Silver-white composite coating and preparation method thereof

By using a multi-target magnetron sputtering process to form amorphous Ti, Al, and Ag alloy layers on watch exterior parts, the problem of insufficient hardness and corrosion resistance of the silver-white coating in the existing technology is solved, and high hardness and corrosion resistance are achieved. Wear-resistant and bio-friendly silver-white coating, and reduces costs.

CN118773547APending Publication Date: 2024-10-15FIYTA HOLDINGS LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410836084.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult to achieve high hardness, wear resistance, corrosion resistance and bio-friendly silver-white coating on watch appearance parts with existing technology, and the cost is high.

Method used

A multi-target magnetron sputtering process is used to form an amorphous Ti, Al, and Ag alloy layer on the surface of the substrate. Through the combination of the base layer and the surface layer, the thickness and particle size of the coating are controlled, and the titanium alloy and water cooling system are combined to Improve the bonding strength and heat resistance of the coating.

Benefits of technology

A silver-white coating with high hardness, corrosion resistance, bio-friendliness, wear and scratch resistance, and low cost is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773547A_ABST
    Figure CN118773547A_ABST
Patent Text Reader

Abstract

The invention discloses a silver composite coating and a preparation method thereof, and belongs to the technical field of material processing. The coating comprises a base layer and a surface layer, the surface layer is a Ti, Al and Ag amorphous alloy layer, and the main component of the base layer is Ti. The coating is prepared by adopting a multi-target magnetron sputtering process, so that the process flow is simple, the components are easier to control, and the plating quality is higher; the product deposited with the base layer is placed in a water cooling system, and the supercooling degree caused by the water cooling system can promote formation of an amorphous alloy surface layer; an amorphous alloy surface layer containing expected components is obtained by controlling parameters such as current and pulse bias voltage of each cathode electron gun; and the thickness and the particle size of the coating are indirectly controlled by controlling process parameters, so that the coating has the required appearance effect and performance. The coating prepared by the scheme has silver white color, and the surface layer is made of amorphous alloy, so that the coating has good corrosion resistance, biological friendliness, high hardness, good wear resistance and scratch resistance and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material processing, and in particular to a silvery white composite coating and a preparation method thereof. Background Art

[0002] Watch cases, bezels, and straps are the main exterior parts of watches, and they have many performance requirements for materials, such as wear resistance, corrosion resistance, scratch resistance, and color. Silvery white is the mainstream color demand in the watch exterior parts industry. In order to meet this color demand and corrosion resistance demand, and comprehensively consider processing performance and cost, there are not many types of materials that can be widely used in watch exterior parts. The most commonly used metal materials are stainless steel and titanium alloy. Stainless steel has low hardness, poor scratch resistance, and contains a certain amount of nickel, which can cause skin allergies in some people. Although titanium alloy is slightly harder than stainless steel, it is dark in color and easily forms an oxide film on the surface, affecting the appearance.

[0003] In the prior art, applying a coating on the surface of a material to improve the various performances of the base material is a common technique in the field of industrial technology. In the watch industry, relatively mature coating systems have been applied, such as gold plating, titanium nitride plating, and diamond-like film plating, but these films are quite different from the color requirements of silver-white. Although pure metals such as chrome plating and platinum plating can achieve a silver-white appearance, these pure metals have low hardness, poor wear resistance, and high cost.

[0004] Therefore, it is necessary to develop a silver-white composite coating that is high in hardness, wear-resistant, corrosion-resistant, and bio-friendly. Summary of the invention

[0005] The technical problem to be solved by the present invention is: in view of the above-mentioned defects of the prior art, a silvery-white composite coating and a preparation method thereof are provided.

[0006] To achieve the above object, the present invention provides a silvery-white composite coating, the composite coating comprising a primer layer and a surface layer sequentially formed on the surface of a substrate, wherein:

[0007] The composition of the surface layer is 60-70% Ti, 0.5-2.5% Ag, and the balance is Al, in terms of mass percentage;

[0008] The base layer contains at least Ti, the mass percentage of which exceeds 70%;

[0009] The surface layer is amorphous.

[0010] Preferably, the particle size of the surface layer is 50nm to 200nm.

[0011] Preferably, the thickness of the surface layer is 0.8-5 um.

