Method for improving adhesion of zinc layer of hot-dip galvanized strip steel
By removing the grease and oxides on the surface of the strip through cleaning and annealing, combined with nitrogen and hydrogen atmosphere and temperature control of the zinc liquid, the problem of insufficient adhesion of the zinc layer in hot-dip galvanizing is solved, and the phenomenon of missed plating and dezincification is significantly reduced. , improving the quality and adhesion of the finished product.
Patent Information
- Application Number
- CN202410918662.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-15
AI Technical Summary
During the hot-dip galvanizing production process, missing plating defects and dezincification during the stamping and molding process of the finished product are prone to occur, resulting in insufficient adhesion of the zinc layer.
Remove surface grease by cleaning the strip, conduct heating and soaking annealing in a nitrogen-hydrogen mixed gas, set different dew point temperatures to reduce oxide production and prevent oxidation, and then galvanize in the zinc liquid at the set temperature, at the furnace nose Set a third dew point temperature to reduce zinc dust production.
It improves the adhesion of the zinc layer, reduces missing plating defects and dezincification, and ensures the surface quality and adhesion of the finished product.
Smart Images

Figure CN118773532A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of steel galvanizing, and in particular to a method for improving the adhesion of a zinc layer of a hot-dip galvanized steel strip. Background Art
[0002] Cold-rolled hot-dip galvanized products are steel strips that have been coated with an alloy layer after passing through zinc liquid. The galvanizing process seriously affects the surface quality of cold-rolled hot-dip galvanized products.
[0003] At present, the hot-dip galvanizing production process is prone to plating defects and dezincification during the stamping process of the finished product. Summary of the invention
[0004] The present application provides a method for improving the adhesion of the zinc layer of hot-dip galvanized steel strip to solve the following technical problem: how to improve the adhesion of the zinc layer of hot-dip galvanized steel strip.
[0005] In a first aspect, the present application provides a method for improving the adhesion of a zinc layer of a hot-dip galvanized steel strip, the method comprising:
[0006] Cleaning the steel strip and controlling the cleaning process parameters to remove grease on the surface of the steel strip;
[0007] Under the condition of nitrogen-hydrogen mixed gas with a set hydrogen content, the cleaned steel strip is annealed including a heating stage and a soaking stage to obtain an annealed steel strip; wherein the heating stage and the soaking stage have a first dew point temperature, and the remaining stage of the annealing has a second dew point temperature;
[0008] The annealed steel strip is galvanized to obtain a hot-dip galvanized steel strip; wherein the galvanized furnace nose has a third dew point temperature.
[0009] Optionally, the first dew point temperature is (-60)°C to (-30)°C.
[0010] Optionally, the second dew point temperature is (-25)°C to (-20)°C.
[0011] Optionally, the third dew point temperature is (-15)°C to (-50)°C.
[0012] Optionally, the hydrogen content is set to be 3 volume % to 10 volume %.
[0013] Optionally, based on a single side of the strip, the cleaning process parameters include: the total amount of residue on the strip at the end of cleaning is less than 20 mg / m 2 ; wherein the residue includes residual iron and residual oil, and the content of the residual iron is ≤10mg / m 2 The content of the residual oil is ≤10mg / m 2 .
[0014] Optionally, the annealed steel strip is galvanized to obtain a hot-dip galvanized steel strip, comprising:
[0015] The annealed steel strip is galvanized using a zinc solution with a set aluminum content and a set temperature to obtain a hot-dip galvanized steel strip.
[0016] Optionally, the set aluminum content is 0.2 wt% to 0.3 wt%, and the set temperature is 450°C to 460°C.
[0017] Optionally, the initial galvanizing temperature of the annealed steel strip is 440°C to 475°C.
[0018] Optionally, the carbon content in the steel strip is 0.05 wt % to 0.15 wt %.
