Ti-Zr-Nb-Fe-Ga high-entropy alloy and preparation method and application thereof

By adding gallium element to titanium alloy to prepare Ti-Zr-Nb-Fe-Ga high-entropy alloy, the problem of infection and insufficient osseointegration ability of traditional titanium alloy in microbial environment is solved, and the antibacterial and osseointegration functions are significantly improved. , suitable for medical implants.

CN118773499APending Publication Date: 2024-10-15SHANGHAI NINTH PEOPLES HOSPITAL SHANGHAI JIAO TONG UNIV SCHOOL OF MEDICINE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410890625.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional titanium and titanium alloys are prone to adhesion of bacteria in microbial environments, leading to infection, and lack antibacterial properties and the ability to promote osseointegration. Gallium has not yet been integrated into titanium alloys through alloying for biofilm inhibition and osseointegration.

Method used

Using Ti-Zr-Nb-Fe-Ga high-entropy alloy, by adding gallium element to the titanium alloy, the preparation method includes preparation, vacuuming, smelting and final stages to achieve the sustained release of gallium ions to inhibit bacterial adhesion and bone breakdown. Cell differentiation promotes osseointegration.

Benefits of technology

It achieves the antibacterial properties and osseointegration functions of high-entropy alloys, significantly inhibits biofilm formation and osteoclast activation, has good biological safety and mechanical properties, and is suitable for medical implants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773499A_ABST
    Figure CN118773499A_ABST
Patent Text Reader

Abstract

The invention discloses a Ti-Zr-Nb-Fe-Ga high-entropy alloy and a preparation method and application thereof.The Ti-Zr-Nb-Fe-Ga high-entropy alloy is composed of Ti, Zr, Nb, Fe and Ga, the atomic ratio of Ti to Zr to Nb to Fe is 1: 1: 1: 1, the mass fraction of Ga is 0.01%-5%, and the preparation method sequentially comprises the preparation stage, the vacuumizing stage, the smelting stage and the ending stage. According to the alloy material for the medical implant, the alloy material is relatively convenient to process, high in biocompatibility and high in antibacterial performance and has the function of promoting osseointegration, the gallium element is added into the titanium alloy to obtain the high-entropy alloy, on one hand, the slow-release gallium ions can inhibit bacterial adhesion and hinder biofilm formation, biofilm related infection is prevented, and on the other hand, the slow-release gallium ions can be used for preparing the high-entropy alloy for the medical implant; on the other hand, the activity of osteoclast activation can be remarkably inhibited, the potential of promoting osseointegration is achieved, and important clinical application value is achieved when the compound is used for medical implants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of medical materials, and in particular relates to a Ti-Zr-Nb-Fe-Ga high entropy alloy and a preparation method and application thereof. Background Art

[0002] Titanium is one of the most widely used oral medical metal materials. However, traditional titanium and titanium alloys do not have antibacterial properties. When placed in a microbial environment (such as the human mouth), they are prone to adhere to bacteria and cause infection, such as peri-implantitis, enamel demineralization and gingivitis after orthodontic treatment, and infection after oral and maxillofacial surgery. According to the data from the "Practical Manual for the Prevention and Control of Nosocomial Infections" issued by the World Health Organization, there are more than 14 million patients with nosocomial infections every day in the world, of which about 60% are related to implant infections. In addition, titanium is an inert metal, which guides bone tissue regeneration poorly and is prone to aseptic bone dissolution. In summary, Ti-6Al-4V (TC4) titanium alloy lacks anti-bacterial biofilm function and has insufficient ability to promote bone integration.

[0003] Gallium ion is a transition metal element that can interfere with bacterial iron metabolism, is not easy to develop drug resistance, and has a significant inhibitory effect on biofilm formation. In addition, gallium ion has good biosafety as a clinical hypercalcemia treatment drug. Using gallium ion as a titanium alloy surface modifier is expected to make a breakthrough in improving the antibacterial properties of alloys. Currently, gallium-containing implants mainly include bioactive glass, hydrogel, hydroxyapatite, etc. These degradable stents can release gallium ions slowly after adsorbing gallium agents to achieve a sustained antibacterial effect, but the mechanical properties of these bioactive materials are far inferior to titanium, and there are great limitations in clinical application. On the other hand, gallium ions have a significant osteoclast inhibitory effect and can promote bone integration. At present, there is no implant device that integrates gallium into titanium alloys by alloying and applies the alloy to biofilm formation inhibition evaluation and osteoclast activation inhibition. In addition, gallium has been approved by the US Food and Drug Administration (FDA) for the treatment of hypercalcemia and malignant tumors. It can effectively inhibit bone resorption and plasma calcium elevation, and has good safety in vivo. Summary of the invention

