Modification method for improving oxidation resistance of aluminide cladding coating
Through the plasma cladding process and the addition of modified elements, the anti-oxidation performance of the aluminide cladding coating is improved, the oxidation and corrosion problems of the existing aluminide coating in high-temperature environments are solved, and the processing of complex-shaped workpieces is realized. Efficient protection.
Patent Information
- Application Number
- CN202410782615.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-18
AI Technical Summary
Existing aluminide coatings are prone to oxidation and corrosion in high-temperature, high-pressure, and high-humidity environments. As the service time is extended and the power of the unit increases, the oxidation resistance decreases, making it difficult to meet the anti-oxidation and thermal corrosion resistance requirements of complex-shaped workpieces.
The aluminide cladding coating is prepared using a plasma cladding process. Pd and Ti elements are added to the cladding powder for co-modification, and NH4Cl is added to the components to improve the stability and oxidation resistance of the coating. Plasma is used to The advantages of concentrated heat and short action time of the cladding process improve the bonding strength between the aluminide coating and the base material.
Significantly improves the anti-oxidation performance and stability of the aluminide cladding coating, enhances its anti-oxidation ability in high-temperature water vapor environments, has high production efficiency, controllable thickness, strong process repeatability, and is suitable for large diameters For workpieces with complex shapes.
Smart Images

Figure CN118773601A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material surface alloying and coating preparation, and specifically relates to a modification method for improving the oxidation resistance of an aluminide cladding coating. Background Art
[0002] In industrial production, boiler pipes play an important role in energy transmission and production process. Since boiler pipes often work in harsh environments such as high temperature, high pressure, and high humidity, they are easily affected by oxidation and corrosion, and measures need to be taken to protect the pipe surface from oxidation erosion. Therefore, it is of great practical significance to research and develop anti-oxidation and corrosion-resistant technologies for the inner and outer wall surfaces of pipes used in boiler units.
[0003] Studies have shown that high-temperature coatings have significant effects in solving the problems of component oxidation corrosion, wear, and high-temperature ablation, and are widely used in various industrial boiler systems. Although the current aluminide coatings have shown excellent antioxidant capabilities on the flow-through components of energy equipment with large aspect ratios, as the service time increases and the unit power increases, the reduction in Al content in the coating will inevitably affect the coating's antioxidant properties. In addition, the antioxidant and thermal corrosion resistance of a single aluminide coating under complex working conditions such as thermal corrosion, oxidation, and flue gas needs to be improved.
[0004] Therefore, there is an urgent need for a modification method to improve the oxidation resistance of aluminide cladding coatings, so as to realize the preparation of new, comprehensive and excellent oxidation-resistant and heat-corrosion-resistant coatings suitable for various complex-shaped workpieces with large aspect ratios. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art and provide a new technical solution for a modification method for improving the oxidation resistance of an aluminide cladding coating.
[0006] According to one aspect of the present invention, a modification method for improving the oxidation resistance of an aluminide cladding coating is provided, comprising the following steps:
[0007] Step S1, the solid phase components are 50-80% NiAl, 10-40% Al, 1-5% Pd, 2-5% Ti and 2-5% NH 4 Cl is stirred, ball-milled and dried to prepare a cladding powder; wherein the sum of the mass percentages of the solid phase components is 100%;
[0008] Step S2, cleaning the surface of the workpiece to be plated, and pouring a sufficient amount of cladding powder into the feed port of the ion cladding device;
[0009] Step S3, placing the workpiece to be plated under an inert atmosphere, using an ion cladding device to spray cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating after cooling;
[0010] Step S4, treating the cladding residue.
[0011] Optionally, in step S1, NiAl, Al, Pd, and Ti are all in powder form, and NiAl, Al, Pd, and Ti are all sieved through a 1000-mesh sieve.
[0012] Optionally, in step S1, the cladding powder is obtained by wet-grinding a solid phase component with a planetary ball mill and then drying it.
