Device and method for preparing large-diameter air-cooled monofilaments
Through the large-diameter air-cooled monofilament preparation device, air-cooling treatment and multi-stage stretching and shaping technology are used to solve the problem that traditional cooling methods are difficult to meet the cooling needs of large-diameter monofilaments, achieving efficient and uniform cooling and performance improvement.
Patent Information
- Application Number
- CN202411084988.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-15
AI Technical Summary
Traditional cooling methods are difficult to meet the high requirements for cooling speed and cooling uniformity of large-diameter monofilaments, resulting in uneven crystallization inside the fiber and reduced performance.
Using a large-diameter air-cooled monofilament preparation device, the matrix and reinforcement materials are mixed to a molten state through a heating and melting unit, spun into triangular-like fibers, and air-cooled in the air-cooled area, combined with multi-stage stretching and shaping treatments , improve heat dissipation efficiency and cooling uniformity.
It improves the cooling speed and uniformity of the monofilament, enhances material properties, reduces internal stress, and improves fiber stability and durability.
Smart Images

Figure CN118773754A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of monofilament preparation, and in particular to a preparation device and method of large-diameter air-cooled monofilament. Background Art
[0002] In the field of textiles and materials science, large-diameter monofilaments play an important role in multiple industrial applications due to their unique physical, chemical and mechanical properties. These applications include but are not limited to reinforcement materials, filter media, medical sutures, high-end ropes and cables, etc. However, in the preparation process of large-diameter monofilaments, the cooling and forming process is particularly critical, which directly affects the quality and performance of the final product.
[0003] Traditional cooling methods, such as natural cooling or simple water cooling, often have problems such as low cooling efficiency and uneven cooling, and it is difficult to meet the high requirements of large-diameter monofilaments for cooling speed and cooling uniformity. Especially when the diameter of the monofilament increases, the internal heat transfer and dissipation becomes more difficult, which can easily lead to uneven crystallization inside the fiber and decreased performance.
[0004] Therefore, a preparation device and method for large-diameter air-cooled monofilament are designed to solve the above problems. Summary of the invention
[0005] The invention overcomes the shortcomings of the prior art and provides a device and method for preparing large-diameter air-cooled monofilaments.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a large-diameter air-cooled monofilament, comprising the following steps:
[0007] Step S1, taking a certain amount of matrix material and reinforcement material, slicing the matrix material and reinforcement material to obtain matrix particles and reinforcement particles;
[0008] Step S2, pre-treating the obtained reinforcement particles, mixing the pre-treated reinforcement particles and matrix particles uniformly, and heating the uniformly mixed reinforcement particles and matrix particles to a molten state to obtain a raw material mixture;
[0009] Step S3, spinning the molten raw material mixture, and extruding it through a spinning head to form a triangular fiber shape, thereby obtaining a fiber with a parallel double-layer structure;
[0010] Step S4, introducing the fiber into the air cooling area, controlling the blowing angle during the air cooling treatment of the fiber, and stretching and collecting the air-cooled fiber to prepare a triangular parallel double-layer structure fiber monofilament.
[0011] In a preferred embodiment of the present invention, in the step S1, the base material includes: one or more of TPEE, TPU, PP, and PE;
[0012] The reinforcement material includes: one or more of PA6, PA66, PBT, and PET;
[0013] The ratio between the matrix material and the reinforcement material is 1-2:2-3.
[0014] In a preferred embodiment of the present invention, in step S2, the uniformly mixed reinforcement particles and matrix particles are heated to a molten state. Specifically, they are heated at 220-290° C. for 6-12 minutes to be in a molten state.
[0015] In a preferred embodiment of the present invention, in the step S2, the reinforcement particles are pre-treated, including cleaning, drying, and surface modification;
[0016] The surface modification of the reinforcement particles is specifically carried out by mixing the reinforcement particles with a silane coupling agent at 80-90° C. for 20-30 minutes.
[0017] In a preferred embodiment of the present invention, in step S4, the fibers are subjected to air cooling treatment, specifically, the triangular-shaped fibers are introduced into an air cooling area, wherein the temperature of the air cooling area is controlled between 25-45°C, the humidity is controlled between 30%-60%, and the blowing angle is specifically that the wind direction is at an angle of 30-45° to the fiber axis, and the wind speed is in the range of 10-20m / s, so as to blow evenly on the fiber surface.
[0018] In a preferred embodiment of the present invention, in step S4, the method for stretching and collecting the air-cooled fibers comprises the following steps:
[0019] Step S41, spraying the oil agent evenly on the surface of the fiber after air cooling, and setting the stretched diameter of the fiber;
[0020] Step S42, introducing the fiber into the three-stage stretching and drawing roller, and stretching and drawing the fiber at a temperature between 60 and 200° C. with a drawing multiple of 2 to 5 times, thereby completing the three-stage stretching and drawing;
[0021] Step S43, the fiber that has completed the third-level traction is introduced into the second-level shaping hot roller, and is traction-shaped at 150-240°C with a traction force of 1-2 times the drafting multiple, and the second-level traction shaping is completed and collected into a roll to obtain a triangular parallel double-layer structure fiber monofilament.
