Method for rapidly preparing ultrathin conductive polymer film and application of ultrathin conductive polymer film

The metal layer is deposited on the liquid substrate through the direct deposition method at the gas-liquid interface, which solves the conductivity and durability problems in the preparation of ultra-thin conductive polymer films in the existing technology, and realizes a high-performance conductive polymer film suitable for in the fields of flexible sensing and biomedicine.

CN118773555APending Publication Date: 2024-10-15LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410896037.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult to prepare polymer films with ultra-thin thickness, good flexibility and excellent conductive properties using existing technology, and the weak adhesion between inert metals and stretchable substrates limits the durability and electron mobility of conductive films. .

Method used

The gas-liquid interface direct deposition method is used to deposit a metal layer on the liquid substrate through plasma sputtering to form a conductive polymer film, achieving strong interface bonding between the inert gold and the liquid substrate, and improving conductivity and flexibility.

Benefits of technology

The conductive polymer film achieves good conductivity and flexibility in the thickness range of 30-300nm, has good transparency and mechanical tolerance, and is suitable for flexible sensing and biomedical fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773555A_ABST
    Figure CN118773555A_ABST
Patent Text Reader

Abstract

The invention discloses a method for rapidly preparing an ultrathin conducting polymer film and application, and relates to the technical field of conducting polymer films, the method comprises the following steps: coating a liquid substrate on a substrate, and putting the liquid substrate into a cavity of an ion sputtering instrument; fixing the metal target material, closing the cavity, vacuumizing, starting sputtering, and controlling the thickness of a conductive layer formed by sputtering by adjusting sputtering power and deposition time; after the cavity is cooled, the sample is taken out, a target substrate is tightly attached to the upper portion of the metal film, and the target substrate and the metal film slowly slide down along the substrate and are soaked in petroleum ether to remove redundant liquid substrate; and obtaining the conductive polymer film. According to the method, the flexible ultrathin conductive polymer film is prepared through direct deposition on a gas-liquid interface, so that strong interface bonding between inert gold and a liquid substrate such as PDMS (polydimethylsiloxane) is achieved, and the method can be applied to the fields of flexible sensing and biomedicine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conductive polymer films, and in particular to a method for rapidly preparing an ultra-thin conductive polymer film and application thereof. Background Art

[0002] With the rapid development of skin and implantable electronics, higher requirements are placed on elastic conductors. Conductive polymers provide a feasible solution for high-performance elastic conductors. However, the preparation of polymer films with ultra-thin thickness, good flexibility and excellent conductive properties is still very challenging. Currently, the most commonly used method is to use polymers as the matrix and then add conductive fillers (graphene, carbon nanotubes, metal nanowires, etc.) to improve the conductivity and flexibility of the polymer. However, the conductivity of this type of conductive polymer composites is relatively low, which limits their further application in high-performance optoelectronic devices. In addition, when the thickness of the polymer is reduced to the micrometer or even nanometer scale, the particle size and morphology of the filler itself will greatly affect the conductivity of the composite film. Therefore, it is of great value to develop technologies with ultra-thin conductive films.

[0003] At present, most of the preparation processes for flexible conductive films are to combine the conductor material with the substrate to prepare a single-layer conductive film through preparation processes such as magnetron sputtering, spin coating, sol-gel method or hot pressing. The simple combination of the conductive material and the substrate makes the formed conductive network easily destroyed under use environments such as bending and friction, resulting in irreversible loss of conductive properties. Comprehensive consideration of conductivity and durability and selection of suitable conductive materials are the primary conditions for preparing the required conductive film.

