Production and smelting method of Phi390mm X52QH round tube blank for pure hydrogen conveying

By using processes such as converter smelting, LF refining and VD vacuum degassing in the production of pure hydrogen transportation pipeline materials to control the chemical composition and non-metallic inclusions of the steel billet, the problem of insufficient material quality in the existing technology is solved, and high quality and The production of safe Φ390mm X52QH round tube blanks for pure hydrogen transportation meets the safety and deep processing performance requirements of long-distance transportation.

CN118773501AInactive Publication Date: 2024-10-15BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410770222.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The quality of existing pure hydrogen transportation pipeline materials is insufficient and difficult to meet the safety and deep processing performance requirements of high-purity hydrogen transportation. In particular, there are deficiencies in pressure and material durability during long-distance transportation.

Method used

A production method including molten iron pretreatment, converter smelting, LF refining, VD vacuum degassing and round billet continuous casting is adopted to control the chemical composition and non-metallic inclusions of the steel billet to ensure the high quality and safety of the steel billet. Specific steps include pre-desulfurization of molten iron, protective casting, vacuum treatment and slow cooling to ensure the low sulfur and low oxygen content of the steel billet and good deep processing performance.

Benefits of technology

The produced Φ390mm X52QH round tube blank for pure hydrogen transportation has 0-1 level sulfur print inspection results and 0-1 level non-metallic inclusions. The gas oxygen content is 15-25PPm. The material has good deep processing performance and safe use. properties to meet the demand for high-purity hydrogen transportation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773501A_ABST
    Figure CN118773501A_ABST
Patent Text Reader

Abstract

The invention discloses a production and smelting method of a Phi390mm X52QH round pipe billet for pure hydrogen conveying. The production process comprises the steps of molten iron pretreatment, converter smelting, LF refining, VD vacuum degassing and round billet continuous casting. The pipe blank comprises the following chemical components in percentage by mass: 0.05 to 0.07 percent of C, 0.20 to 0.35 percent of Si, 0.95 to 1.25 percent of Mn, 0.15 to 0.30 percent of Cr, 0.08 to 0.15 percent of Mo, less than or equal to 0.015 percent of P, less than or equal to 0.003 percent of S, less than or equal to 0.002 percent of Pb, less than or equal to 0.0025 percent of Ti and the balance of iron and trace impurity elements. The steel blank sulfur mark inspection results of the prepared X52QH round pipe blank for pure hydrogen transportation with the diameter of 390mm are 0 to 1 grade; the non-metallic inclusions of the steel billet are 0-1 grade; and the content of gaseous oxygen in the steel billet is 15-25 PPm. The material has good deep processing performance and use safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a production and smelting method of a Φ390mm X52QH round tube billet for pure hydrogen transportation. Background Art

[0002] my country has a sound industrial system and a good foundation for hydrogen production. The production and use of hydrogen as a raw material gas and industrial gas are both large-scale. Since 2015, my country's total annual hydrogen production has been around 24 million tons. By 2025, my country's renewable energy hydrogen production will reach 100,000 to 200,000 tons / year, achieving a carbon dioxide emission reduction of 1 million to 2 million tons / year. By 2035, a hydrogen energy industry system will be formed, and a diversified hydrogen energy application ecosystem covering transportation, energy storage, industry and other fields will be constructed. In the context of large-scale application of hydrogen energy, hydrogen energy transportation, as a channel connecting upstream and downstream, is a key link in the development of the hydrogen energy industry.