[0019] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0020] The method for improving the adhesion of the zinc layer of hot-dip galvanized steel strip provided in an embodiment of the present application comprises: cleaning the steel strip and controlling the process parameters of the cleaning to remove grease on the surface of the steel strip; annealing the cleaned steel strip in a nitrogen-hydrogen mixed gas with a set hydrogen content, including a heating stage and a soaking stage, to obtain an annealed steel strip; wherein the heating section and the soaking section have a first dew point temperature, and the remaining stage of the annealing has a second dew point temperature; galvanizing the annealed steel strip to obtain a hot-dip galvanized steel strip; wherein the galvanized furnace nose has a third dew point temperature. The strip is cleaned and the cleaning process parameters are controlled to remove grease on the surface of the strip, which can promote the formation of the Fe2Al5 intermediate adhesion layer in the coating during the subsequent galvanizing process, thereby improving the adhesion of the coating; in the annealing process, the first dew point temperature is set in the heating stage and the soaking stage, and the second dew point temperature is set in the remaining stages. The dew point temperatures are set according to the temperatures of the strip in different stages of annealing, which can effectively reduce the generation of oxides on the surface of the strip. At the same time, a nitrogen-hydrogen mixed gas with a set hydrogen content is used to effectively prevent the strip from being oxidized, and to better reduce the oxidized strip, thereby obtaining a strip with good surface quality, thereby further promoting the formation of the Fe2Al5 intermediate adhesion layer in the coating during the subsequent galvanizing process, thereby improving the adhesion of the coating; the furnace nose is in direct contact with the zinc liquid surface, and the galvanizing furnace nose is set to the third dew point temperature, which can reduce the oxidation of the strip surface and reduce the volatilization of zinc, thereby reducing the generation of zinc ash at the furnace nose and improving the adhesion of the zinc liquid to the strip. In summary, the defects of missed plating in the hot-dip galvanizing production process are reduced, the adhesion of the zinc layer of the hot-dip galvanized strip is improved, and the dezincification in the stamping process of the finished product is reduced, which provides a guarantee for the product quality of the subsequent production line. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0023] Figure 1 A schematic flow chart of a method for improving the adhesion of a zinc layer of a hot-dip galvanized steel strip according to some embodiments of the present application;
[0024] Figure 2 A schematic diagram of the cross-sectional structure of a zinc layer of a hot-dip galvanized steel strip provided according to some embodiments of the present application;
[0025] Figure 3 A picture of zinc layer dezincification after hot-dip galvanized steel strip stamping provided according to some embodiments of the present application;
[0026] Figure 4 This is a picture of the surface of the zinc layer of a hot-dip galvanized steel strip after stamping provided in Example 1 of the present application;
[0027] Figure 5 This is a picture of the surface of the zinc layer of a hot-dip galvanized steel strip after stamping provided in Example 2 of the present application;
[0028] Figure 6 This is a picture of the surface of the zinc layer of a hot-dip galvanized steel strip after stamping provided in Example 3 of the present application;
[0029] Figure 7 This is a picture of the zinc layer surface of a hot-dip galvanized steel strip provided in Comparative Example 1 of the present application;
[0030] Figure 8 This is a picture of the zinc layer surface of a hot-dip galvanized steel strip after stamping provided in Comparative Example 2 of the present application. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0032] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0033] In this application, the terms "include", "comprising", etc. mean "including but not limited to". In this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations.
[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0035] Figure 1 A schematic diagram of a method for improving the adhesion of the zinc layer of hot-dip galvanized steel strip according to some embodiments of the present application; see Figure 1 The present application provides a method for improving the adhesion of a zinc layer of a hot-dip galvanized steel strip, the method comprising:
[0036] S1, cleaning the steel strip and controlling the cleaning process parameters to remove grease on the surface of the steel strip;
[0037] In some embodiments, the cleaning process parameters include: the total amount of residue on the strip at the end of cleaning is less than 20 mg / m 2 ; wherein the residue includes residual iron and residual oil, and the content of the residual iron is ≤10mg / m 2 The content of the residual oil is ≤10mg / m 2 .
[0038] In the embodiment of the present application, before step S1, after the steel strip is pickled and pickled, there is a lot of grease residue on the surface, which will hinder the formation of the Fe2Al5 adhesion layer and reduce the adhesion of the subsequent hot-dip galvanized coating. For example, the total amount of residue on the steel strip at the end of the cleaning process can be 19 mg / m 2 , 18mg / m 2 , 17mg / m 2 , 16mg / m2 , 15mg / m 2 The residual iron content can be 10mg / m 2 , 9mg / m 2 , 8mg / m 2 , 7mg / m 2 , 6mg / m 2 etc., the residual oil content can be 10mg / m 2 , 9mg / m 2 , 8mg / m 2 , 7mg / m 2 , 6mg / m 2 wait.