[0012] Preferably, the thickness of the base layer is 0.3-1.5 um.

[0013] Preferably, the thickness of the surface layer is 0.8-5 um, and the thickness of the base layer is 0.3-1.5 um.

[0014] The present invention also provides a method for preparing a silvery-white composite coating, wherein the silvery-white composite coating as described above is prepared on the surface of a substrate, and the method comprises the following steps:

[0015] Step S1, in an ultrasonic cleaning device, the substrate is cleaned with a wax removal solution, an oil removal solution and deionized water in sequence, and the substrate is blown dry after cleaning;

[0016] Step S2, using a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reaction furnace and an inert gas introduction device to perform secondary cleaning on the substrate after ultrasonic cleaning;

[0017] Step S3, using a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reaction furnace, an inert gas introduction device and two cathode targets to deposit a base layer on the surface of the substrate; the two cathode targets are titanium alloys with a titanium content greater than 70%; the inert gas introduction device is connected to argon or nitrogen;

[0018] The specific process parameters are as follows:

[0019] Maintaining the vacuum degree in the reaction furnace at 0.1-1 Pa;

[0020] The current of the cathode electron gun is 15 to 30A;

[0021] The pulse negative bias voltage applied to the substrate is -150 to -100 V;

[0022] The working time is 20 to 50 minutes, and the temperature does not exceed 200°C;

[0023] Step S4, using a magnetron sputtering furnace equipped with a water cooling system, a cathode electron gun, an anode, a reaction furnace, an inert gas introduction device and four cathode targets, depositing a surface layer on the surface of the primer layer; the four cathode targets are respectively two pure titanium targets, one aluminum alloy target containing 2-8% Ag and one pure aluminum target; the inert gas introduction device is connected to argon or nitrogen; firstly, the substrate product with the primer layer deposited is placed on a water cooling sample table, and the water cooling system is started; and then the surface layer deposition treatment is performed under the following process parameter conditions:

[0024] Maintaining the vacuum degree in the reaction furnace at 0.05-0.5 Pa;

[0025] The cathode electron gun current I 纯钛 5~7A, I铝合金 6~8A, I 纯铝 6~8A;

[0026] The pulse negative bias voltage applied to the substrate is -180 to -120 V;

[0027] The working time is 3 to 6 hours and the temperature does not exceed 300°C.

[0028] Preferably, in step S1, the ultrasonic cleaning time is 5 to 7 minutes, the cleaning temperature is 50 to 60°C, the ratio of the wax removal solution is wax removal water: pure water = 1:8 to 1:16, and the ratio of the oil removal solution is oil removal agent: pure water = 1:15 to 1:30.

[0029] Preferably, in step S2, the cleaning conditions are as follows:

[0030] The inert gas introduction device is connected to argon or nitrogen;

[0031] Maintain the vacuum degree in the reaction furnace at (8.0-15.0)×10 -3 Pa;

[0032] The current of the cathode electron gun is 120-160A;

[0033] The pulse negative bias voltage applied to the substrate is -400 to -500 V;

[0034] The working time is 5 to 10 minutes.

[0035] The present invention has the following beneficial effects: the coating of the present scheme is composed of a base layer and a surface layer, the surface layer is a Ti, Al, Ag amorphous alloy layer, and the main component of the base layer is Ti. The composition of the titanium alloy and the TiAl surface layer is similar, and the bonding force between the two is stronger to prevent the TiAl surface layer from peeling off. Ag can improve the heat resistance and oxidation resistance of the aluminum alloy, prevent the generation of black spots during the sputtering process, and reduce the surface roughness of the coating. The base layer and the surface layer are prepared by a multi-target magnetron sputtering process, and the process flow is simple, the composition is easier to control, and the coating quality is higher; the product with the base layer deposited is placed in the water cooling system of the magnetron sputtering furnace, and the supercooling caused by the water cooling system can promote the formation of the amorphous alloy surface layer; by controlling the current and pulse bias parameters of each cathode electron gun, the deposition rate of various materials is different, and an amorphous alloy surface layer with a silvery white luster and containing the expected composition is obtained; the thickness and particle size of the coating are indirectly controlled by controlling the process parameters, so that the coating has the desired appearance effect and performance. The coating prepared by the present scheme has a silvery white color, and the surface layer is an amorphous alloy, so it has good corrosion resistance, is bio-friendly, has high hardness, good wear resistance and scratch resistance, and is low in cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0037] Figure 1 A schematic diagram of the structure of the silvery-white composite coating provided in an embodiment of the present invention.