[0013] Optionally, when the solid phase component is wet-milled in a planetary ball mill, the wet-milling medium is anhydrous ethanol, the ball milling speed is 350-400 rpm, the time is 12-24 h, and the drying conditions are vacuum drying at 80-120° C. for 12-24 h.
[0014] Optionally, the process parameters of plasma cladding are as follows:
[0015] The cladding current is 80-120A, the feed rate is 18-22g / min, the scanning rate is 20-40cm / min, the nozzle height is 8-12mm, the rotation speed is 2-5r / min, the ion gas flow rate is 0.2-0.3L / min, and the shielding gas flow rate is 18-20L / min.
[0016] Optionally, the inert gas in the inert atmosphere is Ar or N 2 .
[0017] Optionally, in step S2, the surface of the workpiece to be plated is cleaned with a high-pressure water gun for 5 minutes and then rinsed with alcohol or acetone.
[0018] Optionally, the cladding residue is treated, including:
[0019] Use a high-pressure water gun to wash away the cladding residue on the surface of the workpiece and let it dry naturally.
[0020] Optionally, in step S3, the thickness of the aluminide cladding coating is 0.78-1.84 mm.
[0021] Optionally, the mass percentage of NiAl is 50%, the mass percentage of Al is 35%, the mass percentage of Pd is 5%, the mass percentage of Ti is 5%, and the mass percentage of NH 4 The mass percentage of Cl is 5%.
[0022] A technical effect of the present invention is:
[0023] In the embodiment of the present application, the modification method for improving the anti-oxidation performance of the aluminide cladding coating is to prepare the aluminide cladding coating by adopting a plasma cladding process. Since the plasma cladding process has the advantages of concentrated heat, short action time, and small thermal influence in the cladding area, the aluminide cladding coating has a high bonding strength with the parent material. At the same time, the modification method for improving the anti-oxidation performance of the aluminide cladding coating is to prepare the aluminide cladding coating through an integrated production line, which not only has high production efficiency and controllable thickness of the aluminide cladding coating, but also has high process repeatability and is extremely practical.
[0024] In addition, by adding Pd and Ti elements to the components of the cladding powder to co-modify the aluminide coating, the stability and density of the aluminide cladding coating are significantly improved, and the anti-oxidation performance of the aluminide cladding coating is enhanced. 4 Cl plays a role in catalyzing and activating the infiltration, thereby improving the infiltration rate and the quality of the aluminide cladding coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A schematic flow chart of a modification method for improving the oxidation resistance of an aluminide cladding coating according to an embodiment of the present invention;
[0026] Figure 2 Schematic diagram of the cross-sectional morphology of an aluminide cladding coating according to an embodiment of the present invention. DETAILED DESCRIPTION
[0027] Various exemplary embodiments of the present application will now be described in detail with reference to the accompanying drawings. It should be noted that unless otherwise specifically stated, the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present application.
[0028] The embodiments of the present application will be described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and should not be construed as limitations on the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0029] The term "first" or "second" in the specification and claims of this application may include one or more of the features explicitly or implicitly. In the description of this application, unless otherwise specified, "plurality" means two or more. In addition, "and / or" in the specification and claims means at least one of the connected objects, and the character " / " generally means that the objects connected before and after are in an "or" relationship.
[0030] According to one aspect of the present invention, see Figure 1 , provides a modification method for improving the oxidation resistance of aluminide cladding coatings, which is suitable for the preparation of oxidation-resistant coatings of austenitic steel and high-temperature alloy parts used in large boilers, oil and gas field pipelines and other workpieces with large aspect ratios and various complex shapes.
[0031] Specifically, the modification method for improving the oxidation resistance of the aluminide cladding coating comprises the following steps:
[0032] Step S1, the solid phase components are 50-80% NiAl, 10-40% Al, 1-5% Pd, 2-5% Ti and 2-5% NH 4 Cl is stirred, ball-milled and dried to prepare a cladding powder; wherein the sum of the mass percentages of the solid phase components is 100%; wherein the infiltration source is NiAl, Al powder, the modifier is Pd, Ti, and the activator is NH 4 Cl;
[0033] Step S2, cleaning the surface of the workpiece to be plated, and pouring a sufficient amount of cladding powder into the feed port of the ion cladding device;
[0034] Step S3, placing the workpiece to be plated under an inert atmosphere, using an ion cladding device to spray cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating after cooling;
[0035] Step S4, treating the cladding residue.
