Film coating method

By setting a dirt covering film on the surface of the coating container that is the same as the silicon wafer to be coated, the dirty area is isolated, which solves the problem of high temperature baking that cannot remove dirt, avoids silicon wafer contamination, improves production line yield and reduces manufacturing costs.

CN118773575APending Publication Date: 2024-10-15DAS SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310320727.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing technology, high-temperature baking cannot remove dirt that cannot be decomposed at high temperatures on the surface of the coating container, resulting in contamination of the position where the silicon wafer contacts the coating container, resulting in poor electroluminescence, affecting production line yield and increasing manufacturing costs.

Method used

A dirt covering film is set on the surface of the coating container. The dirt covering film material is the same as the silicon wafer to be coated. It covers the dirty area, isolates the silicon wafer from dirt, avoids contamination, and forms an aluminum oxide film in the atomic layer deposition machine.

Benefits of technology

It effectively avoids contamination at the position where the silicon wafer contacts the coating container, reduces electroluminescence defects, improves production line yield, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773575A_ABST
    Figure CN118773575A_ABST
Patent Text Reader

Abstract

The invention provides a film coating method, and relates to the technical field of photovoltaics. The method comprises the steps that under the condition that the surface of a film coating container for bearing a silicon wafer is dirty, a dirty covering film is arranged on the film coating container, and the dirty covering film covers a dirty area; the material of the smudginess cover film is the same as that of the to-be-coated layer of the silicon wafer; a film coating container provided with a dirty covering film is used for bearing a silicon wafer, and the silicon wafer is subjected to film coating. In the invention, the dirty cover film plays a role in isolating the silicon wafer from a dirty area, so that the position of the silicon wafer in contact with the coating container is prevented from being polluted by the dirty area; the material of the smudginess cover film is the same as that of the to-be-coated layer of the silicon wafer, so that the smudginess cover film does not bring other impurities to the silicon wafer, and the position, in contact with the coating container, of the silicon wafer is prevented from being polluted by other impurities brought by the smudginess cover film; and the coating container provided with the dirty covering film is used for bearing the silicon wafer and coating the silicon wafer, so that the position of the silicon wafer, which is in contact with the coating container, is prevented from being polluted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photovoltaic technology, and in particular to a film coating method. Background Art

[0002] During the manufacturing process of solar cells, when the coating process is performed, the silicon wafer is placed in a coating container, and the coating container carries the silicon wafer into the cavity of the coating machine.

[0003] Before coating, the surface of the coating container is easily affected by the outside world and becomes dirty. In the prior art, the coating container is baked at a high temperature before coating the silicon wafer.

[0004] However, high-temperature baking is used to remove dirt from the surface of the coating container. Dirt that cannot be decomposed at high temperatures cannot be removed. Direct production will cause the position where the silicon wafer contacts the coating container to be contaminated, which will cause EL (Electro Luminescence) corresponding position to be poor, affecting the production line yield and increasing manufacturing costs. Production line refers to placing the coating container in the position to carry the silicon wafer. After production, the coating container carries the silicon wafer into the cavity of the coating machine. Summary of the invention

[0005] The present invention provides a coating method, aiming to solve the problem in the prior art that dirt that cannot be decomposed at high temperature cannot be removed, and directly putting the silicon wafer into production line will cause the position where the silicon wafer contacts the coating container to be contaminated, thereby causing poor EL corresponding position, affecting the production line yield and increasing manufacturing costs.

[0006] The present invention provides a coating method, comprising:

[0007] When the surface of a coating container carrying silicon wafers is dirty, a dirt covering film is provided on the coating container, and the dirt covering film covers the dirty area; the material of the dirt covering film is the same as the material of the layer to be coated on the silicon wafer; the silicon wafers are coated by using the coating container provided with the dirt covering film to carry the silicon wafers.

[0008] In the present invention, when the surface of the coating container carrying silicon wafers is dirty, a dirt covering film is provided on the coating container, and the dirt covering film covers the dirty area. The dirt covering film serves to isolate the silicon wafer from the dirty area, thereby preventing the position where the silicon wafer contacts the coating container from being contaminated by the dirty area. The material of the dirt covering film is the same as the material of the layer to be coated on the silicon wafer, so the dirty covering film will not bring other impurities to the silicon wafer, thereby preventing the position where the silicon wafer contacts the coating container from being contaminated by other impurities brought by the dirty covering film. Then, the coating container provided with the dirty covering film is used to carry the silicon wafer, and the silicon wafer is coated, thereby preventing the position where the silicon wafer contacts the coating container from being contaminated, resulting in poor EL corresponding position, affecting the production line yield, and increasing manufacturing costs.

