A conductive diamond electrode and a method for preparing the same

Diamond electrodes are prepared by chemical vapor deposition method, using the first diamond layer as the support material and the electrolyte barrier layer, and the second diamond layer is a porous structure, solving the problems of complex electrode preparation and poor stability in the prior art, achieving higher Cyclic stability and effective active specific surface area.

CN118773573BActive Publication Date: 2024-11-29WUXI YUBAIFAN NEW MATERIAL TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411274202.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-29
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The existing diamond electrodes have complex processes and high costs during the preparation process. The difference in the diamond film layer and the polycrystalline nickel film layer affect the cyclic stability of the electrode, which can easily lead to electrochemical corrosion and shorten life.

Method used

The conductive diamond electrode is prepared by chemical vapor deposition method. By depositing the first diamond layer and the second diamond layer on the substrate, the first diamond layer serves as a supporting material and an electrolyte barrier layer, the second diamond layer is a porous structure, and the diamond grain size is More than 2μm, the surface has pits, ensuring good adhesion and chemical inertia, and improving circulation stability.

Benefits of technology

The cyclic stability and effective active specific surface area of ​​the electrode are improved, the life of the electrode is extended, and the conductivity and active point of the electrode are enhanced by controlling the SP2 bond content and diamond grain size, ensuring the high performance of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773573B_ABST
    Figure CN118773573B_ABST
Patent Text Reader

Abstract

The present invention discloses a conductive diamond electrode and a preparation method thereof. The electrode comprises a substrate, a first diamond layer and a second diamond layer. The first diamond layer is arranged on the substrate, and the second diamond layer is arranged on the first diamond layer. The grain size of the diamond in the first diamond layer that contacts the second diamond layer is greater than 2 μm. The surface of the diamond grains on the upper surface of the first diamond layer has pits. The second diamond layer is a porous structure. The electrode is made in an integrated manner by a chemical vapor deposition method, and has the characteristics of better cycle stability and high effective active specific surface area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a conductive diamond electrode and a preparation method thereof, belonging to the technical field of vapor deposition. Background Art

[0002] Impurity atoms are doped during the growth of diamond, and impurity energy levels are introduced to form p-type or n-type semiconductors. Heavily doped diamonds even show metal-like conductivity and can be used as solid electrodes. Compared with solid electrodes such as precious metal electrodes, graphitized amorphous carbon electrodes, and composite oxide electrodes, diamond electrodes have very wide potential windows, low background currents, relatively fast electron transfer rates, excellent chemical inertness, good biocompatibility, rich surface chemical compositions, and are not easily contaminated. They have become excellent electrode materials for electrolysis, electrochemical synthesis, electrocatalysis, and energy storage and conversion, and have great application prospects.

[0003] Taking electrochemical double-layer capacitors as an example, increasing the effective active surface area of ​​electrode materials can effectively improve the energy density of capacitors, so constructing porous diamond electrodes with appropriate pore sizes and suitable pore distributions that match the ion size in the electrolyte is particularly important for forming high-performance diamond capacitors. Due to the high mechanical strength of diamond, different diamond nanostructures can be grown, or diamond hybrid materials can be synthesized with other materials to expand the effective active surface area of ​​conductive diamond.

[0004] In the prior art, diamond nanostructures can be obtained by mask etching. For example, Patent Document 1 (Publication No.: CN110407299A) discloses a porous boron-nitrogen-nickel co-doped diamond electrode, comprising a substrate, a boron-nitrogen-nickel co-doped diamond film layer and a polycrystalline nickel film layer sequentially arranged on one side or both sides of the substrate, wherein the surface layer of the diamond film layer is provided with a plurality of nanopores, and the polycrystalline nickel film layer covers the surface of the diamond film layer where the nanopores are not provided.

[0005] Although the diamond electrode of Patent Document 1 has the characteristic of large specific surface area due to its porous structure, it is prepared by using a polycrystalline nickel film layer with multiple nano-through holes on the surface as a mask to etch the diamond film layer under the multiple nano-through holes to form multiple nano-holes on the surface of the diamond film layer. The process is complicated and costly, and the diamond film layer and the polycrystalline nickel film layer are made of different materials, which affects the cycle stability of the electrode.