[0036] In the embodiment of the present application, the modification method for improving the anti-oxidation performance of the aluminide cladding coating is to prepare the aluminide cladding coating by adopting a plasma cladding process. Since the plasma cladding process has the advantages of concentrated heat, short action time, and small thermal influence in the cladding area, the aluminide cladding coating has a high bonding strength with the parent material. At the same time, the modification method for improving the anti-oxidation performance of the aluminide cladding coating is to prepare the aluminide cladding coating through an integrated production line, which not only has high production efficiency and controllable thickness of the aluminide cladding coating, but also has high process repeatability and is extremely practical.
[0037] In addition, by adding Pd and Ti elements to the components of the cladding powder to co-modify the aluminide coating, the stability and density of the aluminide cladding coating are significantly improved, and the anti-oxidation performance of the aluminide cladding coating is enhanced. 4 Cl plays a role in catalyzing and activating the infiltration, thereby improving the infiltration rate and the quality of the aluminide cladding coating.
[0038] It should be noted that the addition of the modifying element Pd can inhibit the diffusion of the Al element, maintain the Al content in the NiAl phase and the aluminide cladding coating, and form a dense oxide film during oxidation, thereby improving the antioxidant performance.
[0039] The addition of modified element Ti can promote the oxide film transformation process and accelerate the θ-Al 2 O 3 Opposite α-Al 2 O 3 In addition, it can produce fine-grained corrosion products, improve the "stickiness" of the oxide film, and further enhance the oxidation and corrosion resistance of the coating.
[0040] Optionally, in step S1, NiAl, Al, Pd, and Ti are all in powder form, and NiAl, Al, Pd, and Ti are all sieved through a 1000-mesh sieve.
[0041] In the above embodiment, it helps to ensure that each component is dispersed more evenly and finely, and remove impurities and particles therein, thereby better ensuring the cladding effect of the aluminide cladding coating.
[0042] Optionally, in step S1, the cladding powder is obtained by wet-grinding a solid phase component with a planetary ball mill and then drying it.
[0043] In the above embodiment, a cladding powder in which each component is fully and evenly mixed can be obtained, which helps to better ensure the quality of the aluminide cladding coating during the cladding process.
[0044] Optionally, when the solid phase component is wet-milled in a planetary ball mill, the wet-milling medium is anhydrous ethanol, the ball milling speed is 350-400 rpm, the time is 12-24 h, and the drying conditions are vacuum drying at 80-120° C. for 12-24 h.
[0045] In the above-mentioned embodiment, the wet grinding method of the solid phase component is relatively reasonable, which helps to ensure the uniform fineness of the cladding powder.
[0046] Optionally, the process parameters of plasma cladding are as follows:
[0047] The cladding current is 80-120A, the feed rate is 18-22g / min, the scanning rate is 20-40cm / min, the nozzle height is 8-12mm, the rotation speed is 2-5r / min, the ion gas flow rate is 0.2-0.3L / min, and the shielding gas flow rate is 18-20L / min.
[0048] In the above embodiment, the various parameters of the plasma cladding process are reasonably set, so that the cladding process has the advantages of concentrated heat, short action time, and small thermal impact in the cladding area, thereby making the bonding strength between the aluminide cladding coating and the parent material higher.
[0049] Optionally, the inert gas in the inert atmosphere is Ar or N 2 . Using chemically stable Ar or N 2 Providing an inert atmosphere helps to ensure that the workpiece to be plated is not oxidized during the cladding process.
[0050] Optionally, in step S2, the surface of the workpiece to be plated is cleaned with a high-pressure water gun for 5 minutes and then rinsed with alcohol or acetone.