[0004] In practical applications, a large number of artificial skins adopt chemically inert metals (such as gold and platinum) as functional layers and interconnects to sense or transmit the latest signals because of their high intrinsic conductivity, good chemical stability and bio-nontoxicity. For these inert metal-based artificial skins, one of the most challenging issues is the weak adhesion between the inert metal and the stretchable substrate due to poor interfacial chemical bonding. Although an encapsulation strategy of encapsulating the functional metal layer into a durable polymer has been developed to defend against friction interference, it hinders the metal layer from directly contacting the skin and other media for signal acquisition. Another promising strategy is to directly enhance the interfacial adhesion between the metal layer and the elastic substrate through interfacial structural engineering and chemical engineering. The former compensates the deformation stress applied to the metal layer by increasing the interfacial microstructure configuration, but the weak van der Waals force at the metal-substrate interface leads to limited interfacial bonding ability. The latter usually chemically modifies the metal layer and the elastic substrate with specific chemical groups or adhesion additives to directly enhance their interfacial bonding. However, the chemically modified residues inevitably penetrate into the inert metal and substrate layers, thereby destroying the structural integrity and limiting the electron mobility of the device, resulting in poor mechanical tolerance and low electrical conductivity. Summary of the invention

[0005] The present invention provides a method for rapidly preparing an ultrathin conductive polymer film and its application. The method directly deposits a flexible ultrathin conductive polymer film at a gas-liquid interface to achieve a strong interface bond between inert gold and a liquid substrate, such as PDMS (polydimethylsiloxane), which can be applied to flexible sensing and biomedical fields.

[0006] To achieve the above object, the technical solution of the present invention is:

[0007] A method for rapidly preparing an ultrathin conductive polymer film comprises the following steps:

[0008] (1) firstly, the liquid substrate is coated on the flat surface of the substrate so that it is evenly covered on the substrate, and then the substrate with the liquid substrate is placed in the chamber of the ion sputtering device;

[0009] (2) Fix the metal target, close the chamber, evacuate the chamber, start sputtering, and control the thickness of the conductive layer formed by sputtering by adjusting the sputtering power and deposition time. Cool for three minutes after sputtering is completed;

[0010] (3) After the cavity is cooled, the sample is taken out, the target substrate is placed closely on the metal film, the target substrate and the metal film are slowly slid down along the substrate, and soaked in petroleum ether to remove excess liquid substrate; thus obtaining a conductive polymer film.

[0011] Preferably, in the step (1), the method of coating the liquid substrate on the flat substrate surface is drop coating, spin coating or casting, and the substrate is glass.

[0012] Preferably, in step (1), the liquid substrate is a mixture of one or more of polydimethylsiloxane, ionic liquid, glycerol, polyethylene glycol, polyalphaolefin, or perfluoropolyether.

[0013] Preferably, in step (2), the sputtering power is 5W-20W, and the deposition time is 5-25s.

[0014] Preferably, in step (2), the metal target material is at least one of Au, Ag, Cu, Cr, Mo, W, Pt, Bi and alloy materials.

[0015] Preferably, in step (3), the target substrate is a silicon wafer or SiO2 or PET or PDMS or a sapphire sheet or a glass sheet.

[0016] The invention discloses an application of a method for rapidly preparing an ultrathin conductive polymer film, which is applied to the preparation of ultrathin conductive polymer films in the fields of flexible sensing and biomedicine.

[0017] The method for rapidly preparing an ultra-thin conductive polymer film of the present invention and the beneficial effects of its application are as follows:

[0018] 1. The present invention adopts a plasma sputtering device and utilizes high-energy plasma to solidify the liquid surface. The metal is deposited on the polymer surface to form a conductive layer. The conductive polymer film is directly deposited on the surface of the liquid substrate. The obtained polymer film has a thickness in the range of 30-300nm and has good conductivity and flexibility.

[0019] 2. The polymer film prepared by the present invention is thin, the metal electrode has good conductivity, and has good transparency and flexibility;

[0020] 3. The present invention can prepare large-sized ultra-thin polymer films in a short time (i.e. within 5-25 seconds);

[0021] 4. The conductive polymer film prepared by the present invention can be used in flexible sensing and biomedical fields.

[0022] Instruction Manual

[0023] Figure 1 This is a light microscopy image of the conductive polymer film provided in Example 9;

[0024] Figure 2 This is an optical microscopy image of the conductive polymer after transfer provided in Example 9;

[0025] Figure 3An atomic force microscope image of the conductive polymer provided in Example 9;

[0026] Figure 4 Resistance test of the conductive polymer film provided in Example 9;

[0027] Figure 5 Resistance test of the conductive polymer film provided in Example 10;

[0028] Figure 6 This is a light microscopy image of the conductive polymer film provided in Example 11;

[0029] Figure 7 This is a light microscope image of the conductive polymer film provided in Example 12 after transfer.