[0006] The prior art can also use porous heterogeneous materials as templates for diamond growth, such as: Patent document 2 (publication number: CN110407299A) discloses a method for preparing a boron-doped diamond thin film electrode based on porous titanium, comprising the following steps: Step 1: Soak porous titanium with a porosity of 20-50% in a hot sodium hydroxide aqueous solution to fully remove oil, then ultrasonically clean the deoiled porous titanium with water and place it in a 10% hydrochloric acid solution and heat it to a slightly boiling state until the solution gradually turns light purple, ultrasonically clean it with deionized water and place it in deionized water for protection and standby; Step 2: Use the porous titanium treated in the above step as a substrate, tantalum wire as a hot wire, methane and hydrogen as gas sources, trimethyl borate as a boron source, and use a hot wire chemical vapor deposition method to grow a boron-doped diamond film in a methane and hydrogen atmosphere.

[0007] Although the electrode of Patent Document 2 has the characteristic of large specific surface area, the diamond film is in direct contact with the substrate, which easily causes electrochemical corrosion and affects the cycle stability and life of the electrode.

[0008] Therefore, it is hoped that a technical solution can be provided to solve or at least alleviate the above-mentioned deficiencies of the prior art. Summary of the invention

[0009] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a conductive diamond electrode having better cycle stability and high effective active specific surface area.

[0010] To achieve the above object, the present invention adopts the following technical solutions:

[0011] A conductive diamond electrode comprises a substrate, a first diamond layer and a second diamond layer, wherein the first diamond layer is arranged on the substrate and the second diamond layer is arranged on the first diamond layer; the grain size of diamonds in the first diamond layer in contact with the second diamond layer is greater than 2 μm; the surface of diamond grains on the upper surface of the first diamond layer has pits; and the second diamond layer is a porous structure.

[0012] The first diamond layer serves as the supporting material of the second diamond layer and the electrolyte barrier layer of the electrode. The first diamond layer and the second diamond layer are homogeneous materials, and the diamond grains in the second diamond layer grow coherently on the surface of the first diamond layer, so that the second diamond layer has good adhesion on the first diamond layer, and diamond has excellent chemical inertness, which avoids the second diamond layer from falling off or structural damage due to low adhesion or electrochemical corrosion of the supporting material, ensuring the cycle stability of the electrode, thereby improving the life of the electrode.

[0013] The surface of the diamond grains on the upper surface of the first diamond layer has pits, which increases the support area of ​​the second diamond layer, which is beneficial to increasing the effective active specific surface area of ​​the electrode. At the same time, the grain size of the diamond in the first diamond layer that contacts the second diamond layer is controlled to be above 2 μm, thereby ensuring that the second diamond layer can grow along the surface of the first diamond layer.

[0014] The second diamond layer has a porous structure, which is beneficial to increasing the effective active specific surface area of ​​the electrode.

[0015] Furthermore, the thickness of the first diamond is 5-20 μm, which can more effectively ensure the bonding force between the first diamond layer and the substrate and better support the second diamond layer, thereby preventing electrolyte leakage and corrosion and improving the cycle stability of the electrode.

[0016] Further, the electrode does not include a substrate, and the thickness of the first diamond layer is preferably 50-300 μm.

[0017] Furthermore, the thickness of the second diamond layer is 5-20 μm, and the diamond grain size is 10-30 nm, which is conducive to obtaining a higher effective active specific surface area.

[0018] Furthermore, the second diamond layer contains B; the content of SP2 bonds in the second diamond layer is 1%-5%.

[0019] The second diamond layer contains B, which can make the electrode have more excellent conductivity.

[0020] The SP2 bond content in the second diamond layer is controlled at 1%-5%, which is beneficial to ensure the cycle stability of the electrode while increasing the active sites of the electrode.

[0021] The present invention also provides a method for preparing a conductive diamond electrode, comprising the following steps:

[0022] S1. Prefabricated seed crystal on substrate surface

[0023] Prefabricating diamond seed crystals on the surface of the substrate;

[0024] S2. First diamond layer deposition

[0025] The first diamond layer is deposited on the substrate surface of the S1 prefabricated diamond seed crystal, and the deposition atmosphere contains hydrogen, argon and methane, wherein the hydrogen flow rate is 6-10SLM, the argon flow rate is 2.5-6SLM, and the methane flow rate is CH4 / H2=1-2%; the deposition temperature is 780-950°C, the deposition pressure is 2.5-4.5kPa, and the deposition time is 0.5-60h;

[0026] S3, pits are formed on the surface of diamond grains in the first diamond layer

[0027] Plasma etching is performed on the surface of the first diamond layer to form pits, the hydrogen flow rate in the atmosphere is 6-10 SLM, the argon flow rate is 2.5-6 SLM; the etching temperature is 750-1050° C., the etching pressure is 2.5-5 kPa, and the etching time is 5-30 min;

[0028] S4, second diamond layer deposition

[0029] S4.1 The deposition atmosphere contains hydrogen, argon and methane, wherein the hydrogen flow rate is 7-9SLM, the argon flow rate is 2.5-5SLM, and the methane flow rate is CH4 / H2=4-10%; the deposition temperature is 700-820℃, the deposition pressure is 2.5-4.5kPa, and the deposition time is 5-15min;

[0030] S4.2 The introduction of methane is stopped to form a H2 / Ar etching atmosphere and hydrogen plasma etching is performed. The etching time is 1 / 4-1 / 3 of the deposition time.