[0039] In some embodiments, the carbon content in the steel strip is 0.05 wt % to 0.15 wt %.
[0040] In the embodiment of the present application, the Fe-Zn reaction in the steel strip with a high carbon content is violent, so that the iron-zinc alloy layer is thickened, while the Fe2Al5 adhesion layer generated is thin, causing problems such as missed plating, dezincification, slag inclusion, etc., resulting in reduced adhesion of the iron-zinc alloy layer. Exemplarily, the carbon content in the above steel strip can be 0.05 weight%, 0.07 weight%, 0.09 weight%, 0.11 weight%, 0.13 weight%, 0.15 weight%, etc. In addition, the chemical composition of the steel strip can also include: Si content <0.07 weight%, Al content 0.01-0.03 weight%.
[0041] S2. Under the condition of nitrogen-hydrogen mixed gas with a set hydrogen content, annealing the cleaned steel strip including a heating stage and a soaking stage to obtain an annealed steel strip; wherein the heating stage and the soaking stage have a first dew point temperature, and the remaining stage of the annealing has a second dew point temperature;
[0042] In some embodiments, the first dew point temperature is (-60)°C to (-30)°C.
[0043] In some embodiments, the second dew point temperature is (-25)°C to (-20)°C.
[0044] In some embodiments, the third dew point temperature is (-15)°C to (-50)°C.
[0045] In some embodiments, the set hydrogen content is 3 volume % to 10 volume %.
[0046] In the embodiment of the present application, the annealing process is divided into a preheating section, a heating section, a soaking section, a slow cooling section, a rapid cooling section and a balancing section. The first dew point temperature is set in the heating stage and the soaking stage with a higher temperature, and the lower dew point temperature reduces the degree of oxidation reaction on the surface of the strip in the furnace. The temperature of the remaining stages (preheating section, slow cooling section, rapid cooling section and balancing section) is relatively low, and a higher second dew point temperature is set. Therefore, the dew point temperature is set according to the temperature of the strip in different stages of annealing to reduce the occurrence of oxidation reaction on the surface of the strip during annealing, which can effectively reduce the generation of oxides on the surface of the strip. At the same time, the use of a nitrogen-hydrogen mixed gas with a set hydrogen content can effectively prevent the strip from being oxidized and better reduce the oxidized strip, thereby obtaining a strip with good surface quality, thereby further promoting the formation of an Fe2Al5 intermediate adhesion layer in the coating during the subsequent galvanizing process, thereby improving the adhesion of the coating. Exemplarily, the first dew point temperature may be -60°C, -55°C, -50°C, -45°C, -40°C, -35°C, -30°C, etc., the second dew point temperature may be -25°C, -24°C, -23°C, -22°C, -21°C, -20°C, etc., and the set hydrogen content may be 3 volume%, 4 volume%, 5 volume%, 6 volume%, 7 volume%, 10 volume%.
[0047] S3. Galvanizing the annealed steel strip to obtain hot-dip galvanized steel strip; wherein the galvanized furnace nose has a third dew point temperature.
[0048] In the embodiment of the present application, the furnace nose is a channel connecting the annealing furnace and the galvanizing area. The furnace nose is in direct contact with the surface of the zinc liquid. The galvanized furnace nose is set to the third dew point temperature, which can prevent the strip from being oxidized before entering the zinc pot, reduce the generation of iron oxide film on the surface of the strip, that is, form a barrier layer, enhance the good wetting of the strip with the zinc liquid after immersing in the zinc pot, enhance the adhesion of the zinc layer, and reduce the volatilization of zinc, thereby reducing the generation of zinc ash at the furnace nose and improving the adhesion of the zinc liquid to the strip. Exemplarily, the above-mentioned third dew point temperature can be -15°C, -18°C, -20°C, -22°C, -25°C, -50°C, -45°C, -40°C, -35°C, -30°C, etc.