[0038] Figure 2 A schematic diagram of the steps of a method for preparing a silvery-white composite coating provided in an embodiment of the present invention.

[0039] Figure 3 This is a morphology image of the surface layer of the silvery-white composite coating prepared in Example 1 of the present invention under a scanning electron microscope.

[0040] Figure 4 This is an energy spectrum analysis diagram of the surface layer of the silver-white composite coating prepared in Example 2 of the present invention.

[0041] Figure 5 This is a graph showing the XRD phase analysis results of the surface layer of the silvery-white composite coating prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] The embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings of the specification. It should be understood that the embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0044] The silver-white composite coating provided by the present invention is suitable for being applied to the surface of watch exterior parts such as watch cases, bezels, and watch straps, so that these exterior parts appear silver-white and meet the requirements of high hardness, wear resistance, corrosion resistance, and bio-friendliness. The silver-white composite coating provided by the present invention is also suitable for other products that require silver-white exterior parts that meet the requirements of high hardness, wear resistance, corrosion resistance, and bio-friendliness.

[0045] like Figure 1 As shown, an embodiment of the present invention provides a silvery-white composite coating, the composite coating comprising a primer layer and a surface layer sequentially formed on the surface of a substrate, wherein:

[0046] The composition of the surface layer is 60-70% Ti, 0.5-2.5% Ag, and the balance is Al, in terms of mass percentage;

[0047] The base layer contains at least Ti, the mass percentage of which exceeds 70%;

[0048] The surface layer is amorphous.

[0049] The particle size of the surface layer is 50nm to 200nm.

[0050] The present invention has no particular limitation on the thickness of the surface layer and the primer layer. In practical applications, the thickness of the surface layer and the primer layer is determined based on factors such as cost, efficiency, and durability.

[0051] In some embodiments of the present invention, the thickness of the surface layer is 0.8-5 um.

[0052] In some embodiments of the present invention, the thickness of the primer layer is 0.3-1.5 um.

[0053] In some embodiments of the present invention, the thickness of the surface layer is 0.8-5 um, and the thickness of the primer layer is 0.3-1.5 um.

[0054] In the embodiment of the present invention, the substrate refers to the watch case, watch strap, bezel, etc., and common materials thereof include 316L steel, titanium alloy, aluminum alloy, etc.

[0055] The appearance of the watch's exterior parts has extremely high requirements for appearance effects, and must be wear-resistant, corrosion-resistant, and bio-friendly. The surface layer of the composite coating provided in the embodiment of the present invention is an amorphous alloy layer whose main components are Ti, Al, and Ag, and its color is silvery white and bright. Compared with crystalline materials with the same components, amorphous materials have the advantages of high hardness, high strength, and good corrosion resistance. The nano-amorphous material coating of the embodiment of the present invention can make the nano-hardness of the coated surface as high as 750HVIT or more, while the nano-hardness of ordinary 316L stainless steel is only 400-550HVIT; the composite coating of the embodiment of the present invention has good wear resistance and scratch resistance, excellent corrosion resistance, and because the surface layer does not contain nickel, it is bio-friendly.

[0056] Among them, amorphous Ti and Al are used to provide silver-white visual effects and hardness, and the Ag element can improve the heat resistance and oxidation resistance of the aluminum alloy, prevent black spots from being generated during the sputtering process, and reduce the surface roughness of the coating.

[0057] The embodiment of the present invention limits the particle size of the surface layer to the range of 50nm-200nm because oversized particles will cause sand holes or pits on the coating surface, which will deteriorate its mechanical properties and appearance. However, the present invention does not impose any particular restrictions on the particle size. In practical applications, the particle size range can be fine-tuned according to actual conditions.

[0058] like Figure 2 As shown, the embodiment of the present invention also provides a method for preparing a silver-white composite coating, and the silver-white composite coating as described above is prepared on the surface of a substrate, and the method comprises the following steps:

[0059] Step S1, in an ultrasonic cleaning device, the substrate is cleaned with a wax removal solution, an oil removal solution and deionized water in sequence, and the substrate is blown dry after cleaning. The ultrasonic cleaning time is 5 to 7 minutes, the cleaning temperature is 50 to 60°C, the wax removal solution ratio is wax removal water: pure water = 1:8 to 1:16, and the oil removal solution ratio is oil removal agent: pure water = 1:15 to 1:30.