[0022] In a preferred embodiment of the present invention, in the step S41, the stretching diameter, specifically, the fiber diameter reaches a threshold value in the range of 0.07-0.20 mm.
[0023] In a preferred embodiment of the present invention, in the step S42, three-stage stretching and drawing is completed, specifically, the fiber is introduced into a traction hot roller with a temperature between 60-100°C, and the fiber is stretched and drawn with a stretching multiple of 2-3 times to complete the first stage of stretching and drawing. The fiber that has completed the second stage of stretching and drawing is introduced into a traction hot roller with a temperature between 100-150°C, and the fiber is stretched and drawn again with a stretching multiple of 3-4 times to complete the second stage of stretching and drawing. The fiber is then introduced into a traction hot roller with a temperature between 150-200°C, and the fiber is stretched and drawn with a stretching multiple of 4-5 times to complete the third stage of stretching and drawing.
[0024] In a preferred embodiment of the present invention, in the step S43, secondary traction and shaping is completed, specifically, the fiber that has completed the third-stage stretching and traction is introduced into a shaping hot roller with a temperature between 150-200°C, and the fiber is stretched and shaped using a shaping stretching multiple of 1-1.5 times to complete the first-stage traction and shaping, and then the fiber is introduced into a shaping hot roller with a temperature between 200-240°C, and the fiber is stretched and shaped using a shaping stretching multiple of 1.5-2 times to complete the second-stage traction and shaping.
[0025] A large-diameter air-cooled monofilament preparation device comprises: a heating and melting unit, a spinning die head, an air-cooling unit, a stretching unit and a shaping unit, and a control unit;
[0026] The heating and melting unit is used to mix the matrix particles and the reinforcement particles uniformly and heat them to a molten state. The spinning die is installed at the extrusion outlet of the heating and melting unit, and a triangular flow channel is opened in the spinning die;
[0027] The air cooling unit is used to quickly air cool the spun fibers;
[0028] The stretching unit and the shaping unit are used to perform multi-stage stretching and shaping treatment on the air-cooled fibers, and the stretching unit and the shaping unit include: three groups of traction hot rollers; the three groups of traction hot rollers are alternately installed left and right in the vertical falling direction of the monofilaments, and two traction hot rollers are symmetrically arranged in each group;
[0029] The shaping unit comprises two sets of shaping hot rollers; the two sets of shaping hot rollers are located below the traction hot rollers, and the shaping hot rollers have the same structure as the traction hot rollers;
[0030] The control unit is used to control the temperature and time of the heating and melting unit for mixing and heating the matrix particles and the reinforcement particles, control the wind speed, blowing time and blowing angle of the air cooling unit, and control the stretching parameters of the stretching unit and the shaping unit.
[0031] The present invention solves the defects existing in the background technology and has the following beneficial effects:
[0032] (1) The present invention provides a device and method for preparing large-diameter air-cooled monofilaments. By preparing a parallel double-layer structure fiber monofilament similar to a triangular monofilament, the surface area of the monofilament is increased, thereby enhancing the molecular heat exchange efficiency between the monofilament and the cooling air, accelerating the heat loss and cooling speed; at the same time, the double-layer structure balances the problem of local excessive cooling and improves the uniformity of cooling, thereby further improving the heat dissipation efficiency while ensuring uniform cooling.
[0033] (2) The present invention improves the dispersibility of the reinforcement particles in the matrix particles by modifying the reinforcement material, ensures the uniform distribution of the particles in the matrix, enhances the compatibility between the matrix particles and the reinforcement particles, promotes the interface bonding between the two, improves the uniformity of the mixing of the matrix material and the reinforcement material, and further improves the overall performance of the composite material; at the same time, the monofilament obtained by using the matrix material and the reinforcement material realizes the complementarity between the materials, thereby improving the overall performance of the monofilament.
[0034] (3) The present invention improves the heat exchange efficiency between air and fiber by air cooling the fiber having a parallel double-layer structure. While accelerating the cooling rate, it reduces the internal stress caused by the different shrinkage rates of two materials with different properties, thereby improving the stability and durability of the fiber.
[0035] (4) The present invention prepares triangular-shaped fibers and cooperates with the air-cooling area so that the airflow can bypass various parts of the fiber, including the corners and the back, thereby achieving full coverage of the fiber surface, ensuring that the cooling rates of the corner areas and the center area are consistent, reducing local overheating or overcooling, and thus improving the overall cooling uniformity and efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.