[0049] In some embodiments, the annealed steel strip is galvanized to obtain a hot-dip galvanized steel strip, comprising:
[0050] The annealed steel strip is galvanized using a zinc solution with a set aluminum content and a set temperature to obtain a hot-dip galvanized steel strip.
[0051] In some embodiments, the set aluminum content is 0.2 wt% to 0.3 wt%, and the set temperature is 450°C to 460°C.
[0052] In the embodiment of the present application, after the strip passes through the zinc liquid, a coating will be produced. Since the iron-zinc alloy layer is hard and brittle, it has poor adhesion to the steel substrate. Adding Al elements and strictly controlling the aluminum content in the zinc liquid will play a role in isolating the steel substrate from zinc, hindering the diffusion of Fe into Zn, and preventing the formation of Fe-Zn compounds, thereby increasing the thickness of the Fe2Al5 adhesion layer and improving the adhesion performance of the zinc layer. In addition, when the zinc liquid temperature exceeds 480°C, the iron loss increases sharply in a parabolic manner, reaching a maximum when the zinc liquid temperature is about 500°C. At this time, the amount of bottom slag produced per unit time is also the largest, so the above-mentioned zinc liquid temperature is limited. Exemplarily, the aluminum content in the above-mentioned zinc liquid can be 0.2% by weight, 0.22% by weight, 0.24% by weight, 0.26% by weight, 0.30% by weight, etc., and the above-mentioned zinc liquid temperature can be 450°C, 452°C, 454°C, 456°C, 458°C, 460°C, etc.
[0053] In some embodiments, the initial galvanizing temperature of the annealed steel strip is 440°C to 475°C.
[0054] In the embodiment of the present application, the initial galvanizing temperature of the annealed steel strip is limited, that is, the temperature of the steel strip entering the zinc pot, and the temperature fluctuation of the zinc liquid is reduced, which can ensure the thickness of the Fe2Al5 adhesion layer, and at the same time reduce the heat of the steel strip entering the zinc liquid, reduce iron loss, and avoid the thickening of the Fe-Zn alloy layer, thereby improving the adhesion of the coating. Exemplarily, the initial galvanizing temperature of the annealed steel strip can be 440°C, 445°C, 460°C, 465°C, 470°C, 475°C, etc. Figure 2 This is a schematic diagram of the cross-sectional structure of a zinc layer of a hot-dip galvanized steel strip provided according to some embodiments of the present application; see Figure 2 , showing the coating structure of the embodiment of the present application.
[0055] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0056] Example 1
[0057] A method for improving the adhesion of the zinc layer of hot-dip galvanized steel strip, comprising: a galvanizing unit production specification of 1.5*905mm (thickness*width)
[0058] (1) Strip material composition control: The chemical composition of the steel strip raw material requires C content of 0.15%, Si content of 0.06%, and Al content of 0.015%;
[0059] (2) Strip surface cleanliness control: The residual iron on the strip surface after the cleaning section is 5 mg / m 2 (single side), residual oil content 6mg / m 2 (single side), total residue 15mg / m 2 (single-sided);
[0060] (3) Furnace atmosphere control: the dew point in the heating section and soaking section is -45°C, the other stages are -20°C, the dew point at the furnace nose is -25°C, and the hydrogen content in the nitrogen-hydrogen mixed gas in the furnace is 7%;
[0061] (4) Zinc liquid temperature control: The optimal zinc liquid temperature during production is 455°C;
[0062] (5) Temperature control of the strip entering the zinc pot: The temperature of the strip entering the zinc pot is 440℃.
[0063] (6) Zinc liquid composition control: The aluminum content in the zinc liquid is 0.225%.
