Gold nano-disc dimer, ultra-small-mode-volume plasmon nano-cavity and preparation method and application of gold nano-disc dimer and ultra-small-mode-volume plasmon nano-cavity
Using cucurbituril molecule-assisted assembly technology, an ultra-small-module volume gold nanodisk dimer plasmon cavity is formed, which solves the problem of insufficient photon-radion coupling strength of the plasmon cavity at room temperature and achieves a high degree of Localized light field and electric field enhancement are suitable for the construction and application of quantum optical devices.
Patent Information
- Application Number
- CN202411167450.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-10-15
AI Technical Summary
The photon-radion coupling strength of existing plasmon nanocavities cannot overcome system attenuation at room temperature, and quantum state manipulation and coherence are poor, which limits the construction and application of quantum optical devices.
Cucurbituril molecule-assisted assembly technology is used to assemble gold nanodisks side by side into gold nanodisk dimers, forming an ultra-small mode volume plasmon nanocavity. By precisely controlling the length and gap width of the nanocavity, the light field can be controlled. High localization and enhancement of electric fields.
An ultra-small mode volume plasmon nanocavity of sub-20 nm3 has been realized. The maximum electric field enhancement reaches |E/E0| = 600. It is suitable for fields such as nanolasers, quantum light sources, and single-molecule Raman detection, and has huge applications. potential, especially to achieve single-photon level quantum state manipulation and strong light-matter coupling at room temperature.
Smart Images

Figure CN118778158A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanophotonics, and in particular to a gold nanodisc dimer, an ultra-small mode volume plasmon nanocavity, and a preparation method and application thereof. Background Art
[0002] The precise construction and control of new light fields is not only the core content of the physics and application of light field control, but also an important foundation for the study of light-matter interactions. Its research content is of great significance and value both from the basic theoretical point of view of nanophotonics and quantum optics and from the perspective of the development of quantum optoelectronic devices. At present, relevant research results have been widely used in many research fields such as quantum computing, quantum networks, quantum information processing, and highly sensitive quantum sensing. Therefore, in recent years, the construction and control of new light fields has gradually developed into a frontier field internationally.
[0003] Optical micro-nanostructures can achieve highly localized light field control at the micro / nano scale, providing an ideal research platform for light-matter interaction research. Therefore, the construction and control of light fields based on optical micro-nanostructures is a current research hotspot. We know that according to the strength of the interaction, light-matter interaction research can be divided into weak coupling research and strong coupling research. In the weak coupling research, people use optical micro-nanostructures to tailor the localized state density of photons around quantum radiators to achieve efficient control of their spontaneous radiation, thereby laying the foundation for the development of quantum optical devices such as on-chip high-brightness single-photon sources and low-threshold nanolasers at the micro-nano scale. At present, this type of weak coupling interaction research has made many breakthroughs and important research results, providing theoretical and technical accumulation for the development and application of quantum devices and quantum chips. In strong coupling, the quantum system is strongly coupled with the light field, and ultrafast and reversible coherent energy exchange occurs between the two subsystems. The energy exchange rate is much faster than the decay rate of the system. From the frequency domain, it manifests as mode hybridization and vacuum Rabi splitting of photons and quantum radiators. This strong coupling can greatly suppress the quantum decoherence effect of the system and maintain the coherence state of the system to the maximum extent, making it an important prerequisite and foundation for quantum information processing such as quantum computing, quantum communication, and quantum networks.
[0004] At present, there are two main types of micro-nano systems used for the preparation and precise control of new light fields. One is the traditional cavity-quantum electrodynamics (cavity-QED) system, which uses various solid-state optical media / semiconductor microcavities to control the light field and its interaction with the quantum system. The advantages of this type of system are stable structure and low photon loss, which is very conducive to the control of light-matter coherent coupling; the disadvantage is that the localization ability of this type of system on the light field cannot break through the optical diffraction limit, and it usually needs to be carried out under low temperature and high vacuum conditions, which seriously limits its practical application. Therefore, in recent years, plasmon metal nanoresonator (plasmon nanocavity) system has gradually developed into another important platform for the study of light-matter strong coupling and quantum state control. This type of system has many advantages such as photon localization ability that can break through the optical diffraction limit, ultrafast response speed, wide bandwidth and room temperature control. It is very suitable for the control of photon-radion room temperature strong coupling and the miniaturization and high integration of quantum optical devices based on this, which has great application potential in the fields of room temperature quantum information processing and has aroused people's strong research interest.
