Positive lithium supplementing material, positive plate and lithium ion secondary battery

By using a transition metal oxide core to coat the surface layer of B element organic lithium salts and triphenylamine derivatives in the positive electrode lithium replenishing material of lithium-ion batteries, the problem of active Li+ consumption and oxidation electrolyte production during the first cycle of lithium-ion batteries is solved. It eliminates gas problems, improves battery efficiency and stability, and extends battery life.

CN118782802APending Publication Date: 2024-10-15ZHUHAI COSMX BATTERY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411101617.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the first cycle of existing lithium-ion batteries, the in-situ electrochemical reduction of lithium salt anions or organic solvents leads to the formation of a solid electrolyte layer, which consumes a large amount of active Li+, resulting in low first Coulombic efficiency and huge capacity loss, and lithium-rich ternary batteries The oxidized electrolyte of the compound produces serious gas, has poor environmental stability, has high residual alkali on the surface, and has the risk of gelation.

Method used

The surface cathode lithium supplement material uses a transition metal oxide core to coat the first organic matter. The organic lithium salt of the B element is combined with oxygen to absorb oxygen, inhibit the oxidation of the oxidized electrolyte, reduce oxygen precipitation, and combine triphenylamine with lone pairs of electrons. Derivatives convert singlet oxygen into triplet oxygen, reducing gas production in the cell and residual alkali on the surface, and improving battery stability.

Benefits of technology

The cathode lithium supplement material with low gas production, low residual alkali and good environmental stability has been realized, which improves the first Coulombic efficiency, energy density and cycle performance of the battery, reduces the cell expansion rate and high-temperature storage gas production, and prolongs the battery life. cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782802A_ABST
    Figure CN118782802A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium batteries, and provides a positive electrode lithium supplementing material, a positive plate and a lithium ion secondary battery. The anode lithium supplementing material comprises an inner core of a transition metal oxide LixMOy and a surface layer coated on the inner core, wherein x is greater than or equal to 2 and less than or equal to 6, y is greater than 0 and less than or equal to 5, and the element M comprises one or more of Mn, Fe, Co, Ni, Mo or Cu; the surface layer comprises a first organic matter, and the first organic matter is an organic lithium salt containing B element. The positive electrode lithium supplementing material comprises the transition metal oxide core and the surface layer coating the first organic matter, and has the advantages of small gas production rate, low residual alkali, good environmental stability and the like, so that the battery containing the positive electrode lithium supplementing material has the advantages of high initial coulombic efficiency, low cell expansion rate, high capacity, high energy density, high cycle performance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a positive electrode lithium supplement material, a positive electrode sheet and a lithium ion secondary battery. Background Art

[0002] Lithium-ion batteries have dominated the market and are widely used in portable electronic products and electric vehicles due to their high energy density, long cycle life, and low self-discharge. However, during the first cycle, due to the in-situ electrochemical reduction of lithium salt anions (such as PF6-) or organic solvents within the operating voltage window, a solid electrolyte layer (SEI) will be produced, which will inevitably consume a large amount of active Li + , resulting in low initial Coulombic efficiency and huge capacity loss. Therefore, it is necessary to develop an economical and effective lithium replenishment method to solve this problem.

[0003] Compared with other lithium replenishment technologies, cathode pre-lithiation technology can directly add cathode lithium replenisher (i.e., positive electrode lithium replenishing material) during the homogenization process of the positive electrode slurry. It does not require additional process improvements and has low cost. It is considered to be a promising technology. It offsets the initial lithium loss by providing additional active lithium before the battery cycle and sacrificing specific pre-lithiation reagents / materials to improve the energy density of lithium-ion batteries. In recent years, lithium-rich ternary compounds have received increasing attention as cathode additives due to their suitable electrochemical window. However, lithium-rich ternary compounds easily oxidize the electrolyte, causing serious gas production in the battery cell; at the same time, lithium-rich ternary compounds also have poor environmental stability and high residual alkali on the surface, resulting in the risk of gelation during the process. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art, and to provide a positive electrode lithium supplement material, a positive electrode sheet comprising the positive electrode lithium supplement material, and a lithium ion secondary battery comprising the positive electrode lithium supplement material or the positive electrode sheet. The positive electrode lithium supplement material of the present invention comprises a transition metal oxide core and a surface layer coated with a first organic matter, and has the advantages of small gas production, low residual alkali, good environmental stability, etc., so that the battery containing the positive electrode lithium supplement material has the advantage of low battery cell expansion rate.

[0005] Furthermore, the battery containing the positive electrode lithium supplement material in the present invention has the advantages of high initial coulombic efficiency, high capacity, high energy density, and high cycle performance.