[0004] In view of the deficiencies in the prior art, the main purpose of the present invention is to provide a Ti-Zr-Nb-Fe-Ga high entropy alloy, which has the functions of antibacterial, inhibiting osteoclast differentiation, and promoting angiogenesis.

[0005] Another object of the present invention is to provide a method for preparing the Ti-Zr-Nb-Fe-Ga high entropy alloy.

[0006] Another object of the present invention is to provide applications of the Ti—Zr—Nb—Fe—Ga high entropy alloy.

[0007] To achieve the above object, the present invention adopts the following technical solution:

[0008] In a first aspect, a Ti-Zr-Nb-Fe-Ga high entropy alloy is composed of Ti, Zr, Nb, Fe and Ga, wherein the atomic ratio of Ti, Zr, Nb and Fe is 1:1:1:1, and the mass fraction of Ga is 0.01%-5%.

[0009] Preferably, in the Ti-Zr-Nb-Fe-Ga high entropy alloy, the atomic ratio of Ti, Zr, Nb and Fe is 1:1:1:1, and the mass fraction of Ga is 1%.

[0010] In a second aspect, the preparation method of the Ti-Zr-Nb-Fe-Ga high entropy alloy comprises a preparation stage, a vacuuming stage, a smelting stage and an end stage in sequence, specifically comprising the following steps:

[0011] (a) Preparation stage:

[0012] (a1) Open the furnace and clean the electrodes and crucible with alcohol;

[0013] (a2) placing the metal to be smelted into the crucible according to the proportion, closing the furnace body, and keeping all valves closed;

[0014] (a3) Turn on the main power switch and circulating water valve, turn on the circulating water power switch and power switch on the equipment in turn, wait until the equipment runs stably, and turn on the molecular pump power switch in the control cabinet;

[0015] (b) Vacuuming stage:

[0016] (b1) First stage vacuuming: After the equipment is stable, open the furnace valve and the pump switch power supply, start the pressure display screen, and tighten the fasteners on the furnace cover and the furnace seal during the vacuuming process to ensure the sealing;

[0017] (b2) Second stage vacuuming: After the pressure in the furnace reaches the primary setting, open the molecular pump valve and molecular pump switch in sequence, and close the furnace valve and pump switch;

[0018] (b3) After the pressure in the furnace reaches the set value, close the molecular pump valve and the molecular pump button switch in sequence, and the equipment is vacuumed;

[0019] (b4) filling the evacuated furnace with 99.99% high-purity argon gas until the pressure reaches one atmosphere;

[0020] (c) Melting stage:

[0021] (c1) aligning the moving electrode with the electrode on the crucible, and observing in real time through the observation window during the movement to ensure that the distance between the two reaches the required value;

[0022] (c2) Increase the current to prepare for smelting, press the arc-starting button, use the hand wheel on the rocker to move the two electrodes in the furnace to contact the arc, and immediately turn the hand wheel to separate the two electrodes after arcing, and use the rocker to move the moving electrode away to prevent burning the electrode on the crucible. The whole process is operated through the observation window;

[0023] (c3) using an electric arc to melt the metals to be melted in sequence, and turning off the electric arc after the melting is completed;

[0024] (c4) using a manipulator to flip the metal in the crucible and smelt it repeatedly to ensure uniform smelting;

[0025] (d) Ending stage:

[0026] (d1) Open the furnace body, clean the furnace cavity, remove smoke, sand and splashed metal, clean the copper mold and put it back into the mold channel, and tighten the sealing cover;

[0027] (d2) After the furnace cavity is cleaned and dried, the furnace body is closed and vacuumed at the same time;

[0028] (d3) After vacuuming is completed, turn off the molecular pump switch, circulating water switch, external circulating water valve and main power switch in sequence;

[0029] (d4) Check whether the switches and valves of the equipment are in the open or closed state.