[0037] Figure 1 It is a flow chart of a method for preparing a large-diameter air-cooled monofilament of the present invention;
[0038] Figure 2 It is a schematic diagram of the internal structure of a large-diameter air-cooled monofilament preparation device of the present invention;
[0039] In the figure: 1. Heating and melting unit; 2. Spinning die head; 3. Air cooling unit; 4. Control unit; 5. Stretching unit; 6. Shaping unit. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0042] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the scope of protection of the present application. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the invention, unless otherwise specified, "multiple" means two or more.
[0043] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium, and it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood by specific circumstances.
[0044] like Figure 1 As shown, a method for preparing a large-diameter air-cooled monofilament comprises the following steps:
[0045] Step S1, taking a certain amount of matrix material and reinforcement material, wherein the matrix material specifically includes: one or more of TPEE, TPU, PP, and PE, and the reinforcement material includes: one or more of PA6, PA66, PBT, and PET, and slicing the matrix material and the reinforcement material. Specifically, a slicer is used to slice the matrix material and the reinforcement material, and large blocks of matrix material and reinforcement material are refined into smaller particles to obtain matrix particles and reinforcement particles, thereby facilitating uniform mixing and melting of materials in subsequent processing. At the same time, by slicing, the size of the material particles can be ensured to be relatively consistent, thereby improving the uniformity after mixing and reducing the performance difference caused by uneven particle size.
[0046] Step S2, pre-treating the obtained reinforcement particles, mixing the pre-treated reinforcement particles and matrix particles uniformly, and heating the uniformly mixed reinforcement particles and matrix particles to a molten state to obtain a raw material mixture;
[0047] The matrix particles and reinforcement particles are materials of different properties, and the temperatures required for them to be in a molten state are different. The uniformly mixed reinforcement particles and matrix particles are heated to a molten state. Specifically, they are heated at 220-290°C for 6-12 minutes to be in a molten state. After the matrix particles and reinforcement particles are in a molten state, the uniformity of the mixing of the matrix material and the reinforcement material is further improved.
[0048] Step S3, spinning the molten raw material mixture, and extruding it through a spinning head to form a triangular fiber shape, thereby obtaining a fiber with a parallel double-layer structure;
[0049] Specifically, a single-screw extruder is used to spin the molten raw material mixture, wherein the screw speed of the extruder is set at 50-100 rpm to control the fluidity of the molten mixture, the extrusion pressure is set at 80 MPa to ensure the uniformity and continuity of the fiber, the spinning temperature is controlled at 220-290°C to ensure that the material remains in a molten state during the extrusion process, the spinning speed is set to 20 m / min, so that the fiber can enter the air cooling area in time for cooling and shaping after extrusion, and the initial diameter of the extruded fiber is 800 μm, thereby obtaining a fiber with a parallel double-layer structure.
[0050] Step S4, introducing the fiber into the air cooling area, controlling the blowing angle during the air cooling treatment of the fiber, and stretching and collecting the air-cooled fiber to prepare a triangular parallel double-layer structure fiber monofilament.
[0051] In the present invention, the ratio between the matrix material and the reinforcement material is 1-2:2-3.
[0052] In the present invention, in step S2, the reinforcement particles are pretreated, including cleaning, drying, and surface modification;
[0053] Clean the surface of the reinforcement particles to remove impurities such as oil, dust, etc. to ensure that the silane coupling agent can fully contact and act on the material surface to achieve the purpose of uniform mixing of the reinforcement particles and the matrix particles.
[0054] The surface modification of the reinforcement particles is specifically performed by mixing the reinforcement particles with a silane coupling agent at 80-90° C. for 20-30 minutes;
[0055] The silane coupling agent is 97% vinyl triethoxysilane, and the vinyl triethoxysilane is added to an ethanol solution to dilute it to a vinyl triethoxysilane solution with a concentration of 0.8% to 1%, and the vinyl triethoxysilane solution is added to the reinforcement particles, and the mass proportion of the vinyl triethoxysilane solution is 1.5%. The vinyl triethoxysilane solution and the reinforcement particles are heated and stirred in a gradually increasing temperature manner, specifically, heated to 80-90°C and maintained for 20-30 minutes to ensure that the reinforcement particles are evenly coated, thereby reducing the agglomeration tendency of the reinforcement material in the matrix material, so that the reinforcement material exists in the matrix material with a smaller particle size and a more uniform distribution state, and then the obtained reinforcement particles are dried at 100°C for 30 minutes.
[0056] In the present invention, in the step S4, the fibers with the parallel double-layer structure obtained in the step S3 need to be air-cooled. Specifically, the triangular fibers are introduced into the air-cooling area, wherein the temperature of the air-cooling area is controlled between 25-45°C, the humidity is controlled between 30%-60%, and the blowing angle is specifically that the wind direction is at an angle of 30-45° to the fiber axis, and the wind speed is in the range of 10-20m / s, so as to blow evenly on the fiber surface.