[0003] According to the purity of hydrogen, pipeline hydrogen transportation can be divided into pure hydrogen transportation and hydrogen-blended transportation. Pure hydrogen transportation is generally carried out by constructing or renovating existing pipelines to transport high-purity hydrogen for direct use in production and life. The construction of foreign hydrogen pipelines was early and the mileage was long. The earliest long-distance pure hydrogen pipeline was built in Ruhr, Germany in 1938, with a total mileage of 208 kilometers, a transportation pressure of 2.5MPa, and pipes of SAE 1016-DN 168~273 (Note: high-quality low-carbon steel, steel pipe diameter is Φ168-273mm). At present, the total mileage of pure hydrogen pipelines in the world is 4,500km, mainly concentrated in North America and Europe, accounting for more than 90%. The materials used for the built hydrogen pipelines are generally low-grade carbon steel and low-alloy steel welded steel pipes or seamless steel pipes. The ultra-short distance transportation pressure is up to 14MPa, and the long-distance transportation pressure is generally below 10MPa, most of which are concentrated in 3~5MPa. Summary of the invention

[0004] The purpose of the present invention is to provide a production and smelting method of X52QH round tube billet for Φ390mm pure hydrogen transportation, the results of the billet sulfur print inspection are all 0-1 level; the non-metallic inclusions of the billet are 0-1 level; the gas oxygen content in the billet is 15-25PPm. The material has good deep processing performance and safety in use.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] The present invention discloses a production and smelting method of a Φ390mm X52QH round tube billet for pure hydrogen transportation, wherein the production process comprises molten iron pretreatment, converter smelting production process, LF refining production process, VD vacuum degassing production process and round billet continuous casting production process; wherein:

[0007] All hot metal used in converter smelting is pre-desulfurized hot metal: hot metal requirements are S≤0.05%, P≤0.12%, and hot metal temperature≥1300℃; converter endpoint control requirements: C≤0.05%, P≤0.012%, and steel tapping temperature≥1630℃; LF refining in-place requirements: molten steel Al is controlled at around 0.030%; LF refining process slag basicity is controlled at 3.0-4.5, the (FeO+MnO) content in the slag is controlled to be <1%, and the white slag retention time is ≥15 minutes; VD vacuum treatment requirements: keep the vacuum degree ≤0.KPa for ≥25 minutes, soft blowing time ≥15min; continuous casting process control requirements: replace the tundish with argon before casting, use protective casting during the casting process, use alkaline covering agent for the tundish, use weak cooling for the secondary cooling water, use electromagnetic stirring for the crystallizer and the solidification end, control the continuous casting speed at 0.5m / min~1.0m / min, and the superheat of the molten steel ≤30℃;

[0008] The chemical composition of the tube blank is as follows: C 0.05-0.07%, Si 0.20-0.35%, Mn 0.95-1.25%, Cr 0.15-0.30%, Mo 0.08-0.15%, P≤0.015%, S≤0.003%, Pb≤0.002%, Ti≤0.0025%, and the rest are iron and trace impurity elements.

[0009] Furthermore, the continuous casting billet is quickly rolled off the production line, and the billet is cooled in a slow cooling pit, with the slow cooling time being ≥ 72 hours; the temperature of the continuous casting billet is < 100°C before leaving the slow cooling pit.

[0010] Furthermore, the results of sulfur print test of the steel billets are all level 0 to 1; the non-metallic inclusions of the steel billets are level 0 to 1; the gas oxygen content in the steel billets is 15 to 25 PPm, and the material has good deep processing performance and safety of use.

[0011] Furthermore, the chemical composition of the tube blank is as follows by mass percentage: C 0.06%, Si 0.25%, Mn 1.13%, Cr0.18%, Mo 0.10%, P 0.011%, S 0.002%, Pb 0.0008%, Ti 0.0015%, and the rest are iron and trace impurity elements.

[0012] Furthermore, the chemical composition of the tube blank is as follows by mass percentage: C 0.05%, Si 0.24%, Mn 1.14%, Cr0.20%, Mo 0.11%, P 0.010%, S 0.003%, Pb 0.0010%, Ti 0.0017%, and the rest is iron and trace impurity elements.

[0013] Furthermore, the chemical composition of the tube blank is as follows by mass percentage: C 0.06%, Si 0.26%, Mn 1.16%, Cr0.21%, Mo 0.11%, P 0.09%, S 0.003%, Pb 0.0011%, Ti 0.0019%, and the rest is iron and trace impurity elements.