[0060] Step S2, using a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reaction furnace and an inert gas supply device, the substrate that has been ultrasonically cleaned is subjected to secondary cleaning. The purpose of this step is to wash away the oxide layer on the surface of the substrate or impurities such as dust contaminated during the transfer of the substrate. The cleaning conditions are as follows:

[0061] The inert gas introduction device is connected to argon or nitrogen;

[0062] Maintain the vacuum degree in the reaction furnace at (8.0-15.0)×10 -3 Pa;

[0063] The current of the cathode electron gun is 120-160A;

[0064] The pulse negative bias voltage applied to the substrate is -400 to -500 V;

[0065] The working time is 5 to 10 minutes.

[0066] Step S3, using a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reaction furnace, an inert gas introduction device and two cathode targets to deposit a base layer on the surface of the substrate; the two cathode targets are titanium alloys with a titanium content greater than 70%; the inert gas introduction device is connected to argon or nitrogen;

[0067] The specific process parameters are as follows:

[0068] Maintaining the vacuum degree in the reaction furnace at 0.1-1 Pa;

[0069] The current of the cathode electron gun is 15 to 30A;

[0070] The pulse negative bias voltage applied to the substrate is -150 to -100 V;

[0071] The working time is 20 to 50 minutes, and the temperature does not exceed 200°C;

[0072] Step S4, using a magnetron sputtering furnace equipped with a water cooling system, a cathode electron gun, an anode, a reaction furnace, an inert gas introduction device and four cathode targets, depositing a surface layer on the surface of the primer layer; the four cathode targets are respectively two pure titanium targets, one aluminum alloy target containing 2-8% Ag and one pure aluminum target; the inert gas introduction device is connected to argon or nitrogen; firstly, the substrate product with the primer layer deposited is placed on a water cooling sample table, and the water cooling system is started; and then the surface layer deposition treatment is performed under the following process parameter conditions:

[0073] Maintaining the vacuum degree in the reaction furnace at 0.05-0.5 Pa;

[0074] The cathode electron gun current I 纯钛 5~7A, I 铝合金 6~8A, I 纯铝 6~8A;

[0075] The pulse negative bias voltage applied to the substrate is -180 to -120 V;

[0076] The working time is 3 to 6 hours and the temperature does not exceed 300°C.

[0077] Amorphous alloys are materials whose atoms or ions in the microstructure are not arranged regularly and are long-range disordered. The system is in a metastable state in energy and has complex multiple relaxation behaviors. In contrast, the atoms in a crystal are arranged periodically in space according to a certain rule, which is a long-range ordered and highly ordered structure. Most solid substances in nature are crystals. This is because crystals are stable and the system energy is more stable. To form amorphous materials, more stringent preparation conditions are required.

[0078] In order to prepare the surface layer of amorphous alloy material, the patent of the present invention sets a cooling stage and specific sputtering parameters in the magnetron sputtering furnace.

[0079] The cooling stage can keep the substrate at a low temperature, forming supercooling when the atoms or ions of the target material are sputtered on the substrate surface, which helps the atoms or ions to be arranged chaotically and unable to continue to diffuse, forming a thermodynamically metastable amorphous state and retaining it, and finally forming the desired amorphous surface layer.

[0080] The specific sputtering parameters include the current of the cathode electron gun and the pulsed negative bias voltage applied to the substrate. The current of 5 to 8A and the high bias voltage of -180 to -120V can provide sufficient energy for the high-energy particles in the sputtering process, so that the atoms or ions of the target material can be reorganized on the substrate and rearranged irregularly, thereby promoting the generation of amorphous materials. However, the current and bias voltage should not be too high. If they are too high, the rearranged atoms or ions will continue to diffuse faster due to the excess energy, and eventually return to a stable crystalline state.