[0057] In the present invention, in step S4, the method for stretching and collecting the air-cooled fibers comprises the following steps:
[0058] Step S41, spraying the oil agent evenly on the surface of the fiber after air cooling, and setting the stretched diameter of the fiber;
[0059] Step S42, introducing the fiber into the three-stage stretching and drawing roller, and stretching and drawing the fiber at a temperature between 60 and 200° C. with a drawing multiple of 2 to 5 times, thereby completing the three-stage stretching and drawing;
[0060] Step S43, the fiber that has completed the third-level traction is introduced into the second-level shaping hot roller, and is traction-shaped at 150-240°C with a traction force of 1-2 times the drafting multiple, and the second-level traction shaping is completed and collected into a roll to obtain a triangular parallel double-layer structure fiber monofilament.
[0061] In the present invention, in the step S41, the stretching diameter, specifically, the fiber diameter reaches a threshold value in the range of 0.07-0.20 mm.
[0062] In the present invention, in the step S42, three-stage stretching and drawing is completed, specifically, the fiber is introduced into a traction hot roller with a temperature between 60-100°C, and the fiber is stretched and drawn with a stretching multiple of 2-3 times to complete the first stage of stretching and drawing. The fiber that has completed the second stage of stretching and drawing is introduced into a traction hot roller with a temperature between 100-150°C, and the fiber is stretched and drawn again with a stretching multiple of 3-4 times to complete the second stage of stretching and drawing. The fiber is then introduced into a traction hot roller with a temperature between 150-200°C, and the fiber is stretched and drawn with a stretching multiple of 4-5 times to complete the third stage of stretching and drawing.
[0063] In the present invention, in the step S43, the secondary traction and shaping is completed, specifically, the fiber that has completed the third-stage stretching and traction is introduced into a shaping hot roller with a temperature between 150-200°C, and the fiber is stretched and shaped using a shaping drafting multiple of 1-1.5 times to complete the first-stage traction and shaping, and then the fiber is introduced into a shaping hot roller with a temperature between 200-240°C, and the fiber is stretched and shaped using a shaping drafting multiple of 1.5-2 times to complete the second-stage traction and shaping.
[0064] The properties of the matrix material and the reinforcement material are different, and their respective densities are different. During the cooling process of the mixed prepared monofilament, internal stress is generated due to the different shrinkage rates of the materials, which affects the performance of the monofilament.
[0065] The following experiment was conducted to investigate the different ratios between the matrix material and the reinforcement material, resulting in different internal stresses caused by shrinkage of the prepared monofilaments.
[0066] Experimental example:
[0067] (I) Detection method
[0068] 1. Tensile strength test: Use a universal material testing machine to fix the monofilament on the universal material testing machine, stretch the sample until it breaks, record the maximum load and the original cross-sectional area of the sample, and then calculate the tensile strength according to the formula: tensile strength = maximum load / original cross-sectional area.
[0069] 2. Elongation at break test: Use a universal material testing machine to fix the monofilament on the universal material testing machine, stretch it until it breaks, record the original length and the length after breaking of the sample, and then calculate the elongation at break according to the formula: elongation at break = (length after breaking - original length) / original length.
[0070] 3. Shrinkage rate detection: Take a single filament with a length of 100 mm, put it into an oven, and heat it at 200°C for 10 minutes. By comparing the original length and the length after heating, the shrinkage rate is obtained, specifically: Shrinkage rate = [(length after heating-original length) / original length] × 100%.
[0071] (II) Implementation methods
[0072] A. Take PP material and PA6 material, and divide the PP material and PA6 material into eight groups, wherein the ratios between PP material and PA6 material in groups one to eight are 1:3, 1:2.5, 1:2, 1.5:2.5, 2:3, 1.5:2, 2:2.5, and 1:1 respectively;
[0073] B. Slice the PP material and PA6 material using a slicer, and refine the large pieces of PP material and PA6 material into smaller particles. Mix the PA6 material with a 0.8% concentration of vinyl triethoxysilane solution, and the mass proportion of the vinyl triethoxysilane solution is 1.5%. Heat at 85°C for 20 minutes, then heat to 100°C, and stir and dry for 30 minutes.
[0074] C. The PA6 material and the PP material pretreated in step B are mixed and heated at 245° C. for 10 minutes until they are in a molten state to obtain a raw material mixture, and the molten raw material mixture is spun to form a triangular fiber shape through a spinning head to obtain a fiber with a parallel double-layer structure;
[0075] D. During the fiber preparation process, the triangular fibers are introduced into the air cooling area for air cooling treatment, wherein the temperature of the air cooling area is controlled between 25-45°C, the humidity is controlled between 30%-60%, the wind direction of several air outlets is at an angle of 30-45° to the fiber axis, the wind speed is within the range of 10-20m / s, and the fiber surface is blown evenly until the temperature of the fiber is between 25-45°C;
[0076] E. The air-cooled monofilament is introduced into the three-stage stretching and drawing roller, and is drawn into the drawing hot roller at a temperature of 80°C, and the fiber is stretched and drawn using a 2-fold stretching multiple to complete the first stage of stretching and drawing. The fiber that has completed the second stage of stretching and drawing is introduced into the drawing hot roller at a temperature of 120°C, and the fiber is stretched and drawn again using a 3-fold stretching multiple to complete the second stage of stretching and drawing. The fiber is then introduced into the drawing hot roller at a temperature of 180°C, and the fiber is stretched and drawn using a 5-fold stretching multiple to complete the third stage of stretching and drawing.