[0005] However, due to the huge loss of plasmon resonance at room temperature and the small transition dipole moment of a single radiator, the photon-radiator coupling strength is difficult to overcome the attenuation of the system, and the quantum decoherence effect of the coupled system is significant, which is not conducive to the manipulation of quantum states and the construction of corresponding quantum optical devices. An effective way to increase the coupling strength and overcome the attenuation of the system is to further compress the light field, reduce the light field mode volume and thus increase the local state density of photons. At present, the minimum light field mode volume that can be achieved experimentally using plasmon nanocavities is the 2016 report by Professor JJ Baumberg's research group at the University of Cambridge in the journal Nature ( Nature 2016 , 535, 127–130.) The NPoM structure reported in 3 Ultra-small mold volume. Summary of the invention
[0006] In view of the technical problems existing in the prior art, the present invention proposes a gold nanodisc dimer, an ultra-small mode volume plasmon nanocavity, and a preparation method and application thereof, wherein the gold nanodiscs whose upper and lower surfaces are protected by CTAB are assembled side by side into a gold nanodisc dimer by using cucurbituril molecule-assisted active assembly technology, and the gap width thereof is equal to the thickness of the cucurbituril ring molecule (about 0.9 nm), thereby achieving sub-nanometer precise control of the length of the plasmon nanocavity; In order to achieve the above object, the technical solution of the present invention is achieved as follows: A gold nanodisc dimer is a side-by-side dimer assembled with the assistance of cucurbituril molecules. There is a gap between two gold nanodiscs in the dimer, the gap is 0.63-1.04 nm, and the preferred gap is 0.9 nm.
[0007] The gold nanodisc has a diameter of 30-60 nm and a thickness of 5-9 nm. The cucurbituril molecule is cucurbit[5]uril, cucurbit[6]uril, cucurbit[7]uril or cucurbit[8]uril.
[0008] An ultra-small mode volume gold nanodisk dimer plasmon nanocavity comprises the gold nanodisk dimer and an absorption substrate placed on the lower surface of the dimer, wherein the absorption substrate is SiO2 or SiO2 / Si.
[0009] The plasmon nanocavity "focuses" the light field localized in the dimer gap toward the substrate surface; forming a nanocavity smaller than 20 nm 3 Ultra-small mode volume; the mode area (the area of the light field on the substrate surface) is about 2-5 nm 2 .
[0010] The method for preparing the gold nanodisc dimer comprises the following steps: (1) Mixing the CTAB solution of gold nanotriangular prisms and the HAuCl4 solution and allowing to stand for reaction I, and then centrifuging and adding water to disperse to obtain a gold nanodisc aqueous solution; (2) The cucurbituril solution and the gold nanodisc aqueous solution are mixed evenly and allowed to stand for reaction II to obtain dimers of gold nanodiscs assembled side by side.
[0011] In the step (1), the side length of the gold nanotriangular prism is 100-180 nm, and the concentration of the gold nanotriangular prism in the CTAB solution of the gold nanotriangular prism is (1.5-2.0)×10 -10 mol / L, the concentration of CTAB is 0.03-0.07 mol / L; the concentration of HAuCl4 solution is 0.005-0.03 mol / L, and the volume ratio of CTAB solution and HAuCl4 solution of gold nanotriangular prisms is 22-28:1.
[0012] In the step (1), the gold nano-triangular pillars are purified; the temperature of the static reaction is 25-30° C., and the time is 4-5 hours.
[0013] The concentration of the cucurbituril solution in step (2) is (0.5-2)×10 -7 mol / L; the concentration of the gold nanodisc aqueous solution is (1.71-6.84)×10 -10mol / L (calculated based on the side length of the gold triangle piece of 110nm); the diameter of the gold nanodisc is 30-60nm; the volume ratio of cucurbituril solution to gold nanodisc solution is 30-50 μL: 1-2mL.
[0014] In the step (2), the temperature of the standing reaction II is 20-30° C. and the time is 3-5 hours.
[0015] The method for preparing the ultra-small mode volume gold nanodisc dimer plasmon nanocavity comprises the following steps: dropping a gold nanodisc dimer solution on an absorbing substrate and allowing it to stand, then removing the droplets, rinsing and drying, to obtain the ultra-small mode volume plasmon nanocavity.