[0014] Compared with the prior art, the beneficial technical effects of the present invention are:

[0015] The X52QH round tube billet with a diameter of 390 mm for pure hydrogen transportation prepared by the present invention has a sulfur print test result of 0 to 1 level, a non-metallic inclusion of 0 to 1 level, and a gas oxygen content of 15 to 25 PPm in the billet. The material has good deep processing performance and safety in use. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The present invention will be further described below in conjunction with the accompanying drawings.

[0017] Figure 1 This is a low-magnification photo of the hot acid of Example 1;

[0018] Figure 2 This is a low-magnification photo of thermal acid in Example 2;

[0019] Figure 3 This is a low-magnification photo of the hot acid of Example 3. DETAILED DESCRIPTION

[0020] The technical features and advantages of the present invention are described in more detail below in conjunction with embodiments.

[0021] All hot metal used in converter smelting is pre-desulfurized hot metal: hot metal S: 0.03%, P: 0.115%, hot metal temperature: 1305℃; converter endpoint control requirements: C: 0.04%, P: 0.011%, steel tapping temperature: 1635℃;

[0022] LF refining in place: Al in molten steel is controlled at 0.035%; LF refining process slag basicity (R = CaO / SiO2) is controlled at 5.0, the (FeO + MnO) content in the slag is controlled to be less than 0.9%, and the white slag is kept for 17 minutes; VD vacuum treatment: the vacuum degree is maintained at 40Pa for 26 minutes, and the soft blowing time is 20min; continuous casting process control: argon gas replacement of the tundish before casting, protective casting is used in the casting process, alkaline covering agent is used for the tundish covering agent, weak cooling is used for the secondary cooling water, electromagnetic stirring is used for the crystallizer and the solidification end, the continuous casting speed is controlled at 1.0m / min, and the superheat of the molten steel is 28℃. The continuous casting billet is quickly off the line, and the billet enters the slow cooling pit for cooling, and the slow cooling time is 72 hours; the continuous casting billet temperature is 80℃ out of the slow cooling pit.

[0023] The above process produces a Φ390mm X52QH round tube for pure hydrogen transportation, whose chemical composition mass percentage is: C 0.05-0.07%, Si 0.20-0.35%, Mn 0.95-1.25%, Cr 0.15-0.30%, Mo 0.08-0.15%, P≤0.015%, S≤0.003%, Pb≤0.002%, Ti≤0.0025%, and the rest is iron and trace impurity elements.

[0024] Table 1 Chemical composition content of each example (%)

[0025] Example C Si Mn P S Cr Mo Ti Pb Example 1 0.06 0.25 1.13 0.011 0.002 0.18 0.10 0.015 0.0008 Example 2 0.05 0.24 1.14 0.010 0.003 0.20 0.11 0.017 0.0010 Example 3 0.06 0.26 1.16 0.09 0.003 0.21 0.11 0.19 0.0011

[0026] Table 2 Gas content of each example (PPm)

[0027] Example H O N Example 1 0.89 18 40 Example 2 0.85 15 42 Example 3 0.75 20 39

[0028] The hot acid test ratings of the embodiments are shown in Table 3.

[0029] Table 3 Hot acid test rating results for each example

[0030]

[0031] The non-metallic inclusion detection results of each embodiment are shown in Table 4.

[0032] Table 4 Non-metallic inclusion detection and rating results for each example

[0033] Example A-type fine series B-type fine system C-type D-type fine system DS series Example 1 0.5 1.0 0 0.5 0 Example 2 0.5 0.5 0 0.5 0 Example 3 0.5 0.5 0 0.5 0

[0034] The results of the hot acid low magnification photos of each embodiment are shown in Figure 1 , Figure 2 , Figure 3 .