[0077] F. The fiber that has completed the third-stage stretching and drawing is introduced into a shaping hot roller with a temperature of 180°C, and the fiber is stretched and shaped using a shaping drafting multiple of 1.5 times to complete the first-stage traction and shaping. The fiber is then introduced into a shaping hot roller with a temperature of 220°C, and the fiber is stretched and shaped using a shaping drafting multiple of 2 times to complete the second-stage traction and shaping. After the second-stage traction and shaping is completed and collected into a roll, eight groups of triangular-like parallel double-layer structure fiber monofilaments are obtained.
[0078] The detection method was tested on the triangular parallel double-layer structure fiber monofilaments obtained from the above eight groups of PP materials and PA6 materials in different proportions, as shown in Table 1;
[0079] Table 1:
[0080]
[0081]
[0082] In summary, with the increase of PP material content, the tensile strength and elongation at break of the monofilament also increase, making the monofilament have good ductility. This is mainly because, in the process of uniformly mixing PP material and PA6 material to prepare the monofilament, the high crystalline region of PP will be more embedded in the matrix of PA6. With the increase of PP material content, the number of crystalline regions in the raw material mixture increases, providing more physical cross-linking points. At the same time, the amorphous region between the crystalline regions absorbs and buffers external forces, so that the monofilament can better disperse stress during the stretching process, so that the monofilament exhibits higher strength and toughness during stretching. The crystalline region increases the mutual connection and cross-linking points between the molecular chains of the material, making the overall molecular structure of the material more compact and orderly, and the formation of the crystalline region reduces the gaps and free space between the molecular chains of the material, avoiding the free movement and relaxation of the molecular chains, thereby reducing the dimensional change of the material during the cooling process. At the same time, the molecular chains in the crystalline region are interconnected by strong intermolecular forces, so that the material can be evenly transmitted and dispersed under the action of external forces without causing excessive stress concentration in local areas.
[0083] However, as the content of PP material continues to increase and the proportion of PP material is too large, the number of crystalline regions will be too large, the number of amorphous regions will be reduced, and the structure inside the monofilament will become more complex and dense, unable to effectively absorb and disperse external forces, causing the material to become too rigid and brittle. Excessive crystalline regions will lead to uneven internal structure of the material, that is, when the shrinkage rate of different parts of the monofilament changes due to the unevenness of the material structure, the excessive crystalline region will hinder the release and dispersion of the internal stress of the material, resulting in uneven deformation, unable to effectively disperse the generated stress, and thus become the core of stress concentration, resulting in increased local shrinkage and deformation rate of the material. At the same time, the heat conduction path inside the crystalline region is shorter and the cooling rate is faster, which further leads to uneven shrinkage of the monofilament, thereby increasing the internal stress of the monofilament; in summary, the ratio between PP material and PA6 material is 1.5:2, and the monofilament obtained is the optimal solution.
[0084] The matrix materials mentioned above specifically include: one or more of TPEE, TPU, PP, and PE, and the reinforcement materials include: one or more of PA6, PA66, PBT, and PET. The method of the above-mentioned experimental example 1 can be used to perform performance testing on the prepared monofilament.
[0085] In the air cooling process, the wind direction of the air outlet is at different angles to the fiber axis, which will affect the cooling efficiency of the monofilament.
[0086] Example 1 is generally the same as the implementation method in the above-mentioned experimental example, except that PP material and PA6 material with a mass ratio of 1.5:2 are used to prepare triangular fibers, and in the air-cooling treatment, the temperature of the air-cooling area is controlled between 30-45°C, the humidity is controlled at 45%, the wind direction of several air outlets is at an angle of 30° to the fiber axis, the wind speed is 20m / s, and the fiber surface is blown evenly. An infrared temperature sensor is used to detect the temperature of the fiber in real time until the temperature of the fiber drops to 40°C, and the time taken is recorded.
[0087] Embodiment 2 is substantially the same as Embodiment 1, except that the wind direction of the plurality of air outlets is at an angle of 35° to the fiber axis, and an infrared temperature sensor is used to detect the fiber temperature in real time until the fiber temperature drops to 40°C, and the time taken is recorded.