[0016] The substrate is SiO2 or SiO2 / Si; the static treatment time is 5 minutes; the rinsing treatment adopts deionized water rinsing, and the drying treatment adopts nitrogen blowing.
[0017] The present invention has the following beneficial effects: (1) In the present invention, cucurbituril molecule-assisted active assembly technology is used to assemble the upper and lower surfaces of CTAB-protected gold nanodisks side by side into gold nanodisk dimers, and the dimers are placed on a substrate to form a plasmon nanocavity. The method is simple and easy to operate.
[0018] (2) The gold nanodisc dimer plasmon nanocavity prepared in the present invention has the smallest mode volume reported so far (sub 20 nm 3 ), and its plasmon resonance mode can be precisely controlled by controlling the diameter of the gold nanodisk. When it is placed on an absorbing medium substrate (such as SiO2, SiO2 / Si), its light field can be further localized to the substrate surface. Its mode area is further compressed to about 3 nm 2 , which can make the light field highly localized. At this time, the maximum value of the electric field enhancement within the mode area can reach | E / E 0| = 600, which is the maximum value that can be achieved experimentally so far.
[0019] (3) Such a strong electric field enhancement capability makes the plasmon nanocavity structure have great application potential in the fields of light-matter weak coupling research such as nanolasers, quantum light sources, single-molecule Raman detection, and enhanced high-order harmonics. In particular, if a single-layer two-dimensional transition metal sulfide exciton material is grown on a SiO2 / Si substrate, and then the prepared gold nanodisk dimer plasmon nanocavity is placed on the single-layer two-dimensional exciton material, a plasmon-single exciton coupling system can be formed.
[0020] (4) In the present invention, the electric field of the plasmon will be highly localized on the surface of the two-dimensional exciton material. At this time, the ultra-small mode area of the plasmon nanocavity can only accommodate one in-plane exciton to couple with the electric field, and the direction of the electric field is also the in-plane electric field, which can be well matched with the exciton transition dipole moment. In this case, it is very likely to realize the strong coupling between plasmons and single exciton radiators based on two-dimensional transition metal sulfides (Note: At present, the minimum number of excitons for the strong coupling between plasmons and excitons at room temperature achieved by two-dimensional transition metal sulfides internationally is about 7, which has not yet reached the single level, Nano Lett.2024, 1579–1586. Nano Lett.2022, 22, 2177−2186).
[0021] (5) The present invention has sub-20 nm 3 The ultra-small mode volume gold nanodisk dimer plasmon nanocavity provides an ideal platform for preparing and manipulating quantum states at room temperature and single-photon level. At the same time, this invention will also provide an ideal research platform for the study of weak light-matter coupling such as plasmon nanolasers, high-brightness single-photon sources, single-molecule enhanced spectroscopy, and enhanced high-order harmonics.
[0022] (6) The gap plasmon mode of the nanocavity in the present invention is an in-plane resonance mode, which can be well matched with the in-plane single exciton transition in the two-dimensional exciton material, which is conducive to the coupling of the two and is also suitable for integrating the two to prepare optical quantum devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 TEM image of high-purity gold nanotriangular prisms used in the embodiments of the present invention.
[0025] Figure 2 The figure is a schematic diagram of the process of preparing gold nanodisc dimers according to the present invention.
[0026] Figure 3 The normalized UV-visible absorption spectra and corresponding TEM images of the gold nanodisks with different sizes prepared in the examples of the present invention are shown.
[0027] Figure 4 TEM images of gold nanodisc dimer plasmon nanocavities with different diameters prepared in the embodiments of the present invention.
[0028] Figure 5 This is the electric field distribution diagram of different cross sections of the gold nanodisk dimer plasmon nanocavity (placed on a SiO2 substrate) in Example 1 of the present invention (FDTD simulation results).
[0029] Figure 6 The scattering spectra (FDTD calculation results) of the dimer (spacing 0.9 nm) composed of the gold nanodisks of Example 1 (40 nm), Example 3 (30 nm), and Example 4 (50 nm) on the SiO2 substrate.
[0030] Figure 7 The mode volume of the gold nanodisk dimer plasmon nanocavity (placed on a SiO2 substrate) with a disk diameter of 40 nm and a spacing of 0.9 nm in Example 2 ( V m ) changes with wavelength; the purple arrow shows the resonant wavelength position of the plasmon nanocavity.