[0035] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A production and smelting method of X52QH round tube billet with a diameter of Φ390 mm for pure hydrogen transportation, characterized in that: The production process includes molten iron pretreatment, converter smelting, LF refining, VD vacuum degassing and round billet continuous casting; among which: All hot metal used in converter smelting is pre-desulfurized hot metal: hot metal requirements are S≤0.05%, P≤0.12%, and hot metal temperature≥1300℃; converter endpoint control requirements: C≤0.05%, P≤0.012%, and steel tapping temperature≥1630℃; LF refining in-place requirements: molten steel Al is controlled at around 0.030%; LF refining process slag basicity is controlled at 3.0-4.5, the (FeO+MnO) content in the slag is controlled to be <1%, and the white slag retention time is ≥15 minutes; VD vacuum treatment requirements: keep the vacuum degree ≤0.KPa for ≥25 minutes, soft blowing time ≥15min; continuous casting process control requirements: replace the tundish with argon before casting, use protective casting during the casting process, use alkaline covering agent for the tundish, use weak cooling for the secondary cooling water, use electromagnetic stirring for the crystallizer and the solidification end, control the continuous casting speed at 0.5m / min~1.0m / min, and the superheat of the molten steel ≤30℃; The chemical composition of the tube blank is as follows: C 0.05-0.07%, Si 0.20-0.35%, Mn 0.95-1.25%, Cr 0.15-0.30%, Mo 0.08-0.15%, P≤0.015%, S≤0.003%, Pb≤0.002%, Ti≤0.0025%, and the rest are iron and trace impurity elements.

2. The production and smelting method of Φ390mm X52QH round tube for pure hydrogen transportation according to claim 1 is characterized in that: The continuous casting billet is quickly rolled off the production line and sent into a slow cooling pit for cooling. The slow cooling time is ≥ 72 hours. The continuous casting billet temperature is < 100°C before leaving the slow cooling pit.

3. The production and smelting method of Φ390mm X52QH round tube for pure hydrogen transportation according to claim 1 is characterized in that: The results of sulfur print test of steel billets are all level 0-1; the non-metallic inclusions of steel billets are level 0-1; the gas oxygen content in the steel billets is 15-25PPm, and the material has good deep processing performance and safety of use.

4. The method for producing and smelting Φ390 mm X52QH round tube for pure hydrogen transportation according to claim 1, characterized in that: The chemical composition of the tube blank is as follows by mass percentage: C 0.06%, Si 0.25%, Mn 1.13%, Cr 0.18%, Mo0.10%, P 0.011%, S 0.002%, Pb 0.0008%, Ti 0.0015%, and the rest is iron and trace impurity elements.

5. The method for producing and smelting Φ390 mm X52QH round tube for pure hydrogen transportation according to claim 1 is characterized in that: The chemical composition of the tube blank is as follows: C 0.05%, Si 0.24%, Mn 1.14%, Cr 0.20%, Mo0.11%, P 0.010%, S 0.003%, Pb 0.0010%, Ti 0.0017%, and the rest are iron and trace impurity elements.

6. The method for producing and smelting Φ390 mm X52QH round tube for pure hydrogen transportation according to claim 1, characterized in that: The chemical composition of the tube blank is as follows: C 0.06%, Si 0.26%, Mn 1.16%, Cr 0.21%, Mo 0.11%, P 0.09%, S 0.003%, Pb 0.0011%, Ti 0.0019%, and the rest are iron and trace impurity elements.

Citation Information

Patent Citations

  • X70 pipeline steel with hydrogen sulfide corrosion resistance for longitudinal welded pipe and production method of X70 pipeline steel

    CN104818427A

  • High-toughness ferrite type hot continuous rolling steel band for oil-gas pipeline and production method of high-toughness ferrite type hot continuous rolling steel band

    CN109182922A

  • Solid welding wire for low-pressure hydrogen-doped fuel gas conveying pipeline and preparation method of solid welding wire

    CN116586818A

  • Production and smelting method of phi 430 mm hydrogen transmission pipeline round pipe blank

    CN116623065A

  • Production and smelting method of phi 350mm rare earth-containing bearing circular tube blank

    CN118147509A