[0009] Optionally, when the surface of the coating container carrying the silicon wafer is dirty, providing a dirty covering film on the coating container includes:

[0010] When the film-forming container is transported, the contamination covering film is provided on the film-forming container after transport, and the contamination covering film covers the contamination area.

[0011] Optionally, when the surface of the coating container carrying the silicon wafer is dirty, providing a dirty covering film on the coating container includes:

[0012] When the coating container is placed in the air for a time period greater than or equal to a preset time period, the coating container is provided with the dirt covering film after being placed, and the dirt covering film covers the dirty area.

[0013] Optionally, the preset duration is 4 hours.

[0014] Optionally, the thickness of the dirt covering film is greater than or equal to 20 nanometers.

[0015] Optionally, after providing the dirty covering film on the coating container, the method further comprises:

[0016] The coating container is grasped by a robot arm and placed at a position for supporting the silicon wafer.

[0017] Optionally, the coating container is an aluminum boat.

[0018] Optionally, the dirt covering film is an aluminum oxide film.

[0019] Optionally, the provision of a dirt covering film comprises:

[0020] The first step is to introduce trimethylaluminum into the chamber of the atomic layer deposition machine;

[0021] In the second step, nitrogen is introduced to purge the trimethylaluminum;

[0022] The third step is to introduce ozone;

[0023] The fourth step is to introduce nitrogen to purge the ozone;

[0024] Steps 1 to 4 form a cycle;

[0025] Set the number of loops to 80 to 180.

[0026] Optionally, before introducing trimethylaluminum into the cavity of the atomic layer deposition machine, providing a dirty covering film further comprises:

[0027] The pressure of the chamber of the atomic layer deposition machine is set to 0.002 Torr to 0.005 Torr. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0029] Figure 1 A flow chart showing the steps of a coating method in an embodiment of the present invention is shown;

[0030] Figure 2 A flow chart showing the steps of another coating method in an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The present invention provides a coating method, referring to Figure 1 , Figure 1 A flow chart of the steps of a coating method in an embodiment of the present invention is shown, and the method comprises:

[0033] Step 101, when the surface of a coating container carrying silicon wafers is dirty, a dirt covering film is provided on the coating container, the dirt covering film covers the dirty area; the material of the dirt covering film is the same as the material of the layer to be coated on the silicon wafer.

[0034] In the embodiment of the present invention, the surface of the coating container carrying silicon wafers refers to the surface of the coating container contacting with the silicon wafers, and the surface of the coating container carrying silicon wafers may be the inner surface of the coating container, etc. Dirt specifically refers to dirt; unclean. The surface of the coating container carrying silicon wafers is dirty, which means that the surface of the coating container carrying silicon wafers is not clean, for example, the surface of the coating container carrying silicon wafers is contaminated with dust or oil. In the case where the surface of the coating container carrying silicon wafers is dirty, it means that the surface of the coating container carrying silicon wafers and the silicon wafers that may contact are dirty. A dirty covering film is provided for the coating container, and the dirty covering film covers the dirty area, so that the dirty covering film plays the role of isolating the silicon wafer from the dirty area, and preventing the position of the silicon wafer contacting the coating container from being contaminated by the dirty area; the material of the dirty covering film is the same as the material of the silicon wafer layer to be coated, so that the dirty covering film will not bring other impurities to the silicon wafer, and the position of the silicon wafer contacting the coating container is prevented from being contaminated by other impurities brought by the dirty covering film.

[0035] Step 102: Use a coating container provided with the dirty covering film to carry a silicon wafer and coat the silicon wafer.

[0036] The dirty covering film serves to isolate the silicon wafer from the dirty area, and the material of the dirty covering film is the same as the material of the layer to be coated on the silicon wafer, thereby preventing the position where the silicon wafer contacts the coating container from being contaminated. The coating container provided with the dirty covering film is used to carry the silicon wafer and coat the silicon wafer, thereby preventing the position where the silicon wafer contacts the coating container from being contaminated, resulting in poor EL corresponding position, affecting the production line yield, and increasing manufacturing costs.