[0064] Example 2
[0065] A method for improving the adhesion of the zinc layer of hot-dip galvanized steel strip, comprising: a galvanizing unit production specification of 0.8*1415 (thickness*width),
[0066] (1) Strip material composition control: The chemical composition of the steel strip raw material requires C content of 0.05%, Si content of 0.05%, and Al content of 0.02%;
[0067] (2) Strip surface cleanliness control: After the strip passes through the cleaning section, the residual iron on the surface is 4 mg / m 2 (single side), residual oil content 5mg / m 2 (single side), total residue 12mg / m 2 (single-sided);
[0068] (3) Furnace atmosphere control: the dew point in the heating section and soaking section is -40°C, the dew point in the other stages is -25°C, the dew point at the furnace nose is -25°C, and the hydrogen content in the nitrogen-hydrogen mixed gas in the furnace is controlled at 4%;
[0069] (4) Zinc liquid temperature control: The optimal zinc liquid temperature during production is 452°C
[0070] (5) Temperature control of the strip entering the zinc pot: The temperature of the strip entering the zinc pot is 470℃.
[0071] (6) Zinc liquid composition control: The aluminum content in the zinc liquid is 0.230%.
[0072] Example 3
[0073] A method for improving the adhesion of the zinc layer of hot-dip galvanized steel strip, comprising: a galvanizing unit production specification of 0.8*1415 (thickness*width),
[0074] (1) Strip material composition control: The chemical composition of the steel strip raw material requires C content of 0.10%, Si content of 0.05%, and Al content of 0.03%;
[0075] (2) Strip surface cleanliness control: The residual iron on the strip surface after the cleaning section is 5 mg / m 2 (single side), residual oil content 5mg / m 2 (single side), total residue 13mg / m 2 (single-sided);
[0076] (3) Furnace atmosphere control: the dew point in the heating section and soaking section is -50°C, the dew point in the other stages is -22°C, the dew point at the furnace nose is -30°C, and the hydrogen content in the nitrogen-hydrogen mixed gas in the furnace is controlled at 9%;
[0077] (4) Zinc liquid temperature control: The optimal zinc liquid temperature during production is 455°C
[0078] (5) Temperature control of the strip entering the zinc pot: The temperature of the strip entering the zinc pot is 460℃.
[0079] (6) Zinc liquid composition control: The aluminum content in the zinc liquid is 0.3%.
[0080] Comparative Example 1
[0081] A method for improving the adhesion of the zinc layer of hot-dip galvanized steel strip, comprising: a galvanizing unit production specification of 1.5*905mm (thickness*width)
[0082] (1) Strip material composition control: The chemical composition of the steel strip raw material requires C content of 0.15%, Si content of 0.06%, and Al content of 0.015%;
[0083] (2) Strip surface cleanliness control: The residual iron on the strip surface after the cleaning section is 15 mg / m 2 (single side), residual oil content 13mg / m 2 (single side), total residue 30mg / m 2 (single-sided);
[0084] (3) Furnace atmosphere control: the dew point in the heating section and soaking section is -45°C, the other stages are -20°C, the dew point at the furnace nose is -25°C, and the hydrogen content in the nitrogen-hydrogen mixed gas in the furnace is 7%;
[0085] (4) Zinc liquid temperature control: The optimal zinc liquid temperature during production is 455°C;
[0086] (5) Temperature control of the strip entering the zinc pot: The temperature of the strip entering the zinc pot is 440℃.
[0087] (6) Zinc liquid composition control: The aluminum content in the zinc liquid is 0.225%.
[0088] Comparative Example 2
[0089] A method for improving the adhesion of the zinc layer of hot-dip galvanized steel strip, comprising: a galvanizing unit production specification of 1.5*905mm (thickness*width)
[0090] (1) Strip material composition control: The chemical composition of the steel strip raw material requires C content of 0.15%, Si content of 0.06%, and Al content of 0.015%;
[0091] (2) Strip surface cleanliness control: The residual iron on the strip surface after the cleaning section is 5 mg / m 2 (single side), residual oil content 6mg / m 2 (single side), total residue 15mg / m 2 (single-sided);
[0092] (3) Furnace atmosphere control: the dew point in the heating section and soaking section is -20°C, the other stages are -10°C, the dew point at the furnace nose is -10°C, and the hydrogen content in the nitrogen-hydrogen mixed gas in the furnace is 2%;
[0093] (4) Zinc liquid temperature control: The optimal zinc liquid temperature during production is 455°C;
[0094] (5) Temperature control of the strip entering the zinc pot: The temperature of the strip entering the zinc pot is 440℃.
[0095] (6) Zinc liquid composition control: The aluminum content in the zinc liquid is 0.225%.