[0051] In the above embodiment, oil stains, dust, etc. on the surface of the workpiece to be plated can be well removed, and the oxide scale can be removed, and it can be rinsed with alcohol or acetone to provide a neat and metallic surface for subsequent cladding, thereby helping to ensure the strength and stability of the combination between the workpiece surface and the aluminide cladding coating.
[0052] Optionally, the cladding residue is treated, including:
[0053] Use a high-pressure water gun to wash away the cladding residue on the surface of the workpiece and let it dry naturally.
[0054] In the above embodiment, the cladding residue can be thoroughly processed to ensure the cleanliness of the workpiece surface.
[0055] Optionally, in step S3, the thickness of the aluminide cladding coating is 0.78-1.84 mm, which makes the aluminide cladding coating have good metallurgical bonding performance, so that the aluminide cladding coating has high bonding strength with the parent material.
[0056] Optionally, the mass percentage of NiAl is 50%, the mass percentage of Al is 35%, the mass percentage of Pd is 5%, the mass percentage of Ti is 5%, and the mass percentage of NH 4 The mass percentage of Cl is 5%.
[0057] In the above embodiment, the Pd element, the Ti element, the NH 4 The mass percentage of Cl is relatively reasonable, which not only helps to further improve the stability and density of the aluminide cladding coating, enhance the oxidation resistance of the aluminide cladding coating, but also helps to further improve the quality of the aluminide cladding coating.
[0058] It should be noted that the modification method for improving the oxidation resistance of the aluminide cladding coating can prepare an aluminide oxidation resistance coating with a thickness of 0.78-1.84 mm and good metallurgical bonding under the conditions of adjusting the main process parameters such as the composition of the cladding powder, the proportion of the modified elements added, and the plasma cladding parameters. Moreover, the aluminide cladding coating obtained by the present invention has an oxidation resistance of 20 to 64 times that of the parent material in a 600°C pure water vapor environment, and an oxidation resistance of 24 to 86 times that of the parent material in a 650°C pure water vapor environment, which can be explained that the aluminide cladding coating of the present invention effectively improves the oxidation resistance of the alloy parent material in a water vapor environment.
[0059] Example 1
[0060] Step S1, weighing each component of the solid phase component according to mass percentage, including 50% NiAl, 35% Al, 5% Pd, 5% Ti and 5% NH 4 Cl, placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 380 rpm, the time is 24 h, and vacuum drying is performed at 100 ° C for 24 h to obtain the cladding powder.
[0061] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0062] Step 3: Place the workpiece to be plated in Ar or N 2 In an inert atmosphere, an ion cladding device is used to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and after cooling, an aluminide cladding coating with antioxidant properties is obtained. The plasma cladding process parameters are: cladding current of 90A, feed rate of 18g / min, scanning rate of 35cm / min, nozzle height of 10mm, rotation speed of 3r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0063] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0064] Example 2-Example 11
[0065] The cladding process of Example 2 to Example 11 is the same as that of Example 1. Example 1 to Example 11 maintain the same ratio of the penetrant component. The specific conditions are shown in Table 1. Table 1 is the specific parameters of Example 1 to Example 11 of the modification method for improving the antioxidant properties of the aluminide cladding coating. According to the preparation steps in the above Example 1 and the specific preparation parameters in the table, aluminide cladding coatings of different thicknesses can be obtained.
[0066] Table 1
[0067]
[0068] By analyzing and studying the above-mentioned embodiments, the thickness of the infiltration layer is measured to be about 0.78-1.84 mm. The specific results are shown in Table 1. The cross-sectional morphology of the cladding coating prepared in Example 1 is as follows: Figure 2 As shown in Table 1 and the cross-sectional morphology, it is found that the diffusion layer has a uniform structure, moderate thickness, sufficient diffusion of Al atoms, and a good metallurgical bond between the diffusion layer and the matrix, and is not easy to fall off.
[0069] Example 12
[0070] Step S1, weighing each component of the solid phase component according to mass percentage, including 80% NiAl, 10% Al, 2% Pd, 4% Ti and 4% NH 4 Cl, placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 350 rpm, the time is 24 h, and vacuum drying is performed at 100 ° C for 24 h to obtain the cladding powder.
