Deformed magnesium alloys are mainly divided into Mg-A1 series, Mg-RE series and Mg-Zn series. Among them, Mg-Zn series deformed magnesium alloys can obtain higher mechanical properties and thermal conductivity through solid solution strengthening, such as Mg-2.4Zn-0.3Mn deformed magnesium alloy, whose tensile strength reaches 258MPa and thermal conductivity reaches 121W / (m·K), and Mg-2.8Zn-0.6Ca-0.5A1-1.3Mn deformed magnesium alloy, whose tensile strength is increased to 281MPa and thermal conductivity is increased to 133W / (m·K), with high thermal conductivity and high strength (thermal conductivity greater than 125W / (m·K), tensile strength greater than 280MPa).
[0004] It can be seen that when optimizing the mechanical properties and thermal conductivity of Mg-Zn deformable magnesium alloys, multiple metal elements are usually added to the alloy to form a complex crystal phase structure. However, the complex element composition will lead to a significant increase in the process complexity of the magnesium alloy production process and bring about effects such as increased costs. Therefore, it is urgent to provide a solution to improve this problem. Summary of the invention
[0005] The purpose of the present invention is to provide a high thermal conductivity and high strength deformable magnesium alloy containing high-abundance rare earths and a preparation method thereof. The addition of three elements, Zn, Mn and La, synergistically improves the thermal conductivity and mechanical properties of the magnesium alloy by simplifying the composition of the magnesium alloy and optimizing the element ratio. At the same time, it can also reduce production costs and process complexity, and is suitable for industrial large-scale production.
[0006] In a first aspect, the present invention provides a high thermal conductivity and high strength deformable magnesium alloy containing high-abundance rare earths, which is composed of 1.45-1.55wt.% Zn, 0.45-0.55wt.% Mn, 0.15-1.5wt.% La and the remainder Mg and inevitable impurities.
[0007] The high thermal conductivity and high strength deformable magnesium alloy containing high-abundance rare earths provided by the present invention adopts Zn, Mn and La to dope Mg, which can not only simplify the element composition of the magnesium alloy, but also reduce the raw material cost of the magnesium alloy. At the same time, the addition of 0.15-1.5wt.% of La can play the role of fine grain strengthening and second phase strengthening, and can effectively improve the microstructure, mechanical properties and thermal conductivity of the magnesium alloy.
[0008] In a second aspect, the present invention provides a method for preparing a high thermal conductivity and high strength deformable magnesium alloy containing a high abundance of rare earths, comprising the following steps: heating and melting pure Mg under a protective atmosphere and then molten mixing it with pure Zn to obtain a Mg-Zn mixed melt; adding Mg-Mn intermediate alloy and Mg-La intermediate alloy into the Mg-Zn mixed melt in sequence for molten mixing to obtain an alloy melt; under an inert atmosphere, adding a refining agent to the alloy melt for stirring and refining, spreading a covering agent for insulation and then slagging, casting it into a mold preheated at 710°C and cooling it to obtain an alloy ingot; after keeping the alloy ingot warm at 410-420°C for 11-13h, cooling it to 355-365°C and extruding it to obtain a high thermal conductivity and high strength deformable magnesium alloy.
[0009] The preparation method provided by the invention has simple process and is easy to be promoted and produced on a large scale in industrialization.
[0010] In some possible embodiments, after the alloy melt is prepared, the alloy components in the alloy melt are detected and adjusted.
[0011] In some possible embodiments, after pure Mg is heated and melted and before being melted and mixed with pure Zn, pure Mg and pure Zn are dried and preheated in a vacuum environment at 100-150° C.
[0012] In some possible embodiments, before the Mg-Mn master alloy and the Mg-La master alloy are sequentially added to the Mg-Zn mixed melt for melting and mixing, the Mg-Mn master alloy and the Mg-La master alloy are dried and preheated in a vacuum environment at 100-150°C.
[0013] In some possible embodiments, the Mg—Mn master alloy includes a Mg-10 wt. % master alloy.
[0014] In some possible embodiments, the Mg-La master alloy includes a Mg-30wt.% master alloy.
[0015] In some possible embodiments, during the process of heating and melting pure Mg under a protective atmosphere: the protective atmosphere is a mixed gas of SF6 and carbon dioxide, and the volume ratio of SF6 in the protective atmosphere is 0.9-1.1%.
[0016] In some possible embodiments, during the process of heating and melting pure Mg under a protective atmosphere: after heating the pure Mg to 390-410° C. under a protective atmosphere, spread a covering agent on the surface of the pure Mg, and heat the pure Mg to 700-715° C. until the pure Mg is completely melted.