[0096] To verify the adhesion of the zinc layer, a bending test was conducted on the strip steel under simulated stamping conditions, and the adhesion of the zinc layer was reflected by the appearance of the zinc layer after bending. The adhesion of the zinc layer was verified by observing whether there was dezincification at the stamping location. Please refer to the evaluation results of the zinc layer adhesion of hot-dip galvanized strip steel shown in Table 1.
[0097] Table 1 Evaluation results of zinc layer adhesion of hot-dip galvanized steel strip
[0098]
[0099] Through Table 1 and combined Figure 3 to Figure 8 , exemplary, Figure 3 This is a picture of zinc layer dezincification after hot-dip galvanized steel strip stamping according to some embodiments of the present application; please see Figure 3 , indicating the typical dezincification phenomenon produced during stamping; Figure 4This is a picture of the surface of the zinc layer of a hot-dip galvanized steel strip after stamping provided in Example 1 of the present application; Figure 5 This is a picture of the surface of the zinc layer of a hot-dip galvanized steel strip after stamping provided in Example 2 of the present application; Figure 6 This is a picture of the zinc layer surface of a hot-dip galvanized steel strip after stamping provided in Example 3 of the present application; see Figures 4 to 6 , indicating that the surface of the zinc layer of the hot-dip galvanized steel strip in the embodiment of the present application is intact after stamping, and there is no obvious dezincification phenomenon; Figure 7 This is a picture of the zinc layer surface of a hot-dip galvanized steel strip provided according to Comparative Example 1 of the present application; see Figure 7 , indicating that the cleaning process in the embodiment of the present application was not adopted, resulting in the residual oil and grease in the hot-dip galvanized strip, which led to poor adhesion of the zinc layer of the strip. Figure 8 This is a picture of the zinc layer surface of a hot-dip galvanized steel strip after stamping provided in Comparative Example 2 of this application; please refer to Figure 8 , indicating that the dew point control process in the embodiment of the present application was not adopted, so that the zinc layer on the surface of the hot-dip galvanized steel strip fell off after stamping, and the adhesion was relatively poor.
[0100] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for improving the adhesion of the zinc layer of hot-dip galvanized steel strip, It is characterized in that The method comprises: Cleaning the steel strip and controlling the cleaning process parameters to remove grease on the surface of the steel strip; Under the condition of nitrogen-hydrogen mixed gas with a set hydrogen content, the cleaned steel strip is annealed including a heating stage and a soaking stage to obtain an annealed steel strip; wherein the heating stage and the soaking stage have a first dew point temperature, and the remaining stage of the annealing has a second dew point temperature; The annealed steel strip is galvanized to obtain a hot-dip galvanized steel strip; wherein the galvanized furnace nose has a third dew point temperature.
2. The method according to claim 1, It is characterized in that The first dew point temperature is (-60)°C to (-30)°C.
3. The method according to claim 1, It is characterized in that The second dew point temperature is (-25)°C to (-20)°C.
4. The method according to claim 1, It is characterized in that The third dew point temperature is (-15)°C to (-50)°C.
5. The method according to claim 1, It is characterized in that The set hydrogen content is 3 volume % to 10 volume %.
6. The method according to claim 1, It is characterized in that Based on the single side of the strip, the cleaning process parameters include: The total amount of residues on the strip at the end of cleaning is <20mg / m 2 ; wherein the residue includes residual iron and residual oil, The residual iron content is ≤10mg / m 2 The content of the residual oil is ≤10mg / m 2 .
7. The method according to claim 1, It is characterized in that The annealed steel strip is galvanized to obtain a hot-dip galvanized steel strip, comprising: The annealed steel strip is galvanized using a zinc solution with a set aluminum content and a set temperature to obtain a hot-dip galvanized steel strip.
8. The method according to claim 7, It is characterized in that The set aluminum content is 0.2 wt% to 0.3 wt%, and the set temperature is 450°C to 460°C.
9. The method according to claim 1 or 7, It is characterized in that The initial galvanizing temperature of the annealed steel strip is 440°C to 475°C.
10. The method according to claim 1, It is characterized in that The carbon content in the steel strip is 0.05 wt % to 0.15 wt %.