[0071] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0072] Step 3: Place the workpiece to be plated in Ar or N 2 In an inert atmosphere, an ion cladding device is used to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and after cooling, an aluminide cladding coating with antioxidant properties is obtained. The plasma cladding process parameters are: cladding current of 110A, feed rate of 20g / min, scanning rate of 35cm / min, nozzle height of 10mm, rotation speed of 2r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0073] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0074] Example 13
[0075] Step S1, weighing each component of the solid phase component according to mass percentage, including 60% NiAl, 30% Al, 3% Pd, 2% Ti and 5% NH 4 Cl, placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 400 rpm, the time is 24 h, and vacuum drying at 120 ° C for 24 h to obtain the cladding powder.
[0076] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0077] Step 3, placing the workpiece to be plated under an inert atmosphere of Ar, using an ion cladding device to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating with antioxidant properties after cooling. The plasma cladding process parameters are: cladding current of 120A, feed rate of 20g / min, scanning rate of 40cm / min, nozzle height of 12mm, rotation speed of 5r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0078] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0079] Embodiment 14
[0080] Step S1, weighing each component of the solid phase component according to mass percentage, including 60% NiAl, 30% Al, 1% Pd, 4% Ti and 5% NH 4 Cl, placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 400 rpm, the time is 24 h, and vacuum drying at 80 ° C for 24 h to obtain the cladding powder.
[0081] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0082] Step 3, placing the workpiece to be plated under an inert atmosphere of Ar, using an ion cladding device to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating with antioxidant properties after cooling. The plasma cladding process parameters are: cladding current of 120A, feed rate of 20g / min, scanning rate of 30cm / min, nozzle height of 10mm, rotation speed of 4r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0083] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0084] Embodiment 15
[0085] Step S1, weighing each component of the solid phase component according to mass percentage, including 65% NiAl, 25% Al, 4% Pd, 4% Ti and 2% NH 4 Cl, placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 400 rpm, the time is 24 h, and vacuum drying at 120 ° C for 18 h to obtain the cladding powder.
[0086] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0087] Step 3: Place the workpiece to be plated in Ar or N 2 In an inert atmosphere, an ion cladding device is used to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and after cooling, an aluminide cladding coating with antioxidant properties is obtained. The plasma cladding process parameters are: cladding current of 90A, feed rate of 19g / min, scanning rate of 38cm / min, nozzle height of 10mm, rotation speed of 4r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0088] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0089] Example 16
[0090] Step S1, weighing each component of the solid phase component according to mass percentage, including 75% NiAl, 20% Al, 1% Pd, 2% Ti and 2% NH 4 Cl, placing it in a planetary ball mill for wet grinding, wherein the wet grinding medium is anhydrous ethanol, the ball milling speed is 380 rpm, the time is 24 h, and vacuum drying at 110 ° C for 24 h to obtain the cladding powder.
[0091] Step 2: Use a high-pressure water gun to clean the surface of the workpiece to be plated for 5 minutes, and then rinse it with alcohol or acetone.
[0092] Step 3, placing the workpiece to be plated under an inert atmosphere of Ar, using an ion cladding device to spray the cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating with antioxidant properties after cooling. The plasma cladding process parameters are: cladding current of 110A, feed rate of 21g / min, scanning rate of 30cm / min, nozzle height of 10mm, rotation speed of 3r / min, ion gas flow rate of 0.2L / min, and shielding gas flow rate of 19L / min.
[0093] Step S4: After the cladding is completed, the residue on the surface of the workpiece is washed with a high-pressure water gun or a high-pressure air flow, and the workpiece is naturally dried.
[0094] In the embodiments of the present application, the aluminide cladding coating prepared by the modification method for improving the anti-oxidation performance of the aluminide cladding coating is suitable for austenitic steel and high-temperature alloy components used in large boilers, oil and gas field transportation pipelines and other workpieces with large aspect ratios and various complex shapes. It is not only highly practical, has a high diffusion rate, and excellent membrane-base bonding strength, but also has excellent industrial mass production benefits.