[0081] The presence of the cooling stage and the low temperature requirement result in the temperature in the magnetron sputtering furnace not exceeding 300°C. However, the lower the sputtering temperature, the worse the coating adhesion, so other methods are needed to compensate for the lack of adhesion. The embodiment of the present invention increases the coating adhesion by adding a titanium alloy transition layer with a titanium content of more than 70% as a base layer. The composition of the titanium alloy and the TiAl surface layer is similar, and the two have a stronger adhesion to prevent the TiAl surface layer from peeling off.

[0082] By adjusting and controlling the current of the multi-target cathode electron gun, the deposition rate is different, so as to obtain the coating of the final target component, so that the coating surface appears silvery and bright. In addition, during the sputtering process, local discharge may occur, resulting in excessive temperature. At this time, the titanium aluminum surface coating is easily oxidized, forming gray-black spots, affecting the appearance. The Ag element can improve the heat resistance and oxidation resistance of the aluminum alloy, prevent the generation of black spots during the sputtering process, and reduce the surface roughness of the coating.

[0083] By strictly controlling the surface bias, the particle size of the surface layer is controlled within the range of 50nm-200nm to obtain the best mechanical properties and appearance. Too large particles will cause sand holes or pits on the coating surface, thus deteriorating its mechanical properties and appearance.

[0084] The above preparation process is simple, the sputtering process has only two steps, and the coating has only two layers; the multi-target sputtering method has a simpler process flow, easier control of composition, and higher coating quality. Compared with pure metal silver-white coatings such as chrome plating and platinum plating, this type of coating has lower cost.

[0085] The preparation method of the silver-white composite coating is described below through several specific embodiments.

[0086] Example 1

[0087] In this embodiment, a silver-white, high-hardness, wear-resistant, corrosion-resistant, and bio-friendly silver-white composite coating is sputtered on a 316L steel watch case. The specific steps are as follows:

[0088] Step S1, the substrate is cleaned in an ultrasonic cleaning device for 5 minutes using a dewaxing solution, a degreasing solution and deionized water in sequence, the cleaning temperature is 60°C, wherein the ratio of the dewaxing solution is dewaxing water: pure water = 1:10, and the ratio of the degreasing solution is degreasing agent: pure water = 1:20, and the substrate is blown dry after cleaning.

[0089] Step S2, a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reaction furnace and an inert gas introduction device is used to perform secondary cleaning on the substrate that has been ultrasonically cleaned. Specifically, argon gas is introduced into the reaction furnace through the inert gas introduction device; the vacuum device is started to draw the vacuum degree in the reaction furnace to 10.0×10 -3Pa, set the cathode electron gun current to 130A, the pulse negative bias to -500V, and the cleaning time to 8 minutes.

[0090] Step S3, using a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reactor, an inert gas introduction device and two pure titanium cathode targets, depositing a base layer on the surface of the substrate. Specifically: introducing argon gas into the reactor through the inert gas introduction device; starting the vacuum pumping device to pump the vacuum degree in the reactor to 0.3 Pa, setting the cathode electron gun current to 15A, the pulse negative bias voltage to -140V, the sputtering time to 20 minutes, and the temperature to 200°C.

[0091] Step S4, using a magnetron sputtering furnace equipped with a water cooling system, a cathode electron gun, an anode, a reactor, an inert gas introduction device and four cathode targets, depositing a surface layer on the surface of the base layer, wherein the four cathode targets are respectively two pure titanium targets, one aluminum alloy target containing 3% Ag and one pure aluminum target, placing the product deposited with the base layer on a water-cooled sample table, starting the water cooling system, and introducing argon gas into the reactor through the inert gas introduction device; starting the vacuum pumping device, pumping the vacuum degree in the reactor to 0.3 Pa, and setting the current I of the cathode electron gun to 0.5V. 纯钛 5A, I 铝合金 For 6A, I 纯铝 The current was 6A, the pulse negative bias was -150V, the sputtering time was 3.5 hours, and the temperature was 300°C.

[0092] The finished product was taken out and subjected to 24-hour salt spray and 24-hour artificial sweat tests according to the standard QB / T 4775-2014 "Test Method for Artificial Sweat Corrosion Resistance of Watch Shell and Accessories". After the test, there was no corrosion on the surface. The hardness of the surface coating was tested with a nano indentation tester, and the test result was 809HVIT. Figure 3 As shown in the figure, the thickness and surface morphology of the composite coating were tested by scanning electron microscopy. The test results showed that the thickness was about 1.5μm, the coating surface particles were fine and smooth, and the quality was good. The surface coating composition was tested by energy dispersive spectrometer, and the test results showed that it contained 63.4% Ti and 0.8% Ag. The surface coating phase material was tested by X-ray diffractometer, and the test curve showed a significant smooth broad peak, indicating that it was an amorphous material.