[0031] Figure 8 Schematic diagram of the room-temperature strong coupling between the gold nanodisc dimer nanocavity and a single in-plane exciton in the two-dimensional transition metal sulfide exciton material in Application Example 1. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The gold nano triangular prisms in the present invention are commercially available products, or are prepared by the method of patent CN 104625086 A, or by the following method, the main steps of which are as follows: Preparation of high-purity gold nanotriangular prisms Before the experiment, all glassware was cleaned with aqua regia (hydrochloric acid and nitric acid volume ratio 3:1) and then rinsed with deionized water several times.
[0034] (1) Synthetic Gold Seed Add 1 mL (0.01 mol / L) of sodium citrate to 36 mL of deionized water, quickly add 1 mL of HAuCl4 (0.01 mol / L), and then inject 1 mL (0.1 mol / L) of freshly prepared frozen NaBH4. Stir evenly for 5 minutes to obtain a seed solution. Store it in a 25°C water bath for two hours before use.
[0035] (2) Preparation of growth medium 75 μL (0.1 mol / L) KI was added to 150 mL (0.05 mol / L) CTAB solution, stirred rapidly and ultrasonicated for 30 s, and then divided into five parts, namely A, B, C, D and E. The first two solutions (A and B) were the same, containing CTAB (0.05 mol / L, 9.0 mL), NaOH (0.1 mol / L, 0.05 mL), HAuCl4 (0.01 mol / L, 0.25 mL) and ascorbic acid (0.1 mol / L, 0.05 mL), respectively. The other solutions C, D and E were the same, containing CTAB (0.05 mol / L, 45 mL), NaOH (0.1 mol / L, 0.25 mL), HAuCl4 (0.01 mol / L, 1.25 mL) and ascorbic acid (0.1 mol / L, 0.25 mL). Note that all five sets of solutions were prepared by adding chemicals in the order listed above. 1 mL of seed solution was added to solution A and gently shaken to start the growth of gold nanotriangular pillars. Then 5 mL of growth solution A was quickly added to B, and then 2, 3, and 4 mL of solution B were added to solutions C, D, and E, respectively, with gentle shaking. After addition, the colors of C, D, and E changed from transparent to dark purple within 30 minutes, and were purified after standing in a 25°C water bath for 2 hours. Finally, three gold nanotriangular pillar samples were obtained, with extinction maxima at approximately 1210, 1100, and 985 nm. Gold nanopillars were prepared based on the preparation of gold nanoparticles.
[0036] (3) Purification of gold nanotriangular columns A purification method based on the difference in surface area of metal nanoparticles can be used to separate uniform nanostructures from a mixture of nanoparticles of almost equal mass and volume. Spherical gold nanoparticles can be removed from a gold nanotriangular prism solution, and this method can be used to obtain high-purity gold nanotriangular prisms ( Figure 1 ) triangular prisms with side lengths of 100-180 nm. The specific operation is: add 45 mL of a mixture of gold nanotriangular prisms (containing gold nanosphere impurities) and CTAB (0.05 mol / L) solution into a clean beaker, add (4.0 mol / L, 1.2 mL) of NaCl solution to the mixture, let it stand for 10 hours again, and then gently transfer the supernatant solution to another beaker with a syringe. The gold nanotriangular prisms with a larger surface area first adhere to the bottom of the beaker, and the precipitate is quickly dispersed into the (0.05 mol / L, 10 mL) CTAB solution for protection, and a uniformly dispersed high-purity gold nanotriangular prism solution can be obtained for subsequent experiments.
[0037] Example 1 This embodiment provides a method for preparing a gold nanodisc dimer, comprising the following steps: (1) Using Au 3+ Fabrication of ultra-smooth gold nanodisks by ion oxidation etching of gold nanotriangular prisms First, the required high-purity gold nanotriangular pillars are prepared, and a slow, controllable ratio reaction is used to selectively etch in a self-limiting manner on the surface atoms with the lowest metal coordination number. The reaction occurs selectively at the tip of the gold nanotriangular pillar, rather than on its surface, causing the edge structure to change. Oxidative dissolution occurs selectively at the unsaturated coordination of the nanoparticles and will not significantly affect the rest of the structure. The advantage of this method is that each truncated nanostructure (composed of 0, 1, 2, and 3 truncated angles) synthesized from the gold nanotriangular pillar will be etched into a uniformly sized disk (Figures 2, 3). Using Au in HAuCl4 3+ The Au atoms were etched by oxidation, and the tip of the prepared gold nanotriangular prism was smoothed to obtain a gold nanodisk. The specific operation was as follows: a gold nanotriangular prism (1.75×10 -10 A certain amount of HAuCl4 solution was added to the 2.5 mol / L solution, and the mixture was stirred thoroughly and placed in a 28°C water bath for 4.5 hours. At this time, the extinction value of the gold nanodiscs was about 680 nm. The HAuCl4 concentration was 2.5 mM, and the added volume was about 75 μL.