[0030] Remark: Figure 1 , 2 200 μm and 4 μm in , 3, 6, and 7 represent the image scales. DETAILED DESCRIPTION

[0031] The following description is only a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

[0032] The following embodiments may be understood as individually expressing a part of a local structure or method of the present invention, or may be understood as a combination of the embodiments to explain the connotation of a larger structure or method of the present invention.

[0033] Example 1

[0034] A method for rapidly preparing an ultrathin conductive polymer film comprises the following steps:

[0035] (1) firstly, the liquid substrate is coated on the flat surface of the substrate so that it is evenly covered on the substrate, and then the substrate with the liquid substrate is placed in the chamber of the ion sputtering device;

[0036] (2) Fix the metal target, close the chamber, evacuate the chamber, start sputtering, and control the thickness of the conductive layer formed by sputtering by adjusting the sputtering power and deposition time. Cool for three minutes after sputtering is completed;

[0037] (3) After the cavity is cooled, the sample is taken out, the target substrate is placed closely on the metal film, the target substrate and the metal film are slowly slid down along the substrate, and soaked in petroleum ether to remove excess liquid substrate; thus obtaining a conductive polymer film.

[0038] Example 2

[0039] In the step (1), the method of coating the liquid substrate on the flat surface of the substrate is drop coating, spin coating or casting, and the substrate is glass.

[0040] Example 3

[0041] In the step (1), the liquid substrate is a mixture of one or more of polydimethylsiloxane, ionic liquid, glycerol, polyethylene glycol, polyalphaolefin, or perfluoropolyether.

[0042] Example 4

[0043] Preferably, in step (2), the sputtering power is 5W and the deposition time is 5s.

[0044] Example 5

[0045] Preferably, in step (2), the sputtering power is 20 W and the deposition time is 25 s.

[0046] Example 6

[0047] In the step (2), the metal target material is at least one of Au, Ag, Cu, Cr, Mo, W, Pt, Bi and alloy materials.

[0048] Example 7

[0049] In the step (3), the target substrate is a silicon wafer, SiO2, PET, PDMS, sapphire sheet or glass sheet.

[0050] Example 8

[0051] The invention discloses an application of a method for rapidly preparing an ultrathin conductive polymer film, which is applied to the preparation of ultrathin conductive polymer films in the fields of flexible sensing and biomedicine.

[0052] For example, the prepared film is transferred to the top of the PDMS substrate, the wires are connected through electrodes on both sides of the metal film, and a layer of PDMS is spin-coated on the top for protection to prepare a flexible sensor device. The device can be attached to any part, and the movement of different parts can be recorded by the resistance change of the device. For example, if it is attached to a finger, the movement change of the finger bending can be recorded in the source meter through the resistance change.

[0053] Example 9

[0054] Use a dropper to drop polydimethylsiloxane on the glass substrate, place it in the plasma sputtering chamber, fix the Au target, close the chamber, evacuate, and start sputtering. Keep the target 4 cm away from the sample during the whole process. The power of the sputtering process is 15W and the deposition time is 20s. After the sputtering is completed and the chamber is cooled, take out the sample. The optical microscope image of the prepared conductive polymer film is as follows: Figure 1Place the silicon wafer tightly on top of the metal film, wait for it to slide down slowly, soak it in petroleum ether for 5-10 minutes, take it out and perform ultrasonic cleaning for 5-10 minutes. Figure 2 This is the optical microscopy image of the polymer film after transfer.

[0055] The samples transferred onto the silicon wafer were tested using an atomic force microscope. Under the conditions of a power of 15 W and a deposition time of 20 s, the thickness of the Au film was measured to be 13 nm, and the thickness of the polymer film was 50 nm. Figure 3 The two sides of the prepared Au film are connected to the electrodes through wires, and the resistance of the conductive polymer film is measured by Keithley 2400 source meter. Figure 4 Shown

[0056] Example 10

[0057] Use a dropper to drop polydimethylsiloxane on the glass substrate, place it in the plasma sputtering chamber, fix the Ag target, close the chamber, evacuate, and start sputtering. Keep the target 4 cm away from the sample during the whole process. The power of the sputtering process is 15W and the deposition time is 20s. After the sputtering is completed and the chamber is cooled, take out the sample, and the resistance test of the prepared conductive polymer film is as follows: Figure 5 As shown. Place the silicon wafer tightly on top of the Ag film and wait for it to slide down slowly. Soak it in petroleum ether for 5-10 minutes, then take it out and perform ultrasonic cleaning for 5-10 minutes.