[0031] After completing step S4.2, return to step S4.1 to continue diamond deposition, and repeat steps S4.1 and S4.2 to finally obtain a second diamond layer of desired thickness.

[0032] Furthermore, in step S4.1, the deposition atmosphere contains B, and the boron-carbon ratio B / C is 3000-12000 ppm.

[0033] Furthermore, after step S4, the method further includes step S5 of removing the substrate. The first diamond layer of the electrode is deposited on the surface of the substrate material, including the substrate material, and the substrate material may also be removed after step S4.

[0034] The electrode of the present invention is prepared by integrated chemical vapor deposition. In the chemical vapor deposition chamber, only the atmosphere and process parameters are changed to complete the deposition of the first diamond layer and the second diamond layer. The entire preparation process is simple and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of the conductive diamond electrode structure of the present invention.

[0036] Figure 2 Schematic diagram of diamond grains in the first diamond layer of the electrode of the present invention that are in contact with the second diamond layer.

[0037] Figure 3 This is a SEM image of the surface of diamond grains on the upper surface of the first diamond layer of the electrode of the present invention.

[0038] Figure 4 This is a FE-SEM image of the surface of the second diamond layer of the electrode of the present invention.

[0039] Reference numerals: 1-first diamond layer, 2-second diamond layer, 3-substrate, 4-diamond grains in the first diamond layer in contact with the second diamond layer, 5-pits on the surface of diamond grains DETAILED DESCRIPTION

[0040] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The invention will be further described below with reference to examples to further illustrate the method of the present invention and its advantages.

[0042] Example 1

[0043] A conductive diamond electrode comprises a substrate, a first diamond layer and a second diamond layer, wherein the first diamond layer is arranged on the substrate and the second diamond layer is arranged on the first diamond layer; the thickness of the first diamond is 30 μm, and the grain size of the diamond in contact with the second diamond layer in the first diamond layer is greater than 2 μm; the surface of the diamond grains on the upper surface of the first diamond layer has pits; the second diamond layer is a porous structure, the thickness of the second diamond layer is 25 μm, and the diamond grain size is 50 nm; the SP2 bond content in the second diamond layer is 5%;

[0044] According to the test, after 10,000 cycles of 1.0M Na2SO4 solution, the electrode capacitance maintained 95.7% of the initial capacitance, and the effective active specific surface area of ​​the electrode was: 278.5.

[0045] Example 2

[0046] A conductive diamond electrode comprises a substrate, a first diamond layer and a second diamond layer, wherein the first diamond layer is arranged on the substrate and the second diamond layer is arranged on the first diamond layer; the thickness of the first diamond is 18 μm, the grain size of the diamond in the first diamond layer in contact with the second diamond layer is 3-9 μm, and the surface of the diamond grains on the upper surface of the first diamond layer has pits; the second diamond layer is a porous structure, the thickness of the second diamond layer is 5 μm, and the diamond grain size is 15 nm; the SP2 bond content in the second diamond layer is 4%;

[0047] According to the test, after 10,000 cycles of 1.0M Na2SO4 solution, the electrode capacitance maintained 96.4% of the initial capacitance, and the effective active specific surface area of ​​the electrode was: 302.4.

[0048] Example 3

[0049] A conductive diamond electrode comprises a substrate, a first diamond layer and a second diamond layer, wherein the first diamond layer is arranged on the substrate and the second diamond layer is arranged on the first diamond layer; the thickness of the first diamond is 15 μm, the grain size of the diamond in the first diamond layer in contact with the second diamond layer is 3-7 μm, and the surface of the diamond grains on the upper surface of the first diamond layer has pits; the second diamond layer is a porous structure, the thickness of the second diamond layer is 15 μm, the diamond grain size is 25 nm, and the SP2 bond content in the second diamond layer is 2%; the second diamond layer contains B.