[0088] Embodiment 3 is substantially the same as Embodiment 1, except that the wind direction of the plurality of air outlets is at an angle of 40° to the fiber axis, and an infrared temperature sensor is used to detect the fiber temperature in real time until the fiber temperature drops to 40°C, and the time taken is recorded.
[0089] Embodiment 4 is substantially the same as Embodiment 1, except that the wind direction of the plurality of air outlets is at an angle of 45° to the fiber axis, and an infrared temperature sensor is used to detect the fiber temperature in real time until the fiber temperature drops to 40°C, and the time taken is recorded.
[0090] Comparative Example 1: Take PP material and PA6 material with a mass ratio of 1.5:2, slice the PP material and PA6 material with a slicer, refine the large pieces of PP material and PA6 material into smaller particles, and use 0.8% concentration of vinyl triethoxysilane solution to mix with PA6 material for pretreatment, and the mass proportion of vinyl triethoxysilane solution is 1.5%, heat at 85°C for 20 minutes, then heat to 100°C, and stir and dry for 30 minutes;
[0091] The PA6 material pretreated in step B and the PP material are mixed and heated at 245° C. for 10 minutes until they are in a molten state to obtain a raw material mixture, and the molten raw material mixture is spun and extruded into a circular fiber shape to obtain a fiber with a parallel double-layer structure;
[0092] The circular fiber is introduced into a wind-cooled area with a temperature between 30-45°C and the humidity is controlled at 45%. The wind direction of several air outlets is at a 40° angle to the fiber axis and the wind speed is 20m / s. The fiber surface is blown evenly. An infrared temperature sensor is used to detect the fiber temperature in real time until the fiber temperature drops to 40°C and the time taken is recorded.
[0093] Comparative Example 2 is substantially the same as Comparative Example 1, except that the wind directions of the several air outlets are aligned with the fiber axis, and an infrared temperature sensor is used to detect the temperature of the fiber in real time until the temperature of the fiber drops to 40° C., and the time taken is recorded.
[0094] For the above examples and comparative examples, the following data are obtained, as shown in Table 2;
[0095]
[0096] In summary, the above cooling rate = (initial temperature - predetermined cooling temperature) / cooling time, and cooling uniformity indicates whether the temperature change of the fiber is consistent across the entire surface and inside;
[0097] By comparing the first to fourth embodiments, when the angle between the wind direction of the blowing ports and the fiber axis increases, the heat dissipation efficiency of the triangular-shaped fibers is significantly improved. This is mainly because, as the blowing angle increases, the airflow is no longer directly aligned with the fiber axis, but contacts the fiber at a certain angle, so that the airflow can bypass various parts of the fiber, including the corners and the back, thereby achieving full coverage of the fiber surface, ensuring that the cooling rates of the corner areas and the center area tend to be consistent, reducing the phenomenon of local overheating or overcooling, and thus improving the overall cooling uniformity and efficiency;
[0098] At the same time, the airflow will form eddies and turbulence on the fiber surface, which can destroy the static air layer (boundary layer) near the fiber surface, enhance the convective heat transfer efficiency between the air and the fiber surface, improve the cooling uniformity, and reduce thermal stress and deformation;
[0099] However, if the angle between the wind direction of the air outlet and the fiber axis is too large, the heat dissipation efficiency of the triangular fiber will be reduced. This is because when the blowing angle is too large, the airflow may miss the front of the fiber and focus on the side or back of the fiber. The contact area between the airflow and the fiber surface will be reduced, resulting in reduced cooling efficiency.
[0100] By comparing Example 3, Comparative Example 1, and Comparative Example 2, under the same conditions, the cooling efficiency of the triangular-shaped fibers is significantly higher than that of the circular-shaped fibers, because the triangular-shaped fibers have a larger surface area than the circular-shaped fibers, which means that more fiber surfaces are exposed to the cooling medium (such as air), which can more effectively exchange and conduct heat, and the shape of the triangular-shaped fibers can cause instability and disturbance of the boundary layer, and the airflow blowing on the surface of the triangular-shaped fibers will have eddies and turbulence, which helps to enhance the heat transfer between the airflow and the fiber surface, thereby improving the cooling efficiency; in summary, Example 3 is the optimal solution of the present invention.
[0101] like Figure 2 As shown, a large-diameter air-cooled monofilament preparation device comprises: a heating and melting unit 1, a spinning die 2, an air-cooling unit 3, a stretching unit 5 and a shaping unit 6, and a control unit 4;
[0102] The heating and melting unit 1, specifically a single-screw extruder, is used to mix the matrix particles and the reinforcement particles uniformly and heat them to a molten state. The spinning die 2 is installed at the extrusion port of the heating and melting unit 1, and a triangular flow channel is provided in the spinning die 2, so that the prepared fiber has a triangular shape, so as to cooperate with the subsequent rapid air cooling of the fiber;
[0103] The screw speed of the extruder is set at 50-100 rpm to control the fluidity of the molten mixture, the extrusion pressure is set at 80 MPa to ensure the uniformity and continuity of the fiber, the spinning temperature is controlled at 220-290°C to ensure that the material remains in a molten state during the extrusion process, and the spinning speed is set to 20 m / min so that the fiber can enter the air cooling area in time for cooling and shaping after extrusion. The initial diameter of the extruded fiber is 800 microns.