[0058] Embodiment 11

[0059] Use a dropper to drop polydimethylsiloxane on the glass substrate, place it in the plasma sputtering chamber, fix the Au target, close the chamber, evacuate, and start sputtering. Keep the target 4cm away from the sample during the whole process. The power of the sputtering process is 15w, and the deposition time is changed to 15s. After sputtering, take out the sample after the chamber cools down. Put the silicon wafer tightly on the top of the metal film, wait for it to slide down slowly, soak it in petroleum ether for 5-10min, and then take it out and perform ultrasonic cleaning for 5-10min.

[0060] The two sides of the prepared Au film are connected to electrodes through wires, and the resistance of the conductive polymer film is measured using a Keithley 2400 source meter. The optical microscope image of the conductive polymer in this embodiment is shown in FIG. Figure 6 As shown, other tests are the same as in Example 9.

[0061] Example 12

[0062] Use a dropper to take polydimethylsiloxane on the glass substrate and place it in the cavity. After fixing the Bi target, close the cavity, evacuate, and start sputtering. Keep the target 4 cm away from the sample during the whole process. The power of the sputtering process is 15W and the deposition time is 20s. After sputtering, take out the sample after the cavity cools down, stick the silicon wafer tightly on the top of the metal film, wait for it to slide down slowly, soak it in petroleum ether for 5-10 minutes, and then take it out and perform ultrasonic cleaning for 5-10 minutes. The optical microscope image of the prepared conductive polymer film is shown in the figure. Figure 7 Other tests were the same as in Example 9.

Claims

1. A method for rapidly preparing an ultrathin conductive polymer film, characterized in that: The steps include: (1) firstly, the liquid substrate is coated on the flat surface of the substrate so that it is evenly covered on the substrate, and then the substrate with the liquid substrate is placed in the chamber of the ion sputtering device; (2) Fix the metal target, close the chamber, evacuate the chamber, start sputtering, and control the thickness of the conductive layer formed by sputtering by adjusting the sputtering power and deposition time. Cool for three minutes after sputtering is completed; (3) After the cavity is cooled, the sample is taken out, the target substrate is placed closely on the metal film, the target substrate and the metal film are slowly slid down along the substrate, and soaked in petroleum ether to remove excess liquid substrate; and a conductive polymer film is obtained.

2. A method for rapidly preparing an ultrathin conductive polymer film as claimed in claim 1, characterized in that: In the step (1), the method of coating the liquid substrate on the flat surface of the substrate is drop coating, spin coating or casting, and the substrate is glass.

3. A method for rapidly preparing an ultrathin conductive polymer film as claimed in claim 1, characterized in that: In the step (1), the liquid substrate is a mixture of one or more of polydimethylsiloxane, ionic liquid, glycerol, polyethylene glycol, polyalphaolefin, or perfluoropolyether.

4. A method for rapidly preparing an ultrathin conductive polymer film as claimed in claim 1, characterized in that: In the step (2), the sputtering power is 5W-20W, and the deposition time is 5-25s.

5. A method for rapidly preparing an ultrathin conductive polymer film as claimed in claim 1, characterized in that: In the step (2), the metal target material is at least one of Au, Ag, Cu, Cr, Mo, W, Pt, Bi and alloy materials.

6. A method for rapidly preparing an ultrathin conductive polymer film as claimed in claim 1, characterized in that: In the step (3), the target substrate is a silicon wafer, SiO2, PET, PDMS, sapphire sheet or glass sheet.

7. Application of the method for rapidly preparing an ultrathin conductive polymer film as claimed in claim 1 to the preparation of ultrathin conductive polymer films in the fields of flexible sensing and biomedicine.