[0030] Preferably, in step (b3), the vacuum degree of the evacuation is 1×10 -4 Pa.

[0031] Preferably, in step (c3), the number of repeated smelting is 6-12 times, and the smelting current is 580-597A.

[0032] A third aspect is the use of the Ti-Zr-Nb-Fe-Ga high entropy alloy in the preparation of medical implants.

[0033] The present invention provides an alloy material for medical implants that is relatively easy to process, has high biocompatibility, strong antibacterial properties and promotes bone integration, which is a high entropy metal alloy. At the same time, alloying gallium can not only maintain the excellent mechanical properties of pure titanium, but also slowly release gallium ions for at least 3-6 months to achieve long-lasting antibacterial and bone integration. Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The Ti-Zr-Nb-Fe-Ga high entropy alloy of the present invention adds gallium element to the titanium alloy. The slowly released gallium ions can inhibit bacterial adhesion, hinder biofilm formation, and prevent biofilm-related infections. On the other hand, it can significantly inhibit the activity of osteoclast activation and has the potential to promote bone integration.

[0035] 2. The preparation method of the Ti-Zr-Nb-Fe-Ga high entropy alloy in the present invention is simple and easy to control. It can be made into high entropy alloys with different gallium contents to achieve the effect of promoting bone integration. It can be used for medical implants and has important clinical application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 2 is a scanning electron microscope image (SEM) of the Ti-Zr-Nb-Fe-Ga high entropy alloy in the embodiment and the corresponding element distribution analysis results.

[0037] Figure 2 These are the evaluation results of the biofilm inhibition effects of different alloys in the examples. From left to right, the samples are TC4; Ti-Zr-Nb-Fe-0% Ga; Ti-Zr-Nb-Fe-0.5% Ga; Ti-Zr-Nb-Fe-1% Ga; Ti-Zr-Nb-Fe-2.5% Ga; Ti-Zr-Nb-Fe-5% Ga.

[0038] Figure 3 The tartrate-resistant acid phosphatase (TRAP) staining results after co-incubation of osteoclasts with different alloy extracts in the example, the alloys from left to right are: Ti-Zr-Nb-Fe-0%Ga; Ti-Zr-Nb-Fe-0.5%Ga; Ti-Zr-Nb-Fe-1%Ga; Ti-Zr-Nb-Fe-2.5%Ga; Ti-Zr-Nb-Fe-5%Ga.

[0039] Figure 4 The OD450 test results of different alloy extracts in the example were incubated with L929 cells for one day. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention will be described in detail below in combination with the embodiments of the present invention and the accompanying drawings. However, the following embodiments are only used to understand the present invention and cannot limit the present invention.

[0041] The following examples are used to prepare Ti-Zr-Nb-Fe-Ga high entropy alloys, which include a preparation stage, a vacuuming stage, a smelting stage, and a termination stage. The specific steps are as follows:

[0042] Preparation stage: (1) Open the furnace body and clean the electrodes and crucibles with alcohol, which evaporates quickly; (2) Place the metal to be smelted into the crucible, close the furnace body, tighten all fasteners evenly, and check that all valves of each device are in the closed state; (3) Turn on the main power switch and circulating water valve, and then turn on the circulating water power switch and power switch on the equipment in turn. After the equipment runs stably, turn on the molecular pump power switch in the control cabinet.

[0043] Vacuuming stage: (1) First stage vacuuming. After the equipment is stable, open the furnace valve and the machine pump switch power supply, start the pressure display screen, and during the vacuuming process, tighten the fasteners and furnace seals on the furnace cover to ensure the sealing; (2) Second stage vacuuming. After the pressure in the furnace reaches the primary setting, open the molecular pump valve and molecular pump switch in turn, close the furnace valve, and turn off the machine pump switch; (3) After the pressure in the furnace reaches the setting, close the molecular pump valve and molecular pump button switch in turn, and the equipment is vacuumed; (4) Fill the vacuumed furnace with 99.99% high-purity argon gas to reach one atmosphere (this operation takes 20-30 minutes).