[0006] In order to achieve the above-mentioned object, the present invention provides a positive electrode lithium supplement material in the first aspect, wherein the positive electrode lithium supplement material comprises a transition metal oxide Li x MO yAn inner core and a surface layer coated on the inner core; wherein 2≤x≤6, 0<y≤5, and the M element includes one or more of Mn, Fe, Co, Ni, Mo or Cu; and the surface layer includes a first organic matter, which is an organic lithium salt containing the B element.

[0007] The second aspect of the present invention provides a positive electrode sheet, which includes the positive electrode lithium replenishing material described in the first aspect of the present invention. The positive electrode lithium replenishing material is at least one of the positive electrode lithium replenishing materials provided by the present invention.

[0008] The third aspect of the present invention provides a battery, comprising the positive electrode lithium supplement material described in the first aspect of the present invention, or comprising the positive electrode sheet described in the second aspect of the present invention.

[0009] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0010] (1) The positive electrode lithium supplement material provided by the present invention comprises a transition metal oxide core and a surface layer coated with a first organic matter. The positive electrode lithium supplement material can absorb oxygen and has the advantages of less gas production, good stability, and low residual alkali content;

[0011] (2) The positive electrode provided by the present invention has the advantages of high initial coulombic efficiency, high energy density, good stability and low residual alkali content.

[0012] (3) The battery provided by the present invention has the advantages of less gas production, low battery cell expansion rate, high initial coulombic efficiency, long cycle life and high energy density.

[0013] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 Shown is a schematic structural diagram of the positive electrode lithium supplement material in the present invention.

[0015] Figure 2 Shown is the XRD pattern of Li5FeO4 prepared in Example 1.

[0016] Figure 3 Shown is a SEM image of the positive electrode lithium replenishing material (positive electrode lithium replenishing agent) prepared in Example 1.

[0017] Figure 4The figure shows the SEM morphology of the positive electrode sheet prepared by mixing the lithium supplement agent prepared in Example 1 with lithium cobalt oxide. DETAILED DESCRIPTION

[0018] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0019] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0020] Among lithium-rich ternary compounds, lithium-rich ferrite (Li5FeO4) has become the preferred choice for lithium supplements due to its high irreversible capacity (>700mAh / g), cheap raw materials, and reliable synthesis methods. However, lithium-rich ferrite will produce 3 O2 and 1 O2, some of the O2 can be removed by cutting off the airbag after the battery is formed, but the oxygen remaining in the electrolyte will continue to oxidize the electrolyte, causing serious gas production in the battery cell, among which singlet oxygen ( 1 O2, the first excited state of oxygen molecules) is an important reason for the side reaction. 1 One π* orbital of O2 is occupied by two electrons with opposite spins at the same time, and there is no electron in the other π* orbital. This electronic structure gives 1 O2 has strong oxidizing and electrophilic properties, which can attack most battery components, such as organic solvents, electrolyte salts, redox media, and electrode materials, thereby producing passivation byproducts. In addition, the lithium supplement itself contains a high amount of lithium, and lithium will precipitate on the surface, further reacting with H2O and CO2 to produce residual alkali, resulting in a high residual alkali content on the surface of the lithium-rich ternary compound.

[0021] In order to eliminate the generation of lithium-rich ternary compounds 1 O2 and 3 O2, and inhibit the side reactions induced by it, improve battery stability, improve high-temperature storage gas production and cycle gas production, the present invention provides the following technical solutions:

[0022] The first aspect of the present invention provides a positive electrode lithium supplement material, the positive electrode lithium supplement material comprises a transition metal oxide Li x MO y A core, and a surface layer coated on the core; wherein 2≤x≤6, 0<y≤5, and the M element includes one or more of Mn, Fe, Co, Ni, Mo or Cu;

[0023] The surface layer includes a first organic substance, and the first organic substance is an organic lithium salt containing a B element;

[0024] In some embodiments, the transition metal oxide Li x MO y In the embodiment, x can be 2, 3, 4, 5, or 6, y can be 1, 2, 3, 4, or 5, and the M element can be one or more of Mn, Fe, Co, Ni, Mo, or Cu. Preferably, the M element is any one of Mn, Fe, Co, Ni, Mo, or Cu. The transition metal oxide core can be, for example, Li5FeO 4、 One or more of Li2NiO2, Li6CoO4, Li2MnO4, Li2CuO2 and Li2MoO3.