[0037] The inventors found that in the prior art, dirt on the surface of the coating container is removed by high-temperature baking. Dirt that cannot be decomposed at high temperatures cannot be removed, and the position where the silicon wafer contacts the coating container will be contaminated if it is directly put on line, which will cause poor EL corresponding position, affect the production line yield, and increase manufacturing costs. In the embodiment of the present invention, the inventors creatively set a dirt covering film on the coating container, and the dirt covering film covers the dirty area; the material of the dirt covering film is the same as the material of the silicon wafer layer to be coated, and then use the coating container with the dirt covering film to carry the silicon wafer, and coat the silicon wafer to avoid the position where the silicon wafer contacts the coating container from being contaminated. When the surface of the coating container carrying silicon wafers is dirty, a dirt covering film is provided on the coating container, and the dirty covering film covers the dirty area. The dirty covering film serves to isolate the silicon wafer from the dirty area, thereby preventing the position where the silicon wafer contacts the coating container from being contaminated by the dirty area. If the material of the dirty covering film is the same as the material of the layer to be coated on the silicon wafer, the dirty covering film will not bring other impurities to the silicon wafer, thereby preventing the position where the silicon wafer contacts the coating container from being contaminated by other impurities brought by the dirty covering film. Then, the coating container provided with the dirty covering film is used to carry the silicon wafers, and the silicon wafers are coated, thereby preventing the position where the silicon wafer contacts the coating container from being contaminated, resulting in poor EL corresponding position, affecting the production line yield, and increasing manufacturing costs.

[0038] Optionally, the aforementioned step 101 may include: in the case of transporting the coated container, providing a dirt covering film on the transported coated container, wherein the dirt covering film covers the dirty area.

[0039] The inventors have discovered that when transporting a coating container, the surface of the coating container after transport may be contaminated with dust or oil, etc., causing the surface of the coating container to be dirty. A dirt covering film is provided for the coating container after transport, and the dirt covering film covers the dirty area. The dirt covering film serves to isolate the silicon wafer from the dirty area, thereby preventing the position where the silicon wafer contacts the coating container from being contaminated by the dirty area. The dirty area here refers to the area where the surface of the coating container is contaminated with dust or oil, etc., causing the surface of the coating container to be dirty. In an embodiment of the present invention, transporting includes long-distance transportation and manual transporting. The situation of transporting a coating container includes: when replacing a new coating container, the new coating container is transported to the position for carrying silicon wafers after being cleaned.

[0040] Optionally, the aforementioned step 101 may include: when the coating container is placed in the air for a time period greater than or equal to a preset time period, setting a dirt covering film on the coating container after placement, wherein the dirt covering film covers the dirty area.

[0041] The inventors also found that when the time of being placed in the air is greater than or equal to the preset time, the surface of the coating container after being placed may be contaminated with dust or water vapor, etc., causing the surface of the coating container to be dirty. A dirt covering film is set on the coating container after being placed, and the dirty covering film covers the dirty area. The dirty covering film plays a role in isolating the silicon wafer from the dirty area, preventing the position where the silicon wafer contacts the coating container from being contaminated by the dirty area. The dirty area here refers to the area where the surface of the coating container is contaminated with dust or water vapor, etc., causing the surface of the coating container to be dirty. For example, when the preset time is 5 hours and the coating container is placed in the air for 6 hours, a dirt covering film is set on the coating container after being placed, and the dirty covering film covers the dirty area.

[0042] Optionally, the preset time is 4 hours. The preset time is 4 hours, that is, when the coating container is placed in the air for a time greater than or equal to 4 hours, a dirt covering film is set on the coating container after placement, and the dirt covering film covers the dirty area, which can avoid excessive dirt covering films on the coating container and save energy. In addition, when the coating container is placed in the air for less than 4 hours, the surface of the coating container after placement is less contaminated with dust or water vapor, which has less impact on the silicon wafer and will not cause poor EL corresponding position. For example, when the coating container is placed in the air for 4.5 hours, a dirt covering film is set on the coating container after placement, and the dirt covering film covers the dirty area.

[0043] Optionally, the thickness of the dirt covering film is greater than or equal to 20 nanometers. For example, the thickness of the dirt covering film may be 20 nm (nanometers), 22 nm, 24 nm, 26 nm, 30 nm, or 35 nm. The thickness of the dirt covering film is greater than or equal to 20 nanometers, which can better cover the dirty area, and after the coating container is provided with the dirt covering film, the surface of the coating container is not easily corroded by water vapor, and can be placed in the air for a longer time, avoiding the need to frequently provide the coating container with the dirt covering film, thereby saving energy.