[0104] The air cooling unit 3 is used to quickly cool the spun fibers;
[0105] The stretching unit 5 and the shaping unit 6 are used to perform multi-stage stretching and shaping treatment on the air-cooled fibers. The stretching unit 5 and the shaping unit 6 include: three groups of traction hot rollers; the three groups of traction hot rollers are alternately installed left and right in the vertical falling direction of the monofilaments, and two traction hot rollers are symmetrically arranged in each group;
[0106] Setting unit 6: two sets of setting hot rollers; the two sets of setting hot rollers are located below the traction hot rollers, and the setting hot rollers have the same structure as the traction hot rollers;
[0107] The control unit 4 is used to control the temperature and time of the heating and melting unit 1 for mixing and heating the matrix particles and the reinforcement particles, control the wind speed, blowing time and blowing angle of the air cooling unit 3, and control the stretching parameters of the stretching unit 5 and the shaping unit 6.
[0108] In the production and preparation of monofilaments, the matrix particles and the reinforcement particles are placed in the heating and melting unit 1, heated to a molten state, and mixed evenly. The molten material is extruded through the spinning die 2 into triangular fibers, and then introduced into the air cooling area for rapid air cooling of the fibers. The temperature of the air cooling area is controlled between 25-45°C, and the humidity is controlled between 30% and 60%. The wind direction of several air outlets is at an angle of 30-45° to the fiber axis, and the wind speed is within the range of 10-20m / s. The fiber surface is evenly blown until the temperature of the fiber is between 25-45°C, thereby accelerating the cooling of the fiber.
[0109] The fiber after air cooling is introduced into three groups of traction hot rollers. The temperature of the first group of traction hot rollers is between 80°C. The speed of the first group of traction hot rollers is adjusted. The fiber is stretched and drawn using a 2-fold draft multiple to complete the first-stage stretching and drawing. The fiber that has completed the second-stage stretching and drawing is introduced into the second group of traction hot rollers with a temperature between 120°C. The speed of the second group of traction hot rollers is adjusted. The fiber is stretched and drawn again using a 3-fold draft multiple to complete the second-stage stretching and drawing. The fiber is then introduced into the third group of traction hot rollers with a temperature between 180°C. The speed of the third group of traction hot rollers is adjusted. The fiber is stretched and drawn using a 5-fold draft multiple to complete the third-stage stretching and drawing.
[0110] The fibers that have completed the three-stage stretching and traction will be introduced into the first group of shaping hot rollers at a temperature of 180°C, and stretched and shaped by a shaping drafting multiple of 1.5 times to complete the first stage of traction and shaping. The fibers will then be introduced into the second group of shaping hot rollers at a temperature of 220°C, and stretched and shaped by a shaping drafting multiple of 2 times to complete the second stage of traction and shaping. After the second stage of traction and shaping is completed, the fibers will be collected into rolls to obtain eight groups of triangular parallel double-layer structured fiber monofilaments, which will be wound and collected.
[0111] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing large-diameter air-cooled monofilament, characterized in that: The following steps are involved: Step S1, taking a certain amount of matrix material and reinforcement material, slicing the matrix material and reinforcement material to obtain matrix particles and reinforcement particles; Step S2, pre-treating the obtained reinforcement particles, mixing the pre-treated reinforcement particles and matrix particles uniformly, and heating the uniformly mixed reinforcement particles and matrix particles to a molten state to obtain a raw material mixture; Step S3, spinning the molten raw material mixture, and extruding it through a spinning head to form a triangular fiber shape, thereby obtaining a fiber with a parallel double-layer structure; Step S4, introducing the fiber into the air cooling area, controlling the blowing angle during the air cooling treatment of the fiber, and stretching and collecting the air-cooled fiber to prepare a triangular parallel double-layer structure fiber monofilament.
2. The method for preparing a large-diameter air-cooled monofilament according to claim 1, characterized in that: In the step S1, the base material includes: one or more of TPEE, TPU, PP, and PE; The reinforcement material includes: one or more of PA6, PA66, PBT, and PET; The ratio between the matrix material and the reinforcement material is 1-2:2-3.
3. The method for preparing a large-diameter air-cooled monofilament according to claim 1, characterized in that: In the step S2, the uniformly mixed reinforcement particles and matrix particles are heated to a molten state. Specifically, they are heated at 220-290° C. for 6-12 minutes to a molten state.