[0095] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A modification method for improving the oxidation resistance of an aluminide cladding coating, characterized in that: The steps include: Step S1, stirring, ball-milling and drying 50-80% NiAl, 10-40% Al, 1-5% Pd, 2-5% Ti and 2-5% NH4Cl according to mass percentage of solid phase components to prepare cladding powder; wherein the sum of the mass percentages of the solid phase components is 100%; Step S2, cleaning the surface of the workpiece to be plated, and pouring a sufficient amount of cladding powder into the feed port of the ion cladding device; Step S3, placing the workpiece to be plated under an inert atmosphere, using an ion cladding device to spray cladding powder onto the surface of the workpiece to be plated for plasma cladding, and obtaining an aluminide cladding coating after cooling; Step S4, treating the cladding residue.
2. The modification method for improving the oxidation resistance of aluminide cladding coating according to claim 1 is characterized in that: In step S1, NiAl, Al, Pd, and Ti are all in powder form, and NiAl, Al, Pd, and Ti are all sieved through a 1000-mesh sieve.
3. The modification method for improving the oxidation resistance of aluminide cladding coating according to claim 1 is characterized in that: In step S1, the cladding powder is obtained by wet-grinding the solid phase components with a planetary ball mill and then drying them.
4. The modification method for improving the oxidation resistance of aluminide cladding coating according to claim 3 is characterized in that: When the solid phase components are wet-milled in a planetary ball mill, the wet-milling medium is anhydrous ethanol, the ball milling speed is 350-400 rpm, the time is 12-24 h, and the drying conditions are vacuum drying at 80-120° C. for 12-24 h.
5. The modification method for improving the oxidation resistance of aluminide cladding coating according to claim 1, characterized in that: The process parameters of plasma cladding are as follows: The cladding current is 80-120A, the feed rate is 18-22g / min, the scanning rate is 20-40cm / min, the nozzle height is 8-12mm, the rotation speed is 2-5r / min, the ion gas flow rate is 0.2-0.3L / min, and the shielding gas flow rate is 18-20L / min.
6. The modification method for improving the oxidation resistance of aluminide cladding coating according to claim 1, characterized in that: The inert gas in the inert atmosphere is Ar or N2.
7. The modification method for improving the oxidation resistance of aluminide cladding coating according to claim 1, characterized in that: In step S2, the surface of the workpiece to be plated is cleaned with a high-pressure water gun for 5 minutes and then rinsed with alcohol or acetone.
8. The modification method for improving the oxidation resistance of aluminide cladding coating according to claim 1, characterized in that: Treatment of cladding residues, including: Use a high-pressure water gun to wash away the cladding residue on the surface of the workpiece and let it dry naturally.
9. The modification method for improving the oxidation resistance of aluminide cladding coating according to claim 1, characterized in that: In step S3, the thickness of the aluminide cladding coating is 0.78-1.84 mm.
10. The modification method for improving the oxidation resistance of aluminide cladding coating according to claim 1, characterized in that: The mass percentage of NiAl is 50%, the mass percentage of Al is 35%, the mass percentage of Pd is 5%, the mass percentage of Ti is 5%, and the mass percentage of NH4Cl is 5%.
Citation Information
Patent Citations
New powder composition and use thereof
CN107530771A
Active element-modified beta-NiAl coating and preparation method and workpiece thereof
CN108660412A
Process of using ion fusion covering technology for preparing metal surface coating
CN110424006A
Plasma cladding method for TiC enhanced Al-Co-Cr-Fe-Ni-Nb high-entropy alloy curved surface coating
CN114540808A
Method for preparing Dy modified aluminide coating on surface of nickel-based superalloy
CN115976462A
Cited By
Aluminum-based cladding coating and modification method thereof
CN119859784A
Modification method for improving corrosion resistance of aluminide anti-oxidation coating
CN120006279A