[0044] Optionally, after the dirty covering film is provided on the coating container, the method further comprises: grabbing the coating container by a robot arm and placing the coating container at a position for carrying silicon wafers. This can avoid bringing oil stains to the coating container by grabbing the coating container by hand, thereby avoiding the position where the silicon wafer contacts the coating container from being contaminated, resulting in poor EL corresponding position, affecting the production line yield, and increasing manufacturing costs.

[0045] Optionally, the coating container is an aluminum boat. The cleaning and replacement cycle of the aluminum boat is long, the service life is longer, and the cost is saved. In the coating process of the solar cell manufacturing process, the preparation of aluminum oxide film and silicon nitride film is changed from one process to two processes, and the preparation of aluminum oxide film is changed to separate preparation. The preparation of aluminum oxide film is usually prepared by ALD (Atomic layer deposition) machine. The ALD machine usually uses an aluminum boat as the coating container, and the silicon wafer is placed in the aluminum boat. The aluminum boat carries the silicon wafer into the cavity of the ALD machine to coat the silicon wafer with aluminum oxide film.

[0046] Optionally, the dirt covering film is an aluminum oxide film. Aluminum oxide film is a passivation film commonly used in solar cells. When the dirt covering film is an aluminum oxide film, no unnecessary impurities are introduced when the silicon wafer is plated with the aluminum oxide film.

[0047] Optionally, a dirty covering film is provided, including: the first step of introducing trimethylaluminum into the chamber of the atomic layer deposition machine; the second step of introducing nitrogen to purge the trimethylaluminum; the third step of introducing ozone; the fourth step of introducing nitrogen to purge the ozone; the first step to the fourth step form a cycle; the number of cycles is set to 80 to 180.

[0048] The number of cycles is set to 80 to 180, for example, the number of cycles can be 80, 100, 120, 140, 160, 180. When the number of cycles is set to 80 to 180, the thickness of the aluminum oxide film obtained is thicker, which can better cover the dirty area, and after the coating container is provided with the dirty covering film, the surface of the coating container is not easily corroded by water vapor, and can be placed in the air for a longer time, avoiding the need to frequently provide the coating container with the dirty covering film, thereby saving energy.

[0049] Optionally, before introducing trimethylaluminum into the cavity of the atomic layer deposition machine, a dirt covering film is provided, and the method further includes: setting the pressure of the cavity of the atomic layer deposition machine to 0.002 torr to 0.005 torr.

[0050] The pressure of the cavity of the atomic layer deposition machine is set to 0.002 Torr to 0.005 Torr. For example, the pressure of the cavity of the atomic layer deposition machine can be 0.002 Torr, 0.003 Torr, 0.0035 Torr, 0.004 Torr, 0.0045 Torr, 0.005 Torr. The pressure of the cavity of the atomic layer deposition machine is set to 0.002 Torr to 0.005 Torr. The lower pressure makes the reaction gas flow faster in the cavity, and the gas will not accumulate at the air inlet end of the cavity, so that the distribution of the reaction gas in the cavity can be more uniform, which is beneficial to the reaction of the reaction gas, so that the uniformity of the aluminum oxide film is better, which is beneficial to the subsequent flat placement of the silicon wafer.

[0051] The present invention will be further explained below in conjunction with specific embodiments. Figure 2 , Figure 2 A flow chart of another coating method in an embodiment of the present invention is shown. In this method, the coating container is an aluminum boat, the dirty covering film is an aluminum oxide film, and the aluminum oxide film is coated on the silicon wafer, specifically comprising the following steps:

[0052] S1. Replace the new aluminum boat, move the cleaned new aluminum boat to the position of the calibration equipment, check the aluminum boat to determine whether the fixing screws are loose, the installation is uneven, and the boat rod is not aligned. Use the calibration equipment to calibrate the aluminum boat to ensure the stability of the aluminum boat and the alignment of the boat teeth without loose movement. After calibration, place the aluminum boat in the corresponding aluminum boat placement position on the carrier plate and record the boat number;