[0050] According to the test, after 10,000 cycles of 1.0M Na2SO4 solution, the electrode capacitance maintained 97.8% of the initial capacitance, and the effective active specific surface area of ​​the electrode was: 351.2.

[0051] Example 4

[0052] A conductive diamond electrode comprises a first diamond layer and a second diamond layer, wherein the second diamond layer is arranged on the first diamond layer; the thickness of the first diamond is 100 μm, the grain size of the diamond in the first diamond layer in contact with the second diamond layer is 20-38 μm, and the surface of the diamond grains on the upper surface of the first diamond layer has pits; the second diamond layer is a porous structure, the thickness of the second diamond layer is 18 μm, the diamond grain size is 27 nm, and the SP2 bond content in the second diamond layer is 2%; the second diamond layer contains B.

[0053] According to the test, after 10,000 cycles of 1.0M Na2SO4 solution, the electrode capacitance maintained 98.2% of the initial capacitance, and the effective active specific surface area of ​​the electrode was: 358.3.

[0054] Example 5

[0055] S1. Prefabricated seed crystal on substrate surface

[0056] Prefabricating diamond seed crystals on the surface of the substrate;

[0057] S2. First diamond layer deposition

[0058] The first diamond layer was deposited on the substrate surface of the S1 prefabricated diamond seed crystal. The deposition atmosphere contained hydrogen, argon and methane. The hydrogen flow rate was 8 SLM, the argon flow rate was 2.8 SLM, and the methane flow rate was CH4 / H2=1.25%. The deposition temperature was 870°C, the deposition pressure was 3.5 kPa, and the deposition time was 45 min.

[0059] S3, pits are formed on the surface of diamond grains in the first diamond layer

[0060] Plasma etching is performed on the surface of the first diamond layer to form pits. The hydrogen flow rate in the atmosphere is 7 SLM, and the argon flow rate is 3 SLM. The etching temperature is 900°C, the etching pressure is 3.2 kPa, and the etching time is 6 min.

[0061] The thickness of the first diamond is 6 μm, the grain size of the diamond in the first diamond layer that contacts the second diamond layer is 2-4 μm, and the surface of the diamond grains on the upper surface of the first diamond layer has pits;

[0062] S4, second diamond layer deposition

[0063] S4.1 The deposition atmosphere contains hydrogen, argon, methane, and trimethyl borate, wherein the hydrogen flow rate is 8 SLM, the argon flow rate is 3 SLM, the methane flow rate is CH4 / H2=6%, and the boron-carbon ratio B / C=8000 ppm; the deposition temperature is 760°C, the deposition pressure is 3 kPa, and the deposition time is 10 min;

[0064] S4.2 The introduction of methane is stopped to form a H2 / Ar etching atmosphere and hydrogen plasma etching is performed for 3 minutes;

[0065] After completing step S4.2, return to step S4.1 to continue diamond deposition, and repeat steps S4.1 and S4.2 to finally obtain a second diamond layer with a thickness of 12 μm, a diamond grain size of 22 nm, and an SP2 bond content of 3% in the second diamond layer;

[0066] According to the test, after 10,000 cycles of 1.0M Na2SO4 solution, the electrode capacitance maintained 97.3% of the initial capacitance, and the effective active specific surface area of ​​the electrode was: 331.7.

[0067] Comparative Example 1

[0068] A conductive diamond electrode is provided with a diamond layer on a substrate, the diamond layer has a thickness of 15 μm and a diamond grain size of 20 nm.

[0069] According to the test, the electrode capacitance maintained 84% of the initial capacitance after 10,000 cycles of 1.0M Na2SO4 solution, and the effective active specific surface area of ​​the electrode was 213.6.

[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A conductive diamond electrode, It is characterized in that The electrode comprises a substrate, a first diamond layer and a second diamond layer, wherein the first diamond layer is arranged on the substrate and the second diamond layer is arranged on the first diamond layer; the grain size of diamonds in the first diamond layer in contact with the second diamond layer is greater than 2 μm; the surface of the diamond grains on the upper surface of the first diamond layer has pits; and the second diamond layer is a porous structure.

2. A conductive diamond electrode, It is characterized in that The electrode comprises a first diamond layer and a second diamond layer, wherein the second diamond layer is arranged on the first diamond layer; the grain size of diamond in the first diamond layer in contact with the second diamond layer is greater than 2 μm; the surface of the diamond grains on the upper surface of the first diamond layer has pits; and the second diamond layer is a porous structure.

3. The electrode according to claim 1, It is characterized in that The thickness of the first diamond layer is 5-20 μm.

4. The electrode according to claim 2, It is characterized in that The thickness of the first diamond layer is 50-300 μm.