[0093] Example 2

[0094] In this embodiment, a silvery-white, high-hardness, wear-resistant, corrosion-resistant, and bio-friendly silvery-white composite coating is sputtered on a TC4 titanium alloy watch case. The specific steps are as follows:

[0095] Step S1, the substrate is cleaned in an ultrasonic cleaning device in sequence with a wax removal solution, a degreasing agent and deionized water for 7 minutes at a cleaning temperature of 55°C, wherein the ratio of the wax removal solution is wax removal water: pure water = 1:8, and the ratio of the degreasing solution is degreasing agent: pure water = 1:25. After cleaning, the substrate is blown dry.

[0096] Step S2, a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reaction furnace and an inert gas introduction device is used to perform secondary cleaning on the substrate that has been ultrasonically cleaned. Specifically, nitrogen is introduced into the reaction furnace through the inert gas introduction device; the vacuum device is started to draw the vacuum degree in the reaction furnace to 12.0×10 -3 Pa, set the cathode electron gun current to 150A, the pulse negative bias to -400V, and the cleaning time to 10 minutes.

[0097] Step S3, using a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reactor, an inert gas introduction device and two cathode targets containing 86.4% titanium, depositing a base layer on the surface of the substrate. Specifically: nitrogen is introduced into the reactor through the inert gas introduction device; the vacuum device is started to draw the vacuum degree in the reactor to 0.7 Pa, the current of the cathode electron gun is set to 25A, the pulse negative bias voltage is -120V, the sputtering time is 40 minutes, and the temperature is 150°C.

[0098] Step S4, using a magnetron sputtering furnace equipped with a water cooling system, a cathode electron gun, an anode, a reactor, an inert gas introduction device and four cathode targets, depositing a surface layer on the surface of the primer layer, wherein the four cathode targets are respectively two pure titanium targets, one aluminum alloy target containing 5% Ag and one pure aluminum target, placing the product with the primer layer deposited on a water-cooled sample table, starting the water cooling system, and introducing nitrogen into the reactor through the inert gas introduction device; starting the vacuum pumping device, pumping the vacuum degree in the reactor to 0.1 Pa, and setting the current I of the cathode electron gun to 0.1 Pa. 纯钛 For 6A, I 铝合金 For 6A, I 纯铝 The current was 6A, the pulse negative bias was -170V, the sputtering time was 5 hours, and the temperature was 280°C.

[0099] The finished parts were taken out and subjected to 72-hour salt spray and 72-hour artificial sweat tests according to the standard QB / T 4775-2014 "Test Method for Artificial Sweat Corrosion Resistance of Watch Shell and Accessories". After the test, there was no corrosion on the surface. The nanoindentation tester was used to test the hardness of the surface coating, and the test result was 832HVIT. The scanning electron microscope was used to test the thickness and surface morphology of the composite coating. The test result showed that the thickness was about 2.3μm, the coating surface particles were fine and smooth, and the quality was good. The energy spectrometer was used to test the surface coating composition, and the test results were as follows Figure 4As shown, it contains 66.1% Ti and 1.3% Ag. The surface coating phase material is tested by X-ray diffractometer, and the test curve shows a significant smooth broad peak, indicating an amorphous material.

[0100] Example 3

[0101] In this embodiment, a silver-white composite coating with high hardness, wear resistance, corrosion resistance and bio-friendliness is sputtered on a 7075 aluminum alloy watch case. The specific steps are as follows:

[0102] Step S1, the substrate is cleaned in an ultrasonic cleaning device for 6 minutes using a wax removal solution, a degreasing agent and deionized water, respectively, at a cleaning temperature of 50°C, wherein the wax removal solution ratio is wax removal water: purified water = 1:14, and the degreasing solution ratio is degreasing agent: purified water = 1:15, and the substrate is blown dry after cleaning.