[0038] The gold nanodisc solution obtained by the above method was washed three times by centrifugation at 7000 rpm / 10 min to terminate the reaction and remove CTAB and excess reagents in the solution, and the precipitate was dispersed in an appropriate amount of deionized water. A small amount of CTAB was still adsorbed on the upper and lower surfaces of the gold nanodisc, and there were very few CTAB molecules adsorbed on the side walls of the two edges due to the curvature effect in the right figure. This can ensure the good dispersion of the gold nanodisc and enable it to be coupled side by side under the action of cucurbituril molecules ( Figure 2 ); (2) Using cucurbituril molecules to couple gold nanodisks side by side into dimer nanocavities: Add a certain amount of CB[7] molecules to a solution of gold nanodiscs (40 nm in diameter and 7 nm in thickness) dispersed in deionized water and let it stand for a while to obtain shoulder-to-shoulder gold nanodisc dimers. After the CB[7] molecules are added to the gold nanoparticles, they can actively bind to the surface of the gold nanodisc particles through the carbonyl group on one side. When another gold nanodisc approaches, the carbonyl group on the other side of the CB[7] molecule cage can grab the side wall of the second gold nanodisc, forming shoulder-to-shoulder gold nanodisc dimers with the strongest electric field distribution in the gap between the nanodimers. The concentration of CB[7] added in the above preparation is 10- 7 mol / L, the concentration of the gold nanodisc aqueous solution is 3.04×10 -10 mol / L; the volume of cucurbit[7]uril solution is 50μL; the volume of gold nanodisc solution is 2mL; after the cucurbit[7]uril molecules are added and left to stand at 25℃ for about 4h, the gold nanodisc dimer can be successfully prepared.
[0039] Example 2 A method for preparing an ultra-small mode volume gold nanodisc dimer plasmon nanocavity comprises the following steps: Take 5-10 μL of the gold nanodisc dimer solution prepared in Example 1 and drop it on the surface of SiO2 or SiO2 / Si substrate. After 5-10 min, remove the small droplet and rinse the substrate surface with deionized water 1-2 times, then blow dry the substrate surface with nitrogen. At this time, the gold nanodisc dimer is attached to the surface of the absorbing substrate. The FDTD simulation calculation results show that at this time, the height is localized in the gap between the gold nanodisc dimers, forming a hot spot.
[0040] Example 3 This embodiment provides a method for preparing an ultra-small mode volume gold nanodisc dimer plasmon nanocavity, comprising the following steps: (1) Using Au in HAuCl4 3+ The Au atoms were etched by oxidation, and the tip of the gold nanotriangular prism with a side length of 100 nm was smoothed to obtain a gold nanodisk. The specific operation was as follows: the gold nanotriangular prism (1.5×10 -10 mol / L) solution, add a certain amount of HAuCl4 solution, stir it thoroughly and let it stand in a 25℃ water bath for 5 hours, where the HAuCl4 concentration is 3.0mM and the added volume is about 80 μL.
[0041] (2) The gold nanodisc solution obtained by the above method was centrifuged at 7000 rpm for 10 min and washed three times to terminate the reaction and remove CTAB and excess reagents in the solution, and the precipitate was dispersed in an appropriate amount of deionized water.
[0042] A certain amount of cucurbitacin[7]uril molecules were added to a solution of gold nanodiscs (30 nm in diameter and 7 nm in thickness) dispersed in deionized water and allowed to stand for a period of time to obtain shoulder-to-shoulder gold nanodisc dimers. The concentration of CB[7] added in the above preparation was 10 -7 mol / L, the concentration of 2mL gold nanodisc aqueous solution is 6.84×10 -10 mol / L; 50 μL cucurbitacin[7]uril aqueous solution (concentration 10 -7mol / L); after the CB[7] molecules were added and left to stand at 25°C for about 4 h, the gold nanodisc dimer was successfully prepared.