5. The electrode according to claim 1 or 2, It is characterized in that The thickness of the second diamond layer is 5-20 μm, and the size of the diamond grains is 10-30 nm.

6. The electrode according to claim 1 or 2, It is characterized in that The second diamond layer contains B; the content of SP2 bonds in the second diamond layer is 1%-5%.

7. A method for preparing a conductive diamond electrode as claimed in claim 1, It is characterized in that The preparation method comprises the following steps: S1. Prefabricated seed crystal on substrate surface Prefabricating diamond seed crystals on the surface of the substrate; S2. First diamond layer deposition The first diamond layer is deposited on the surface of the substrate of the S1 prefabricated diamond seed crystal. The deposition atmosphere contains hydrogen, argon, and methane. The hydrogen flow rate is 6-10 SLM, the argon flow rate is 2.5-6 SLM, and the methane flow rate is CH 4 / H 2 =1-2%; deposition temperature is 780-950°C, deposition pressure is 2.5-4.5kPa, and deposition time is 0.5-60h; S3: Pits are formed on the surface of diamond grains in the first diamond layer Plasma etching is performed on the surface of the first diamond layer to form pits, the hydrogen flow rate in the atmosphere is 6-10 SLM, the argon flow rate is 2.5-6 SLM; the etching temperature is 750-1050° C., the etching pressure is 2.5-5 kPa, and the etching time is 5-30 min; S4, second diamond layer deposition S4.1 The deposition atmosphere contains hydrogen, argon, and methane, where the hydrogen flow rate is 7-9 SLM, the argon flow rate is 2.5-5 SLM, and the methane flow rate is CH 4 / H 2 =4-10%; deposition temperature is 700-820℃, deposition pressure is 2.5-4.5KPa, deposition time is 5-15min; S4.2 Stop the introduction of methane to form H 2 / Ar etching atmosphere, hydrogen plasma etching, the etching time is 1 / 4-1 / 3 of the deposition time; After completing step S4.2, return to step S4.1 to continue diamond deposition, and repeat steps S4.1 and S4.2 to finally obtain a second diamond layer of desired thickness.

8. A method for preparing a conductive diamond electrode as claimed in claim 2, It is characterized in that The preparation method comprises the following steps: S1. Prefabricated seed crystal on substrate surface Prefabricating diamond seed crystals on the surface of the substrate; S2. First diamond layer deposition The first diamond layer is deposited on the surface of the substrate of the S1 prefabricated diamond seed crystal. The deposition atmosphere contains hydrogen, argon, and methane. The hydrogen flow rate is 6-10 SLM, the argon flow rate is 2.5-6 SLM, and the methane flow rate is CH 4 / H 2 =1-2%; deposition temperature is 780-950°C, deposition pressure is 2.5-4.5kPa, and deposition time is 0.5-60h; S3, pits are formed on the surface of diamond grains in the first diamond layer Plasma etching is performed on the surface of the first diamond layer to form pits, the hydrogen flow rate in the atmosphere is 6-10 SLM, the argon flow rate is 2.5-6 SLM; the etching temperature is 750-1050° C., the etching pressure is 2.5-5 kPa, and the etching time is 5-30 min; S4, second diamond layer deposition S4.1 The deposition atmosphere contains hydrogen, argon, and methane, where the hydrogen flow rate is 7-9 SLM, the argon flow rate is 2.5-5 SLM, and the methane flow rate is CH 4 / H 2 =4-10%; deposition temperature is 700-820℃, deposition pressure is 2.5-4.5KPa, deposition time is 5-15min; S4.2 Stop the introduction of methane to form H 2 / Ar etching atmosphere, hydrogen plasma etching, the etching time is 1 / 4-1 / 3 of the deposition time; After completing step S4.2, return to step S4.1 to continue diamond deposition, and repeat steps S4.1 and S4.2 to finally obtain a second diamond layer of desired thickness; The method further includes step S5 after step S4, removing the substrate.

9. The method for preparing the electrode according to claim 7 or 8, It is characterized in that In the step S4.1, the deposition atmosphere contains B, and the boron-carbon ratio B / C is 3000-12000 ppm.

Citation Information

Patent Citations

  • Porous boron-nitrogen-nickel co-doped diamond electrode and preparation method and application thereof

    CN110407299A

  • Method for preparing nanocrystalline diamond film field-effect transistor

    CN101303979A

  • Method for preparing diamond substrate for high-heat-conductivity integrated circuit

    CN102157353A