[0103] Step S2, a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reaction furnace and an inert gas introduction device is used to perform secondary cleaning on the substrate that has been ultrasonically cleaned. Specifically, nitrogen is introduced into the reaction furnace through the inert gas introduction device; the vacuum device is started to draw the vacuum degree in the reaction furnace to 8×10 -3 Pa, set the cathode electron gun current to 120A, the pulse negative bias to -460V, and the cleaning time to 6 minutes.

[0104] Step S3, using a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reactor, an inert gas introduction device and two cathode targets containing Ti79.7%, to deposit a base layer on the surface of the substrate. Specifically: nitrogen is introduced into the reactor through the inert gas introduction device; the vacuum device is started to draw the vacuum degree in the reactor to 0.1 Pa, the current of the cathode electron gun is set to 18A, the pulse negative bias voltage is -100V, the sputtering time is 35 minutes, and the temperature is 170°C.

[0105] Step S4, using a magnetron sputtering furnace equipped with a water cooling system, a cathode electron gun, an anode, a reactor, an inert gas introduction device and four cathode targets, depositing a surface layer on the surface of the primer layer, wherein the four cathode targets are respectively two pure titanium targets, one aluminum alloy target containing 8% Ag and one pure aluminum target, placing the product deposited with the primer layer on a water-cooled sample table, starting the water cooling system, and introducing nitrogen into the reactor through the inert gas introduction device; starting the vacuum pumping device, pumping the vacuum degree in the reactor to 0.05 Pa, and setting the current I of the cathode electron gun to 0.05 Pa. 纯钛 For 6A, I 铝合金 8A, I 纯铝 The current was 7A, the pulse negative bias was -120V, the sputtering time was 4 hours, and the temperature was 250°C.

[0106] The finished parts were taken out and subjected to 48-hour salt spray and 48-hour artificial sweat tests according to the standard QB / T 4775-2014 "Test Method for Artificial Sweat Corrosion Resistance of Watch Shell and Accessories". After the test, there was no corrosion on the surface. The hardness of the surface coating was tested using a nanoindentation tester, and the test result was 819HVIT. The thickness and surface morphology of the composite coating were tested using a scanning electron microscope. The test result showed that the thickness was about 1.8μm, the particles on the coating surface were fine and smooth, and the quality was good. The composition of the surface coating was tested using an energy spectrometer, and the test result showed that it contained 62.5% Ti and 2.2% Ag. The surface coating phase material was tested using an X-ray diffractometer, and the test results are as follows: Figure 5 As shown, the curve has a significant smooth broad peak, which is an amorphous material.

[0107] The performance of the silver-white composite coatings prepared in the above three examples is shown in the following table, wherein the corrosion resistance column indicates the salt spray and artificial sweat tests applied to the coatings prepared in the corresponding examples, for example, "24h+24h qualified" indicates that the silver-white composite coating prepared in the example was subjected to 24-hour salt spray and 24-hour artificial sweat tests, and the test results were all qualified. According to the standard QB / T 4775-2014 "Test Method for Artificial Sweat Corrosion Resistance of Watch Shell and Accessories", "24h+24h qualified" means that the test is passed.

[0108] Table 1 Performance of coatings prepared in various embodiments

[0109]

[0110] It is understandable that the above three embodiments use three common substrates in watch exterior parts, but the method for preparing the silver-white composite coating provided by the present invention is not limited to the above three substrates.

[0111] The present invention has the following beneficial effects: the coating of the present scheme is composed of a base layer and a surface layer, the surface layer is a Ti, Al, Ag amorphous alloy layer, and the main component of the base layer is Ti. The composition of the titanium alloy and the TiAl surface layer is similar, and the bonding force between the two is stronger to prevent the TiAl surface layer from peeling off. Ag can improve the heat resistance and oxidation resistance of the aluminum alloy, prevent the generation of black spots during the sputtering process, and reduce the surface roughness of the coating. The base layer and the surface layer are prepared by a multi-target magnetron sputtering process, and the process flow is simple, the composition is easier to control, and the coating quality is higher; the product with the base layer deposited is placed in the water cooling system of the magnetron sputtering furnace, and the supercooling caused by the water cooling system can promote the formation of the amorphous alloy surface layer; by controlling the current and pulse bias parameters of each cathode electron gun, the deposition rate of various materials is different, and an amorphous alloy surface layer with a silvery white luster and containing the expected composition is obtained; the thickness and particle size of the coating are indirectly controlled by controlling the process parameters, so that the coating has the desired appearance effect and performance. The coating prepared by the present scheme has a silvery white color, and the surface layer is an amorphous alloy, so it has good corrosion resistance, is bio-friendly, has high hardness, good wear resistance and scratch resistance, and is low in cost.