[0053] S2, cavity back pressure, N 2 (nitrogen), N 2 The flow rate is 10000sccm (standard cubic centimeter per minute), and N 2 The time is 90 seconds (seconds), the cavity returns to normal atmospheric pressure, the cavity is opened, the carrier carrying the aluminum boat enters the cavity, the temperature is set to 190℃ (Celsius), and after reaching the set temperature, it is kept warm for 300 seconds;

[0054] S3, the flow rate of TMA (trimethylaluminum) is 2000sccm, and the pressure of the TMA pipeline is set to 27mTorr (mTorr). Maintain a stable pressure to ensure that the amount of TMA introduced is balanced. 3The flow rate of ozone is 6000sccm, and the concentration of ozone is set to 290mg / L (milligrams per liter) to ensure that the concentration of ozone introduced is balanced and the temperature is maintained at 190°C; the pressure of the cavity of the atomic layer deposition machine is set to 0.002Torr. In the first step, trimethylaluminum is introduced into the cavity of the atomic layer deposition machine for 4s; in the second step, nitrogen is introduced to purge trimethylaluminum for 6s; in the third step, ozone is introduced for 10s; in the fourth step, nitrogen is introduced to purge ozone for 4s; the first to fourth steps form a cycle; the number of cycles is set to 80, the time for each cycle is 24s, and N is introduced at the end of each cycle. 2 Carry out purging;

[0055] S4, the pressure is set to 0 mTorr, the time is set to 30 s, and the tail gas is cleaned and discharged to discharge the remaining gas in the chamber and the aluminum oxide powder generated by the reaction that has not been deposited on the silicon wafer;

[0056] S5, cavity back pressure, N 2 , N 2 The flow rate is 10000sccm, and N 2 The time is 90s, the cavity is returned to normal atmospheric pressure, the cavity is opened, and the carrier plate carrying the aluminum boat is taken out of the cavity;

[0057] S6. Cool down for 100 seconds to avoid unsafe behaviors caused by high-temperature loading and unloading. After the cooling time is over, the aluminum boat is grabbed by the robot and placed in the position to carry the silicon wafer.

[0058] In S1, the aluminum boat is calibrated to avoid loosening of the aluminum boat and misalignment of the boat rod after the aluminum oxide film is set on the aluminum boat. Misalignment of the boat rod will cause the aluminum boat to carry silicon wafers for coating, resulting in fragments or jams.

[0059] S2, N 2 The flow rate can be 10000 sccm to 20000 sccm. For example, N 2 The flow rate can be 10000sccm, 12000sccm, 14000sccm, 16000sccm, 18000sccm, 20000sccm. 2 The time can be 60s to 90s. For example, N 2The holding time can be 60s, 65s, 70s, 75s, 80s, 90s. The temperature can be set to 190°C to 245°C, for example, the temperature can be set to 190°C, 200°C, 210°C, 220°C, 230°C, 245°C. The holding time can be 300s to 600s, for example, the holding time can be 300s, 360s, 400s, 450s, 500s, 600s. Insulation can make the temperature distribution in the cavity more uniform, improve the temperature difference in the cavity caused by opening and closing the furnace door, thereby facilitating the balanced reaction in the cavity and the uniformity of the aluminum oxide film on the surface of the aluminum boat.

[0060] In S3, the temperature may be maintained at 190° C. to 245° C., for example, the temperature may be maintained at 190° C., 200° C., 210° C., 220° C., 230° C., 245° C. The flow rate of TMA may be 2000 sccm to 4000 sccm, for example, the flow rate of TMA may be 2000 sccm, 2400 sccm, 2800 sccm, 3200 sccm, 3600 sccm, 4000 sccm. The flow rate of ozone may be 4000 sccm to 8000 sccm, for example, the flow rate of ozone may be 4000 sccm, 4500 sccm, 5000 sccm, 6000 sccm, 7000 sccm, 8000 sccm. The flow rate of TMA and ozone is large, and the thickness of the aluminum oxide film formed is large, which can better cover the dirty area, and after the aluminum boat is set with the aluminum oxide film, the surface of the aluminum boat is not easily corroded by water vapor, and can be placed in the air for a longer time, avoiding the need to frequently set the aluminum oxide film on the aluminum boat, saving energy. The temperature can be maintained at 190°C to 245°C. The lower the temperature, the faster the reaction rate of TMA and ozone, which can save reaction time and process time. In addition, the surface of the aluminum boat is heated, which can reduce some dirt on the surface of the aluminum boat, such as oil stains contaminated by manual handling. The pressure of the TMA pipeline can be set to 27mTorr to 35mTorr, for example, the pressure of the TMA pipeline can be set to 27mTorr, 28mTorr, 29mTorr, 30mTorr, 32mTorr, 35mTorr. The concentration of ozone is set to 290 mg / L to 300 mg / L. For example, the concentration of ozone can be set to 290 mg / L, 292 mg / L, 294 mg / L, 296 mg / L, 298 mg / L, and 300 mg / L.