[0017] In some possible embodiments, the process of heating pure Mg to melt and then mixing it with pure Zn to obtain a Mg-Zn mixed melt includes: adding pure Zn to molten Mg at 715-725° C., stirring and melting, and then obtaining a Mg-Zn mixed melt.
[0018] In some possible embodiments, the process of sequentially adding Mg-Mn master alloy and Mg-La master alloy into the Mg-Zn mixed melt for melting and mixing includes: heating the Mg-Zn mixed melt to 745-755°C, sequentially adding Mg-Mn master alloy and Mg-La master alloy, stirring and mixing, spreading a covering agent on the surface of the melt and keeping the mixture warm until it is completely melted. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The SEM microstructure diagram of the high thermal conductivity and high strength deformable magnesium alloy prepared in Examples 1 to 3 and Comparative Example 1 of the present invention;
[0020] Figure 2 OM microstructure diagram and size statistical analysis diagram of the high thermal conductivity and high strength deformable magnesium alloy prepared in Examples 1 to 3 of the present invention and Comparative Example 1;
[0021] Figure 3 The X-ray diffraction analysis results of the high thermal conductivity and high strength deformable magnesium alloys prepared in Examples 1 to 3 and Comparative Example 1 of the present invention are shown;
[0022] Figure 4 It is a tensile curve diagram of the high thermal conductivity and high strength deformable magnesium alloy prepared in Examples 1 to 3 and Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be the common meanings understood by people with general skills in the field to which the present invention belongs.
[0024] The present invention provides a high thermal conductivity and high strength deformable magnesium alloy, which is composed of 1.45-1.55wt.% Zn, 0.45-0.55wt.% Mn, 0.15-1.5wt.% La, and the balance of Mg and inevitable impurities. In fact, when expressing the composition content of the high thermal conductivity and high strength deformable magnesium alloy, it can be written as Mg-1.5Zn-0.5Mn-0.5La.
[0025] Specifically, adding 0.15-1.5 wt. % La to the magnesium alloy composition can improve the microstructure of the magnesium alloy through the effects of grain refinement and second phase strengthening, and synergistically improve the overall mechanical properties and thermal conductivity of the magnesium alloy.
[0026] Specifically, for the Mg-1.5Zn-0.5Mn-0.5La deformable magnesium alloy provided above, the present invention also provides a preparation method, comprising the following steps:
[0027] S1. Alloy smelting: After pure Mg is heated and melted under a protective atmosphere, it is melted and mixed with pure Zn to obtain a Mg-Zn mixed melt, and then Mg-Mn master alloy and Mg-La master alloy are added in sequence to melt and mix to obtain an alloy melt;
[0028] S2, casting: in an inert atmosphere, add a refining agent to the alloy melt, stir and refine it, spread a covering agent to keep it warm, remove the slag, cast it into a preheated mold at 710°C, cool it and shape it into an alloy ingot;
[0029] S3. Extrusion molding: After the alloy ingot is kept at 410-420°C for 11-13 hours, it is cooled to 355-365°C and extruded to obtain a high thermal conductivity and high strength deformable magnesium alloy.
[0030] In fact, before executing step S1, step S0 is executed, i.e., weighing and batching: pure Mg, pure Zn, Mg-Mn master alloy and Mg-La master alloy are weighed in a mass ratio for batching.
[0031] Specifically, during the execution of step S0, Mg-1.5Zn-0.5Mn-0.5La is used as the mass ratio for weighing. At the same time, since the alloy will inevitably suffer smelting loss during the melting process, it is necessary to reserve a burning loss margin during the batching process of step S0.
[0032] In fact, when executing step S0, the pure Mg, pure Zn, Mg-Mn master alloy and Mg-La master alloy weighed are all commercially available conventional products. Specifically, the Mg-Mn master alloy can be a Mg-10wt.%Mn master alloy, and the Mg-La master alloy can be a Mg-30wt.%La master alloy. It should be noted that the Mg-10wt.%Mn master alloy means that the mass fraction of Mn in the Mg-Mn alloy is 10%, and the Mg-30wt.%La master alloy means that the mass fraction of La in the Mg-La alloy is 30%.
[0033] Specifically, during the execution of step S0, after pure Mg, pure Zn, Mg-Mn master alloy and Mg-La master alloy are weighed and mixed, the pure Mg, pure Zn, Mg-Mn master alloy and Mg-La master alloy can be placed in a vacuum environment at 100-150° C. for drying and preheating.
[0034] In fact, during the execution of step S0, after weighing pure Mg, pure Zn, Mg-Mn master alloy and Mg-La master alloy, the surface of the raw materials may be cleaned, which is beneficial to reduce the impurity content during the alloy smelting process.