[0025] In the positive electrode lithium supplement material of the present invention, Figure 1 As shown in the structural schematic diagram of the positive electrode lithium supplement material, in the transition metal oxide Li x MO y The surface of the lithium-rich ternary compound is coated with a layer of organic lithium salt (first organic matter) containing element B, in which element B tends to combine with oxygen free radicals to form BO anions, absorbing the oxygen generated during the lithium-rich ternary compound delithiation process, inhibiting the precipitation of gas, and reducing the cycle of lithium batteries. 1 O2 and 3 O2 attacks the electrolyte, improves the serious gas production problem of the battery cell during high-temperature cycling and storage, and increases the battery cycle life and energy density. In addition, the organic lithium salt containing element B has good environmental stability, can improve the stability of the positive electrode lithium supplement material, reduce the residual alkali on the surface, improve the stability of the positive electrode slurry, and reduce the risk of gelation during the positive electrode slurry process.

[0026] In some embodiments, the surface layer further comprises a second organic substance, and the chemical formula of the second organic substance is shown in Formula I below:

[0027] Wherein, R1, R2, R3 are independently selected from H, halogen, substituted or unsubstituted straight or branched C1-C10 alkyl, and the substituent includes halogen. Straight or branched C1-C10 alkyl means a monovalent alkyl with 1-10 carbon atoms, for example, it can be the following groups: methyl, ethyl, n-propyl, iso-propyl, n-butyl, sec-butyl, iso-butyl, tert-butyl, n-pentyl, 1-ethylpropyl, 2-methylbutyl, 3-methylbutyl, 2,2-dimethylpropyl, n-hexyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, n-heptyl, 2-methylhexyl, 3-methylhexyl, 4-methylhexyl, 5-methylhexyl, n-heptyl, n-octyl, n-nonyl, n-decyl. Preferably, it includes C1-C6 alkyl, more preferably C1-C4 alkyl.

[0028] The second organic compound is triphenylamine and its derivatives containing lone pair electrons and N element. The second organic compound has lone pair electrons and can adsorb highly electrophilic 1 O2, forming a singlet complex, in the process of intersystem crossing, 1 A spin-down electron of O2 undergoes spin flipping and fills the spin-up vacancy in the Pz orbital of the triphenylamine derivative. The singlet complex relaxes into a triplet complex, which then dissociates into 3 O2 and triphenylamine derivatives, the dissociated triphenylamine derivatives can enter the next 1 O2 quench cycle.

[0029] On the basis of coating the surface of the lithium-rich ternary compound with the first organic matter, the second organic matter is adjusted to be coated, and the first organic matter and the second organic matter are used in combination, and the second organic matter can 1 O2 is converted to 3 O2, reducing its oxidizing property, and at the same time, the first organic matter captures and absorbs oxygen, reducing the oxidizing effect of oxygen on the electrolyte, and the first organic matter and the second organic matter are used together to further slow down the expansion of the battery cell caused by the release of gas. In addition, the first organic matter and the second organic matter are used together to improve the environmental stability of the organic matter on the surface, further reduce the residual alkali on the surface of the lithium supplement, improve the slurry stability, and further improve the cycle performance and energy density of the battery.

[0030] In some embodiments, the surface layer may include a first organic coating layer and a second organic coating layer. For example, by using atomic layer deposition (ALD), the second organic is first deposited on the surface of the transition metal oxide core to form a second organic coating layer, and then the first organic is deposited on the surface of the second organic coating layer to form the first organic coating layer, thereby forming a two-layer coating method, or the coating order of the first organic coating layer and the second organic coating layer is replaced.

[0031] In some embodiments, the surface layer includes a composite of a first organic substance and a second organic substance, that is, a transition metal oxide Li x MO y The surface layer on the inner core is a complex of an organic lithium salt containing the B element and triphenylamine and its derivatives containing a lone pair of electrons and the N element.

[0032] In some embodiments, in the composite, the mass ratio of the second organic matter to the first organic matter is 0.2-1, that is, the mass ratio of triphenylamine and its derivatives to the organic lithium salt containing the B element is (0.2-1):1. For example, the mass ratio can be 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, preferably 0.25-1. When the mass ratio of the second organic matter to the first organic matter is too high (exceeding 1:1), the second organic matter is too much and the first organic matter is too little. The excessive second organic matter can make the conversion effect of singlet oxygen better, thereby reducing the oxide of the positive electrode lithium supplement material, but the first organic matter is too little and cannot effectively absorb oxygen, cannot effectively alleviate the release of gas, and the effect of improving the expansion of the battery cell is not good; when the mass ratio of the second organic matter to the first organic matter is too low (less than 0.2:1), the second organic matter is too little and the first organic matter is too much. The excessive second organic matter causes the conversion effect of singlet oxygen to be poor, and cannot effectively reduce the oxide of the positive electrode lithium supplement material, and cannot effectively improve the oxidation effect of the positive electrode lithium supplement material on the electrolyte.