[0061] In S4, the pressure can be set to 0mTorr to 0.05mTorr, for example, the pressure can be set to 0mTorr, 0.01mTorr, 0.02mTorr, 0.03mTorr, 0.04mTorr, 0.05mTorr. The time can be set to 30s to 60s, for example, the time can be set to 30s, 35s, 40s, 45s, 50s, 60s. The pressure can be set to 0mTorr to 0.05mTorr, the pressure value is small, the exhaust gas cleaning exhaust pumping speed is large, which is conducive to the residual gas in the chamber and the aluminum oxide powder that has not been deposited on the silicon wafer by the reaction to be discharged more fully, avoiding affecting the subsequent deposition of the aluminum oxide film; the time can be set to 30s to 60s, the time is long, which is conducive to the residual gas in the chamber and the aluminum oxide powder that has not been deposited on the silicon wafer by the reaction to be discharged more fully, avoiding affecting the subsequent deposition of the aluminum oxide film.

[0062] In S5, N 2 The flow rate can be 10000 sccm to 20000 sccm. For example, N 2 The flow rate can be 10000sccm, 12000sccm, 14000sccm, 16000sccm, 18000sccm, 20000sccm. 2 The time can be 60s to 90s. For example, N 2 The time may be 60s, 65s, 70s, 75s, 80s, or 90s. In S7, the cooling time may be 100s to 300s, for example, the cooling time may be 100s, 140s, 180s, 220s, 260s, or 300s.

[0063] In S6, the cooling time may be 60 s to 300 s, for example, the cooling time may be 60 s, 120 s, 180 s, 200 s, 240 s, or 300 s.

[0064] Through the above steps, an aluminum oxide film with a thickness of about 20nm to 30nm is formed on the surface of the aluminum boat to prevent the silicon wafer from being directly contacted with the dirty area on the surface of the aluminum boat and being contaminated.

[0065] The silicon wafers were prepared into semi-finished solar cells according to the process before the aluminum oxide coating under the same conditions, and then divided into two groups. The first group used the aluminum boat processed according to the above steps to carry the silicon wafers, coated the silicon wafers with aluminum oxide, and then carried out other processes after the aluminum oxide coating to prepare solar cells as Example 1; the second group used the following steps to process the aluminum boat: A1, replace the new aluminum boat, move the cleaned new aluminum boat to the position of the calibration equipment, check the aluminum boat, determine whether the fixing screws are loose, the installation is uneven, and the boat rod is not aligned, use the calibration equipment to calibrate the aluminum boat, ensure the stability of the aluminum boat and the boat teeth correspond neatly without loose movement, after calibration, put the aluminum boat into the position to carry the silicon wafers, and record the boat number. The aluminum boat processed by the second group was used to carry the silicon wafers, and the silicon wafers were coated with aluminum oxide, and then the other processes after the aluminum oxide coating were carried out under the same conditions as Example 1 to prepare solar cells as Comparative Example 1.

[0066] The solar cells prepared in the comparative example 1 and the embodiment 1 were subjected to EL test under the same test conditions. The EL test results were statistically analyzed, and the statistical results are as follows:

[0067] Table 1 EL test results of comparative example 1 and embodiment 1

[0068] Group quantity The proportion of boat pole position errors Proportion of tooth marks on aluminum boats Comparative Example 1 6400 15% 35% Example 1 6400 0 0

[0069] Usually each aluminum boat has 6 boat rods (two upper boat rods and two lower boat rods are installed in alignment, and the two middle boat rods are movable within a small range). The boat teeth of the aluminum boat serve to separate silicon wafers, fix silicon wafers and limit the movement of silicon wafers; in Table 1 above, the proportion of bad boat rod positions refers to the proportion of the number of solar cells that do not show obvious teeth in bad positions to the number of corresponding groups; the proportion of aluminum boat tooth marks refers to the proportion of the number of solar cells that show obvious teeth in bad positions to the number of corresponding groups; the quantity refers to the number of solar cell samples tested.