[0043] (4) Take 7 μL of the prepared gold nanodisc dimer solution and drop it on the surface of SiO2 or SiO2 / Si substrate. After 8 minutes, remove the small droplet and rinse the substrate surface with deionized water 1-2 times. Then blow the substrate surface dry with nitrogen. At this time, the gold nanodisc dimer is attached to the surface of the absorbing substrate. The FDTD simulation calculation results show that at this time, the light field highly localized in the gap between the gold nanodisc dimers will be "focused" toward the substrate surface.
[0044] Example 4 This embodiment provides a method for preparing an ultra-small mode volume plasmon nanocavity, comprising the following steps: (1) Using Au in HAuCl4 3+ The Au atoms were etched by oxidation, and the tip of the prepared gold nanotriangular prism was smoothed to obtain a gold nanodisk. The specific operation was as follows: the gold nanotriangular prism (2.0×10 -10 mol / L) solution, add a certain amount of HAuCl4 solution, stir it thoroughly and let it stand in a 25℃ water bath for 5 hours, where the HAuCl4 concentration is 2.0 mM and the added volume is about 80 μL.
[0045] (2) The gold nanodisc solution obtained by the above method was centrifuged at 7000 rpm for 10 min and washed three times to terminate the reaction and remove CTAB and excess reagents in the solution, and the precipitate was dispersed in an appropriate amount of deionized water.
[0046] A certain amount of CB[7] molecules was added to a solution of gold nanodiscs (50 nm in diameter and 7 nm in thickness) dispersed in deionized water and allowed to stand for a period of time to obtain shoulder-to-shoulder gold nanodisc dimers. -7 mol / L CB[7] solution, 2mL concentration is 1.7×10 -10 mol / L aqueous solution of gold nanodiscs; after the CB[7] molecules are added and left to stand for about 3 hours, the gold nanodisc dimer can be successfully prepared.
[0047] (3) Take 5-10 μL of the above gold nanodisc dimer solution and drop it on the surface of SiO2 or SiO2 / Si substrate. After 5-10 minutes, remove the small droplet and rinse the substrate surface with deionized water 1-2 times. Then blow the substrate surface dry with nitrogen. At this time, the gold nanodisc dimer is attached to the surface of the absorbing substrate to form a plasmon nanocavity structure. The FDTD simulation calculation results show that at this time, the light field highly localized in the gap of the gold nanodisc dimer plasmon nanocavity will further "focus" toward the substrate surface to form a mode volume less than 20 nm. 3 , mold area is about 3 nm 2 Ultra-high local light field.
[0048] Example 5 This embodiment provides a method for preparing an ultra-small mode volume plasmon nanocavity, comprising the following steps: (1) Using Au in HAuCl4 3+ The Au atoms were etched by oxidation, and the tip of the prepared gold nanotriangular prism was smoothed to obtain a gold nanodisk. The specific operation was as follows: the gold nanotriangular prism (2.0×10 -10 A certain amount of HAuCl4 solution was added to a 2.0 mM (1.2 mol / L) solution, which was stirred thoroughly and placed in a 25°C water bath for 5 hours. The HAuCl4 concentration was 2.0 mM and the added volume was about 67 μL.
[0049] (2) The gold nanodisc solution obtained by the above method was centrifuged at 7000 rpm for 10 min and washed three times to terminate the reaction and remove CTAB and excess reagents in the solution, and the precipitate was dispersed in an appropriate amount of deionized water.
[0050] A certain amount of CB[5] molecules was added to a solution of gold nanodiscs (60 nm in diameter and 5 nm in thickness) dispersed in deionized water and allowed to stand for a period of time to obtain shoulder-to-shoulder gold nanodisc dimers. -7 mol / L CB[5] solution, 2mL concentration is 4.75×10 -10 mol / L aqueous solution of gold nanodiscs; after the CB[5] molecules are added and left to stand at 20°C for about 5 hours, the gold nanodisc dimer can be successfully prepared.
[0051] (3) Take 5-10 μL of the above gold nanodisc dimer solution and drop it on the surface of SiO2 or SiO2 / Si substrate. After 5-10 minutes, remove the small droplet and rinse the substrate surface with deionized water 1-2 times. Then blow the substrate surface dry with nitrogen. At this time, the gold nanodisc dimer is attached to the surface of the absorbing substrate to form a plasmon nanocavity structure. The FDTD simulation calculation results show that at this time, the light field highly localized in the gap of the gold nanodisc dimer plasmon nanocavity will further "focus" toward the substrate surface to form a mode volume less than 20 nm. 3 , mold area is about 2 nm 2 Ultra-high local light field.