[0035] Specifically, in the process of heating and melting pure Mg in a protective atmosphere during step S1, the protective atmosphere used is a mixed gas of SF6 and carbon dioxide, and the volume fraction of SF6 in the protective atmosphere is maintained at 0.9-1.1%.
[0036] Specifically, in the process of performing step S1, heating and melting pure Mg under a protective atmosphere, the process includes: heating the pure Mg to 390-410° C. under a protective atmosphere, spreading a covering agent on the surface of the pure Mg, and then heating the pure Mg to 700-715° C. until the pure Mg is completely melted.
[0037] In fact, in the process of executing step S1, heating and melting pure Mg and then melting and mixing it with pure Zn to obtain a Mg-Zn mixed melt, the process includes: heating the molten Mg to 715-725°C, adding pure Zn and stirring and melting to obtain a Mg-Zn mixed melt.
[0038] In fact, in the process of executing step S1, the Mg-Mn master alloy and the Mg-La master alloy are sequentially added into the Mg-Zn mixed melt for melting and mixing, which includes: heating the Mg-Zn mixed melt to 745-755°C, sequentially adding the Mg-Mn master alloy and the Mg-La master alloy, stirring for 3-5 minutes to mix, spreading a covering agent on the surface of the melt and keeping it warm until it is completely melted.
[0039] Specifically, during the process of performing step S2, the inert atmosphere used may be an argon atmosphere, and the refining agent used may be an RJ-2 refining agent. In fact, the amount of the refining agent used in step S2 is 2% of the mass of the alloy melt. Specifically, during the process of performing step S2, when the refining agent is added for stirring and refining, it is necessary to enable the alloy melt surface to have a mirror gloss.
[0040] Specifically, in the process of performing the slag removal after heat preservation in step S2, after the alloy melt is kept at 750° C. for 20 minutes, the slag can be removed from the melt surface.
[0041] Specifically, in the process of performing cooling and forming to obtain the alloy ingot in step S2, the alloy melt after slagging is cooled to 710° C. and then cast into a mold preheated at 710° C. for 20 minutes, and then air-cooled to obtain the alloy ingot.
[0042] Example 1
[0043] This embodiment 1 provides a method for preparing a high thermal conductivity and high strength deformable magnesium alloy containing a high abundance of rare earth, comprising the following steps:
[0044] S0. Weighing ingredients: weigh pure Mg, pure Zn, Mg-10wt.%Mn master alloy and Mg-30wt.%La master alloy according to the mass ratio of Mg-1.5Zn-0.5Mn-0.5La, and dry and preheat them in a vacuum drying oven at 130°C;
[0045] S1. Alloy smelting: After heating the crucible to 400°C, a protective atmosphere is introduced, pure Mg is placed in the crucible, and a covering agent is spread on the surface of the pure Mg, and the temperature is uniformly raised to above 700°C until the pure Mg is completely melted; the temperature is further raised to 720°C, and pure Zn is added and stirred until it is completely melted; the temperature is further raised to 750°C, and Mg-10wt.%Mn master alloy and Mg-30wt.%La master alloy are added in sequence, and the melt is stirred for 3 minutes, and a covering agent is spread on the surface of the melt to keep the temperature until it is completely melted, so as to obtain an alloy melt; under an argon atmosphere, 2% RJ-5 refining agent of the mass of the alloy melt is added into the crucible, and mechanical stirring is performed for 5-10 minutes until a mirror-like gloss appears on the surface of the melt, and then the scum on the surface of the melt is removed and a covering agent is sprinkled, and the slag is skimmed after keeping the temperature at 750°C for 20 minutes;
[0046] S2, casting: cooling to 710°C and casting into a mold preheated at 710°C for 20 minutes, and air cooling to obtain an alloy ingot;
[0047] S3. Extrusion molding: Place the alloy ingot in a box-type resistance furnace and heat it to 415°C and keep it warm for 12 hours. Then take out the alloy ingot and air-cool it to room temperature to remove the surface oxide scale. Preheat the alloy ingot to 360°C and use a metal extruder to extrude it at 360°C with an extrusion ratio of 25:1 and an extrusion rate of 2mm / s to obtain a high thermal conductivity and high strength deformable magnesium alloy rod.
[0048] Example 2
[0049] This embodiment 2 provides a method for preparing a high thermal conductivity and high strength deformable magnesium alloy containing a high abundance of rare earths. The difference from embodiment 1 is that in step S0, the ingredients are weighed and prepared according to the mass ratio of Mg-1.5Zn-0.5Mn-1.0La.
[0050] Example 3
[0051] This embodiment 3 provides a method for preparing a high thermal conductivity and high strength deformable magnesium alloy containing a high abundance of rare earths. The difference from embodiment 1 is that in step S0, the ingredients are weighed and prepared according to the mass ratio of Mg-1.5Zn-0.5Mn-1.5La.