4. The method for preparing a large-diameter air-cooled monofilament according to claim 1, characterized in that: In the step S2, the reinforcement particles are pretreated, including cleaning, drying, and surface modification; The surface modification of the reinforcement particles is specifically carried out by mixing the reinforcement particles with a silane coupling agent at 80-90° C. for 20-30 minutes.
5. A method for preparing a large-diameter air-cooled monofilament according to claim 1, characterized in that: In step S4, the fiber is subjected to air cooling treatment, specifically, the triangular-shaped fiber is introduced into the air cooling area, wherein the temperature of the air cooling area is controlled between 25-45°C, the humidity is controlled between 30%-60%, and the blowing angle is specifically that the wind direction is at an angle of 30-45° to the fiber axis, and the wind speed is in the range of 10-20m / s, so as to blow evenly on the fiber surface.
6. The method for preparing a large-diameter air-cooled monofilament according to claim 1, characterized in that: In step S4, the method for stretching and collecting the air-cooled fibers comprises the following steps: Step S41, spraying the oil agent evenly on the surface of the fiber after air cooling, and setting the stretched diameter of the fiber; Step S42, introducing the fiber into the three-stage stretching and drawing roller, and stretching and drawing the fiber at a temperature between 60 and 200° C. with a drawing multiple of 2 to 5 times, thereby completing the three-stage stretching and drawing; Step S43, the fiber that has completed the third-level traction is introduced into the second-level shaping hot roller, and is traction-shaped at 150-240°C with a traction force of 1-2 times the drafting multiple, and the second-level traction shaping is completed and collected into a roll to obtain a triangular parallel double-layer structure fiber monofilament.
7. The method for preparing a large-diameter air-cooled monofilament according to claim 6, characterized in that: In the step S41, the stretching diameter, specifically, the fiber diameter reaches a threshold value in the range of 0.07-0.20 mm.
8. The method for preparing a large-diameter air-cooled monofilament according to claim 6, characterized in that: In the step S42, the third-level stretching and drawing is completed, specifically, the fiber is introduced into a traction hot roller with a temperature between 60-100°C, and the fiber is stretched and drawn with a stretching multiple of 2-3 times to complete the first-level stretching and drawing. The fiber that has completed the second-level stretching and drawing is introduced into a traction hot roller with a temperature between 100-150°C, and the fiber is stretched and drawn again with a stretching multiple of 3-4 times to complete the second-level stretching and drawing. The fiber is then introduced into a traction hot roller with a temperature between 150-200°C, and the fiber is stretched and drawn with a stretching multiple of 4-5 times to complete the third-level stretching and drawing.
9. The method for preparing a large-diameter air-cooled monofilament according to claim 6, characterized in that: In the step S43, the secondary traction and shaping is completed, specifically, the fiber that has completed the third-stage stretching and traction is introduced into a shaping hot roller with a temperature between 150-200°C, and the fiber is stretched and shaped using a shaping drafting multiple of 1-1.5 times to complete the first-stage traction and shaping, and then the fiber is introduced into a shaping hot roller with a temperature between 200-240°C, and the fiber is stretched and shaped using a shaping drafting multiple of 1.5-2 times to complete the second-stage traction and shaping.
10. A device for preparing large-diameter air-cooled monofilaments, based on a method for preparing large-diameter air-cooled monofilaments according to any one of claims 1 to 9, comprising: Heating and melting unit, spinning die head, air cooling unit, stretching unit and shaping unit, control unit; The heating and melting unit is used to mix the matrix particles and the reinforcement particles uniformly and heat them to a molten state. The spinning die is installed at the extrusion outlet of the heating and melting unit, and a triangular flow channel is opened in the spinning die; The air cooling unit is used to quickly air cool the spun fibers; The stretching unit and the shaping unit are used to perform multi-stage stretching and shaping treatment on the air-cooled fibers, and the stretching unit and the shaping unit include: three groups of traction hot rollers; the three groups of traction hot rollers are alternately installed left and right in the vertical falling direction of the monofilaments, and two traction hot rollers are symmetrically arranged in each group; The shaping unit comprises two sets of shaping hot rollers; the two sets of shaping hot rollers are located below the traction hot rollers, and the shaping hot rollers have the same structure as the traction hot rollers; The control unit is used to control the temperature and time of the heating and melting unit for mixing and heating the matrix particles and the reinforcement particles, control the wind speed, blowing time and blowing angle of the air cooling unit, and control the stretching parameters of the stretching unit and the shaping unit.
Citation Information
Patent Citations
Method for preparing super-thick denier polyester monofilament
CN101831718A
Method and apparatus for air cooling in spinning coarse denier fibers
CN102296372A
Large-diameter polymer bulked monofilament and production method thereof
CN104213239A
Special-shaped spinneret plate and method for producing square-section colored FDY through special-shaped spinneret plate
CN104451922A
Nano-modified large-diameter copolymerized polyamide monofilament and production method thereof
CN105256395A