[0112] The above are only specific implementations of the present invention, which cannot be used to limit the scope of the present invention. Equivalent changes made by ordinary technicians in this technical field based on this creation, as well as changes known to technicians in this field, should still fall within the scope of the present invention.

Claims

1. A silvery white composite coating, characterized in that: The composite coating comprises a primer layer and a surface layer sequentially formed on the surface of a substrate, wherein: The composition of the surface layer is 60-70% Ti, 0.5-2.5% Ag, and the balance is Al, in terms of mass percentage; The base layer contains at least Ti, the mass percentage of which exceeds 70%; The surface layer is amorphous.

2. The silvery white composite coating according to claim 1, characterized in that: The particle size of the surface layer is 50nm to 200nm.

3. The silvery white composite coating according to claim 1, characterized in that: The thickness of the surface layer is 0.8-5 um.

4. The silvery white composite coating according to claim 1, characterized in that: The thickness of the base layer is 0.3-1.5um.

5. The silvery white composite coating according to claim 1, characterized in that: The thickness of the surface layer is 0.8-5 um, and the thickness of the base layer is 0.3-1.5 um.

6. A method for preparing a silvery-white composite coating, comprising preparing the silvery-white composite coating as claimed in any one of claims 1 to 4 on the surface of a substrate, characterized in that: The method comprises the following steps: Step S1, in an ultrasonic cleaning device, the substrate is cleaned with a wax removal solution, an oil removal solution and deionized water in sequence, and the substrate is blown dry after cleaning; Step S2, using a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reaction furnace and an inert gas introduction device to perform secondary cleaning on the substrate after ultrasonic cleaning; Step S3, using a magnetron sputtering furnace equipped with a cathode electron gun, an anode, a reaction furnace, an inert gas introduction device and two cathode targets to deposit a base layer on the surface of the substrate; the two cathode targets are titanium alloys with a titanium content greater than 70%; the inert gas introduction device is connected to argon or nitrogen; The specific process parameters are as follows: Maintaining the vacuum degree in the reaction furnace at 0.1-1 Pa; The current of the cathode electron gun is 15 to 30A; The pulse negative bias voltage applied to the substrate is -150 to -100 V; The working time is 20 to 50 minutes, and the temperature does not exceed 200°C; Step S4, using a magnetron sputtering furnace equipped with a water cooling system, a cathode electron gun, an anode, a reaction furnace, an inert gas introduction device and four cathode targets, depositing a surface layer on the surface of the primer layer; the four cathode targets are respectively two pure titanium targets, one aluminum alloy target containing 2-8% Ag and one pure aluminum target; the inert gas introduction device is connected to argon or nitrogen; firstly, the substrate product with the primer layer deposited is placed on a water cooling sample table, and the water cooling system is started; and then the surface layer deposition treatment is performed under the following process parameter conditions: Maintaining the vacuum degree in the reaction furnace at 0.05-0.5 Pa; The cathode electron gun current I 纯钛 5~7A, I 铝合金 6~8A, I 纯铝 6~8A; The pulse negative bias voltage applied to the substrate is -180 to -120 V; The working time is 3 to 6 hours and the temperature does not exceed 300°C.

7. The method for preparing the silvery-white composite coating according to claim 6, characterized in that: In the step S1, the ultrasonic cleaning time is 5 to 7 minutes, the cleaning temperature is 50 to 60°C, the ratio of the wax removal solution is wax removal water: pure water = 1:8 to 1:16, and the ratio of the oil removal solution is oil removal agent: pure water = 1:15 to 1:

30.

8. The method for preparing the silvery-white composite coating according to claim 6, characterized in that: In step S2, the cleaning conditions are as follows: The inert gas introduction device is connected to argon or nitrogen; Maintain the vacuum degree in the reaction furnace at (8.0-15.0)×10 -3 Pa; The current of the cathode electron gun is 120-160A; The pulse negative bias voltage applied to the substrate is -400 to -500 V; The working time is 5 to 10 minutes.