[0052] Comparative Example 1
[0053] Comparative Example 1 provides a method for preparing a deformed magnesium alloy, which is different from Example 1 in that in step S0, ingredients are weighed and prepared according to the mass ratio of Mg-1.5Zn-0.5Mn.
[0054] Performance testing and data
[0055] The wrought magnesium alloy bars prepared in Examples 1 to 3 and Comparative Example 1 were tested for the following items:
[0056] Composition determination: According to GB / T 13748-2005 "Chemical Analysis Methods for Magnesium and Magnesium Alloys", samples were taken and the composition was tested using an electric spark direct reading spectrometer and an ICP (Inductive Coupled Plasma Emission Spectrometer). The results are shown in Table 1.
[0057] Room temperature thermal conductivity: According to the thermal conductivity determination method specified in GB / T22588-2008 "Flash method for measuring thermal diffusivity or thermal conductivity", a laser thermal conductivity meter (LFA500) was used for determination, and the results are shown in Table 2;
[0058] Room temperature mechanical properties: The processing test was carried out in accordance with GB6397-86 "Metal Tensile Test Specimens". The test equipment was a Labsans 30kN universal testing machine tensile machine. The test items were tensile strength, yield strength and elongation. The results are shown in Table 2.
[0059] Table 1 Measured ingredients
[0060]
[0061] Table 2 Thermal conductivity and mechanical properties
[0062]
[0063]
[0064] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A high thermal conductivity and high strength deformable magnesium alloy containing high abundance rare earth, characterized in that: It consists of 1.45-1.55wt.% of Zn, 0.45-0.55wt.% of Mn, 0.15-1.5wt.% of La, and the balance of Mg and inevitable impurities.
2. A method for preparing a high thermal conductivity and high strength deformable magnesium alloy as claimed in claim 1, characterized in that: The following steps are involved: Pure Mg is heated to melt under a protective atmosphere and then melted and mixed with pure Zn to obtain a Mg-Zn mixed melt; sequentially adding a Mg-Mn master alloy and a Mg-La master alloy into a Mg-Zn mixed melt, melting and mixing the alloy melt; In an inert atmosphere, a refining agent is added to the alloy melt for stirring and refining, a covering agent is spread to keep the temperature, and then the slag is removed, and the alloy ingot is cast into a mold preheated to 710°C and cooled to obtain an alloy ingot; The alloy ingot is kept at 410-420°C for 11-13 hours, cooled to 355-365°C and extruded to obtain a high thermal conductivity and high strength deformable magnesium alloy.
3. The preparation method according to claim 2, characterized in that: After the alloy melt is obtained, the alloy components in the alloy melt are detected and adjusted.
4. The preparation method according to claim 2, characterized in that: After pure Mg is heated and melted, before being melted and mixed with pure Zn, pure Mg and pure Zn are dried and preheated in a vacuum environment at 100-150°C; And / or, before sequentially adding the Mg-Mn master alloy and the Mg-La master alloy into the Mg-Zn mixed melt for melting and mixing, the Mg-Mn master alloy and the Mg-La master alloy are dried and preheated in a vacuum environment at 100-150°C.
5. The preparation method according to claim 2 or 4, characterized in that: The Mg-Mn master alloy includes a Mg-10 wt. % master alloy; and / or, the Mg-La master alloy includes a Mg-30 wt. % master alloy.
6. The preparation method according to claim 2, characterized in that: In the process of heating and melting pure Mg under a protective atmosphere: the protective atmosphere is a mixed gas of SF6 and carbon dioxide, and the volume ratio of SF6 in the protective atmosphere is 0.9-1.1%; and / or, under a protective atmosphere, after the pure Mg is heated to 390-410°C, a covering agent is spread on the surface of the pure Mg, and the temperature is raised to 700-715°C until the pure Mg is completely melted.
7. The preparation method according to claim 2, characterized in that: The process of heating and melting pure Mg and then melting and mixing it with pure Zn to obtain a Mg-Zn mixed melt includes: adding pure Zn into molten Mg at 715-725° C., stirring and melting, and then obtaining a Mg-Zn mixed melt.
8. The preparation method according to claim 2, characterized in that: The process of sequentially adding Mg-Mn master alloy and Mg-La master alloy into the Mg-Zn mixed melt for melting and mixing includes: heating the Mg-Zn mixed melt to 745-755° C., sequentially adding the Mg-Mn master alloy and the Mg-La master alloy, stirring and mixing, spreading a covering agent on the surface of the melt and keeping the temperature until it is completely melted.