[0052] Example 6 This embodiment provides a method for preparing a gold nanodisc dimer, comprising the following steps: (1) Gold nanoparticles (1.75×10 -10 mol / L) solution, add a certain amount of HAuCl4 solution, stir it thoroughly and let it stand in a 28℃ water bath for 4.5 hours, where the HAuCl4 concentration is 2.5 mM and the added volume is about 75 μL.
[0053] The obtained gold nanodisc solution was washed three times by centrifugation at 7000 rpm / 10 min to terminate the reaction and remove CTAB and excess reagents in the solution, and the precipitate was dispersed in an appropriate amount of deionized water; A certain amount of CB[6] molecules was added to a solution of gold nanodiscs (40 nm in diameter and 9 nm in thickness) dispersed in deionized water and allowed to stand for a period of time to obtain shoulder-to-shoulder gold nanodisc dimers. The concentration of CB[6] added in the above preparation was 10 -7 mol / L, the concentration of the gold nanodisc aqueous solution is 3.04×10 -10 mol / L; the volume of cucurbit[6]uril solution is 50μL; the volume of gold nanodisc solution is 2mL; after the cucurbit[6]uril molecules are added and left to stand for about 5h, the gold nanodisc dimer can be successfully prepared.
[0054] Example 7 This embodiment provides a method for preparing a gold nanodisc dimer, comprising the following steps: (1) Gold nanoparticles (1.75×10 -10 mol / L) solution, add a certain amount of HAuCl4 solution, stir it thoroughly and let it stand in a 28℃ water bath for 4.5 hours, where the HAuCl4 concentration is 2.5 mM and the added volume is about 75 μL.
[0055] (2) The obtained gold nanodisc solution was centrifuged and washed three times at 7000 rpm / 10 min to terminate the reaction and remove the CTAB and excess reagents in the solution, and the precipitate was dispersed in an appropriate amount of deionized water; A certain amount of CB[8] molecules was added to a solution of gold nanodiscs (40 nm in diameter and 7 nm in thickness) dispersed in deionized water and allowed to stand for a period of time to obtain shoulder-to-shoulder gold nanodisc dimers. The concentration of CB[8] added in the above preparation was 10 -7 mol / L, the concentration of the gold nanodisc aqueous solution is 3.04×10 -10 mol / L; the volume of cucurbit[8]uril solution is 50μL; the volume of gold nanodisc solution is 2mL; after the cucurbit[8]uril molecules are added and left to stand at 30℃ for about 3h, the gold nanodisc dimer can be successfully prepared.
[0056] Figure 3 UV-Vis absorption spectra (a) and corresponding TEM images (b, c, d) of gold nanodisks of different sizes prepared in the embodiment of the present invention. The diameter of the gold nanodisk is reduced from 60 to 30 nm by etching (black dashed arrow in Figure 3), and the plasmon resonance peak position of the corresponding gold nanodisk gradually decreases from 680 nm to 610 nm.
[0057] like Figure 4 Shown are TEM images of gold nanodisc dimers with different diameters in the present invention.
[0058] The light field in the gap between the gold nanodisc dimers is "focused" toward the substrate surface ( Figure 5 ), by different diameters ( d ) of gold nanodisks (Example 1, spacing 0.9 nm); The resonant scattering spectrum on SiO2 substrate (FDTD calculation results) is shown in Figure 6 As shown, the maximum resonance scattering wavelengths corresponding to the gold nanodisks with diameters of 30 nm, 40 nm, and 50 nm are 680 nm, 760 nm, and 820 nm, respectively.
[0059] The mode volume of the gold nanodisk dimer plasmon nanocavity (placed on a SiO2 substrate) with a disk diameter of 40 nm and a spacing of 0.9 nm in Example 1 is ( V m ) changes with wavelength (as shown in Figure 7). The purple arrow shows the resonant wavelength position of the plasmon nanocavity. 2 Mode area and <20 nm 3 Thus, a sub-20 nm mode volume was prepared. 3Ultrasmall mode volume plasmon nanocavity.