[0044] Melting stage: (1) Align the moving electrode with the electrode on the crucible, and observe in real time through the observation window during the movement to ensure that the distance between the two reaches the required value; (2) Increase the current, prepare for melting, press the arc starting button, and use the hand wheel on the joystick to move the two electrodes in the furnace to contact and start the arc. After the arc is started, immediately turn the hand wheel to separate the two electrodes, and use the joystick to move the moving electrode away to prevent burning of the electrode on the crucible. Operate the entire process through the observation window; (3) Use the electric arc to melt the metals to be melted in turn. After the melting is completed, turn off the arc; (4) Use the robot to flip the metal in the crucible and melt the metal repeatedly to ensure uniform melting.

[0045] Ending stage: (1) Open the furnace body, clean the furnace cavity, remove smoke, sand and splashed metal, clean the copper mold and put it back into the mold channel, and tighten the sealing cover; (2) After the furnace cavity is cleaned and blown dry, close the furnace body and evacuate at the same time; (3) After evacuation, turn off the molecular pump switch, circulating water switch, external circulating water valve, main power switch, etc. in turn; (4) Check the switches of the equipment and the valves are in the correct opening and closing state, and the experiment is completed.

[0046] The main parameters in the above steps are: Vacuum degree: 10 -4 Pa; number of smelting times: 12 times; smelting current: 580-597A; main components of the metal to be smelted: the atomic ratio of Ti, Zr, Nb, and Fe is 1:1:1:1, and the mass fraction of Ga is 0-5%.

[0047] Examples 1-5

[0048] Ti-Zr-Nb-Fe-Ga high entropy alloy was prepared according to the steps of the above method. The only difference between Examples 1-5 is the mass fraction of Ga, which is 0, 0.5%, 1%, 2.5% and 5%, respectively. The obtained alloys are Ti-Zr-Nb-Fe-0%Ga; Ti-Zr-Nb-Fe-0.5%Ga; Ti-Zr-Nb-Fe-1%Ga; Ti-Zr-Nb-Fe-2.5%Ga; Ti-Zr-Nb-Fe-5%Ga.

[0049] The Ti-Zr-Nb-Fe-0%Ga, Ti-Zr-Nb-Fe-0.5%Ga, Ti-Zr-Nb-Fe-1%Ga, Ti-Zr-Nb-Fe-2.5%Ga, Ti-Zr-Nb-Fe-5%Ga and TC4 prepared in Examples 1-5 were tested respectively. The results are as follows: Figure 1-4 As shown, the details are as follows:

[0050] like Figure 1 As shown, the surface morphology of the alloy was observed by scanning electron microscopy (A), the element distribution was analyzed and the alloy composition was tested (B), and the specific element content test results are shown in Table 1. The test results show that the Ti, Zr, Nb, Fe, and Ga alloy system was successfully prepared.

[0051] like Figure 2 As shown in the figure, the formation of biofilm on the alloy by Pa (Pseudomonas aeruginosa) and MRSA (Methicillin-resistant Staphylococcus aureus) was observed by laser confocal microscopy. It can be seen that the high entropy alloy Ti-Zr-Nb-Fe-1%Ga can inhibit the growth of bacteria into biofilm on the surface, while TC-4 titanium alloy and Ti-Zr-Nb-Fe-0%Ga alloy cannot inhibit the growth of bacteria into biofilm on its surface. It can be seen that the high entropy alloy Ti-Zr-Nb-Fe-1%Ga has a better anti-biofilm formation effect than the traditional TC-4 alloy.

[0052] like Figure 3 As shown, the anti-TRAP staining results of osteoclasts in the extracts of different alloys showed that with the increase of Ga addition, the inhibitory effect of the alloy on osteoclast differentiation gradually increased, indicating that the alloy has a good effect on inhibiting osteoclast differentiation.

[0053] like Figure 4 As shown, the extracts of TC-4 titanium alloy, Ti-Zr-Nb-Fe-0%Ga, Ti-Zr-Nb-Fe-0.5%Ga, Ti-Zr-Nb-Fe-1%Ga, Ti-Zr-Nb-Fe-2.5%Ga and Ti-Zr-Nb-Fe-5%Ga alloys were co-incubated with L929 cells, and the absorbance at OD450 was observed to test its cytotoxicity. The results showed that compared with the commonly used TC4 titanium alloy, the gallium-containing Ti-Zr-Nb-Fe-Ga high entropy alloy had no cytotoxicity and had better biosafety.