[0070] As can be seen from Table 1 above, compared with Comparative Example 1, the proportion of bad boat rod position and the proportion of aluminum boat tooth marks in Example 1 are significantly reduced, and the proportion of bad boat rod position and the proportion of aluminum boat tooth marks in Example 1 are both 0. It shows that the proportion of bad boat rod position and the proportion of aluminum boat tooth marks can be reduced by adopting another coating method in the embodiment of the present invention. Another coating method in the embodiment of the present invention is used to set an aluminum boat with an aluminum oxide film, and the aluminum oxide film covers the dirty area. The aluminum oxide film plays a role in isolating the silicon wafer from the dirty area, and avoids the position where the silicon wafer contacts the aluminum boat from being contaminated by the dirty area; the material of the aluminum oxide film is the same as the material of the silicon wafer layer to be coated, so the aluminum oxide film will not bring other impurities to the silicon wafer; then the aluminum boat with an aluminum oxide film is used to carry the silicon wafer, and the silicon wafer is coated with an aluminum oxide film, so as to avoid the position where the silicon wafer contacts the aluminum boat from being contaminated, resulting in poor EL corresponding position.

[0071] It should be noted that, for the method embodiments, for the sake of simplicity of description, they are all expressed as a series of action combinations, but those skilled in the art should be aware that the embodiments of the present application are not limited by the described order of actions, because according to the embodiments of the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions involved are not necessarily required by the embodiments of the present application.

[0072] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0073] Through the description of the above implementation methods, those skilled in the art can clearly understand that the above-mentioned embodiment methods can be implemented by means of software plus a necessary general hardware platform, and of course by hardware, but in many cases the former is a better implementation method. Based on such an understanding, the technical solution of the present invention, or the part that contributes to the prior art, can be embodied in the form of a software product, which is stored in a storage medium (such as ROM / RAM, a magnetic disk, or an optical disk), and includes a number of instructions for enabling a terminal (which can be a mobile phone, a computer, a server, an air conditioner, or a network device, etc.) to execute the methods described in each embodiment of the present invention.

[0074] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.

Claims

1. A coating method, characterized in that: include: When the surface of the coating container carrying the silicon wafer is dirty, a dirt covering film is provided on the coating container, wherein the dirt covering film covers the dirty area; The material of the dirty covering film is the same as the material of the silicon wafer layer to be coated; The coating container provided with the dirty covering film is used to carry silicon wafers, and the silicon wafers are coated.

2. The coating method according to claim 1, characterized in that: When the surface of the coating container carrying the silicon wafer is dirty, the coating container is provided with a dirty covering film, comprising: When the film-forming container is transported, the contamination covering film is provided on the film-forming container after transport, and the contamination covering film covers the contamination area.

3. The coating method according to claim 1, characterized in that: When the surface of the coating container carrying the silicon wafer is dirty, the coating container is provided with a dirty covering film, comprising: When the coating container is placed in the air for a time period greater than or equal to a preset time period, the coating container is provided with the dirt covering film after being placed, and the dirt covering film covers the dirty area.

4. The coating method according to claim 3, characterized in that: The preset duration is 4 hours.

5. The coating method according to any one of claims 1 to 4, characterized in that: The thickness of the dirt covering film is greater than or equal to 20 nanometers.

6. The coating method according to any one of claims 1 to 4, characterized in that: After the dirty covering film is provided on the coating container, the method further comprises: The coating container is grasped by a robot arm and placed at a position for supporting the silicon wafer.

7. The coating method according to any one of claims 1 to 4, characterized in that: The coating container is an aluminum boat.

8. The coating method according to any one of claims 1 to 4, characterized in that: The dirt covering film is an aluminum oxide film.

9. The coating method according to claim 8, characterized in that: The step of providing a dirty covering film comprises: The first step is to introduce trimethylaluminum into the chamber of the atomic layer deposition machine; In the second step, nitrogen is introduced to purge the trimethylaluminum; The third step is to introduce ozone; The fourth step is to introduce nitrogen to purge the ozone; Steps 1 to 4 form a cycle; Set the number of loops to 80 to 180.

10. The coating method according to claim 9, characterized in that: Before introducing trimethylaluminum into the cavity of the atomic layer deposition machine, the dirty covering film is provided, and further comprises: The pressure of the chamber of the atomic layer deposition machine is set to 0.002 Torr to 0.005 Torr.