[0060] Application Example 1 A two-dimensional transition metal sulfide (WS2, MoS2, WSe2 or MoSe2) monolayer is grown on a SiO2 or SiO2 / Si substrate, and the gold nanodisc dimer aqueous solution prepared in Example 1 is dripped onto the surface of the two-dimensional transition metal sulfide exciton material. After standing for 5-10 minutes, the liquid droplets are removed, and then gently rinsed with deionized water 1-2 times, and then blown dry in a nitrogen atmosphere. At this time, the prepared gold nanodisc dimer will fall on the surface of the two-dimensional exciton material to form a plasmon nanocavity. Under the excitation of an external light field, the light field localized in the gap of the plasmon nanocavity will further "focus" on the surface of the two-dimensional exciton material, forming a mode area of only about 3 nm 2 The ultra-high localized light field can only accommodate one in-plane exciton in the light field area, and the direction of the plasmon electric field is also in-plane, which can better match the in-plane excitons of the two-dimensional exciton material, realizing the room temperature strong coupling between the plasmon and the in-plane exciton of a single two-dimensional material (such as Figure 8 It provides an ideal platform for the development of quantum optical devices based on single exciton strong coupling at room temperature.
[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A gold nanodisc dimer, Features: The gold nanodisc dimer is a side-by-side dimer assembled with the assistance of cucurbituril molecules. There is a gap between two gold nanodiscs in the dimer, and the gap is 0.63-1.04 nm.
2. The gold nanodisc dimer according to claim 1, Features: The gold nanodisc has a diameter of 30-60 nm and a thickness of 5-9 nm. The cucurbituril molecule is cucurbit[5]uril, cucurbit[6]uril, cucurbit[7]uril or cucurbit[8]uril.
3. The method for preparing the gold nanodisc dimer according to claim 1 or 2, It is characterized in that The steps include: (1) Mix the CTAB solution of gold nanoparticles and HAuCl 4 The solutions were mixed and allowed to stand for reaction I, and then centrifuged and dispersed in water to obtain a gold nanodisc aqueous solution; (2) The cucurbituril solution and the gold nanodisc aqueous solution are mixed evenly and allowed to stand for reaction II to obtain dimers of gold nanodiscs assembled side by side.
4. The method for preparing the gold nanodisc dimer according to claim 3, Features: In the step (1), the side length of the gold nanotriangular prism is 100-180 nm, and the concentration of the gold nanotriangular prism in the CTAB solution of the gold nanotriangular prism is (1.5-2.0)×10 -10 mol / L, the concentration of CTAB is 0.03-0.07 mol / L; HAuCl 4 The concentration of the solution is 2.0-3.0mmol / L, the CTAB solution of gold nanoparticles and HAuCl 4 The volume ratio of the solution is (25-30):
1.
5. The method for preparing the gold nanodisc dimer according to claim 4, Features: In the step (1), the gold nano-triangular pillars are purified; the temperature of the static reaction I is 25-30° C. and the time is 4-5 h.
6. The method for preparing the gold nanodisc dimer according to claim 5, Features: The concentration of the cucurbituril solution in step (2) is (0.5-2)×10 -7 mol / L; the concentration of the gold nanodisc aqueous solution is (1.71-6.84)×10 -10 mol / L; the diameter of the gold nanodisc is 30-60nm; the volume ratio of cucurbituril solution to gold nanodisc solution is 30-50μL:1-2 mL.
7. The method for preparing the gold nanodisc dimer according to claim 6, Features: In the step (2), the temperature of the standing reaction II is 20-30° C. and the time is 3-5 h.
8. An ultra-small mode volume gold nanodisc dimer plasmon nanocavity, Features: The invention comprises the gold nanodisc dimer as claimed in claim 1 or 2 and an absorption substrate placed on the lower surface of the dimer.
9. The ultra-small mode volume gold nanodisc dimer plasmon nanocavity according to claim 3, Features: The absorption substrate is SiO 2 or SiO 2 / Si; the plasmon nanocavity "focuses" the light field localized in the dimer gap toward the substrate surface; forming a nanocavity no larger than 20 nm 3 Mode volume; mode area is localized to 2-5 nm 2 .
10. The method for preparing the ultra-small mode volume gold nanodisc dimer plasmon nanocavity according to claim 8 or 9, Features: The method comprises the following steps: dropping a gold nanodisc dimer solution on an absorbing substrate and allowing it to stand for a static treatment, then removing the droplets, rinsing and drying, and obtaining a monodispersed gold nanodisc dimer ultra-small mode volume plasmon nanocavity.