[0054] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A Ti-Zr-Nb-Fe-Ga high entropy alloy, characterized in that: It is composed of Ti, Zr, Nb, Fe and Ga, wherein the atomic ratio of Ti, Zr, Nb and Fe is 1:1:1:1, and the mass fraction of Ga is 0.01%-5%.

2. The Ti-Zr-Nb-Fe-Ga high entropy alloy according to claim 1, characterized in that: The atomic ratio of Ti, Zr, Nb and Fe is 1:1:1:1, and the mass fraction of Ga is 1%.

3. The method for preparing the Ti-Zr-Nb-Fe-Ga high entropy alloy according to claim 1 or 2, characterized in that: The process includes a preparation stage, a vacuuming stage, a melting stage and a finishing stage, and includes the following steps: (a) Preparation stage: (a1) Open the furnace and clean the electrodes and crucible with alcohol; (a2) placing the metal to be smelted into the crucible according to the proportion, closing the furnace body, and keeping all valves closed; (a3) Turn on the main power switch and circulating water valve, turn on the circulating water power switch and power switch on the equipment in turn, wait until the equipment runs stably, and turn on the molecular pump power switch in the control cabinet; (b) Vacuuming stage: (b1) First stage vacuuming: After the equipment is stable, open the furnace valve and the pump switch power supply, start the pressure display screen, and tighten the fasteners on the furnace cover and the furnace seal during the vacuuming process to ensure the sealing; (b2) Second stage vacuuming: After the pressure in the furnace reaches the primary setting, open the molecular pump valve and molecular pump switch in turn, and close the furnace valve and pump switch; (b3) After the pressure in the furnace reaches the set value, close the molecular pump valve and the molecular pump button switch in sequence, and the equipment is vacuumed; (b4) filling the evacuated furnace with 99.99% high-purity argon gas until the pressure reaches one atmosphere; (c) Melting stage: (c1) aligning the moving electrode with the electrode on the crucible, and observing in real time through the observation window during the movement to ensure that the distance between the two reaches the required value; (c2) Increase the current to prepare for smelting, press the arc-starting button, use the hand wheel on the rocker to move the two electrodes in the furnace to contact the arc, and immediately turn the hand wheel to separate the two electrodes after arcing, and use the rocker to move the moving electrode away to prevent burning the electrode on the crucible. The whole process is operated through the observation window; (c3) using an electric arc to melt the metals to be melted in sequence, and turning off the electric arc after the melting is completed; (c4) using a manipulator to flip the metal in the crucible and smelt it repeatedly to ensure uniform smelting; (d) Ending stage: (d1) Open the furnace body, clean the furnace cavity, remove smoke, sand and splashed metal, clean the copper mold and put it back into the mold channel, and tighten the sealing cover; (d2) After the furnace cavity is cleaned and dried, the furnace body is closed and vacuumed at the same time; (d3) After vacuuming is completed, turn off the molecular pump switch, circulating water switch, external circulating water valve and main power switch in sequence; (d4) Check whether the switches and valves of the equipment are in the open or closed state.

4. The method for preparing the Ti-Zr-Nb-Fe-Ga high entropy alloy according to claim 3, characterized in that: In step (b3), the vacuum degree of the evacuation is 1×10 -4 Pa.

5. The method for preparing the Ti-Zr-Nb-Fe-Ga high entropy alloy according to claim 3, characterized in that: In step (c3), the number of repeated smelting is 6-12 times, and the smelting current is 580-597A.

6. Use of the Ti-Zr-Nb-Fe-Ga high entropy alloy according to claim 1 or 2 in the preparation of medical implants.

Citation Information

Patent Citations

  • Hydrogen storage high-entropy alloy taking body-centered cubic structure as principal thing and preparation method for hydrogen storage high-entropy alloy

    CN107338385A

  • High-bacterium-resistance titanium alloy as metal implant

    CN109112358A

  • Titanium-gallium alloy cast ingot and preparation method and application thereof

    CN115319061A