[0033] On the basis of coating the surface of the lithium-rich ternary compound with the complex of the first organic matter and the second organic matter, when the mass ratio of the second organic matter to the first organic matter is adjusted within the above range, the second organic matter can better play the effect of converting singlet oxygen, and the first organic matter can better play the effect of capturing oxygen. Under the combined effect, the oxidation effect of oxygen on the electrolyte is further reduced, and the expansion of the battery cell caused by the release of gas is further slowed down.

[0034] In some embodiments, the transition metal oxide Li x MO y The total weight of the surface layer can be, for example, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.8wt%, 2.0wt%, 2.2wt%, 2.4wt%, 2.5wt%, 2.8wt%, 3wt%. The coated surface layer is an inactive material. The less the coating amount, the less the impact on the capacity of the lithium battery. On the basis of coating the surface of the lithium-rich ternary compound with the composite of the first organic matter and the second organic matter, when the mass proportion of the surface layer is adjusted within the above range, the effect of the surface layer in reducing oxidation and absorbing oxygen can be better improved while the coated surface layer has little effect on the energy density of the battery, thereby reducing the oxidation effect of oxygen on the electrolyte, slowing down the expansion of the battery cell caused by the release of gas, and improving the cycle performance and energy density of the battery.

[0035] In some embodiments, the first organic matter includes one or more of lithium dioxalatoborate (LiBOB), lithium difluorooxalatoborate (LiODFB), lithium (2-fluoromalonate) difluoroborate (LIFMDFB), lithium difluoro(1,2-dihydroxyethane-1,1,2,2-tetracarbonitrile)borate (LiDFTCB), more preferably LiBOB. On the basis of coating the surface of the lithium-rich ternary compound with the first organic matter, the type of organic lithium salt containing the B element is further preferred, which can better improve the effect of the first organic matter in absorbing oxygen, thereby facilitating the expansion of the battery cell caused by the release of gas; and further improve the stability of the positive electrode lithium supplement material, reduce the residual alkali on the surface, and improve the stability of the slurry process.

[0036] In some embodiments, the second organic compound includes a compound as shown below:

[0037]

[0038] Triphenylamine (TPA) shown in Formula 1 is preferred. On the basis of coating the surface of the lithium-rich ternary compound with the composite of the first organic matter and the second organic matter, the type of the second organic matter is further preferred, so that the triphenylamine and its derivatives containing lone pair electrons and N elements can better exert the conversion effect of singlet oxygen, reduce the oxidizability of the positive electrode lithium supplement material, reduce the oxidation effect on the electrolyte, and significantly reduce the gas production during high-temperature storage and after high-temperature cycling; and further improve the stability of the positive electrode lithium supplement material, reduce the residual alkali on the surface, and improve the stability of the positive electrode slurry process.

[0039] In some preferred embodiments, the surface layer includes a complex of lithium borate oxalate (LiBOB) and triphenylamine (TPA). TPA in the surface layer can convert singlet oxygen with strong oxidizing properties into triplet oxygen, and can be recycled repeatedly; LiBOB acts as an oxygen adsorption layer, and B in LiBOB tends to combine with oxygen free radicals to form BO anions, inhibiting the release of gas and further reducing the cycle process. 1 O2 and 3 O2 attacks the electrolyte, improves the serious gas generation problem of the battery during high-temperature cycling and storage, and improves the battery cycle life and energy density. At the same time, TPA and LiBOB in the surface layer have good environmental stability, further improving the stability of the positive electrode lithium supplement material, reducing the surface residual alkali, and improving the stability of the slurry process.

[0040] In some embodiments, in the positive electrode lithium replenishing material, the thickness of the surface layer is 1nm-30nm, for example, it can be 1nm, 2nm, 3nm, 5nm, 8nm, 10nm, 12nm, 15nm, 18nm, 20nm, 22nm, 25nm, 28nm, 30nm. On the basis of coating the surface of the lithium-rich ternary compound with the first organic matter and the second organic matter complex, when the thickness of the surface layer is adjusted within the above range, the gram capacity of the positive electrode lithium replenishing material is less affected, and the lithium replenishing efficiency of the cathode lithium replenishing agent is improved; avoid too thick coated surface layer to reduce the gram capacity of the lithium replenishing agent and reduce the lithium replenishing efficiency, and avoid too thin coated surface layer to reduce the effect of reducing oxidizability and oxygen absorption, and ensure that the coated surface layer can reduce the oxidation of the electrolyte and slow down the expansion of the battery cell caused by the release of gas.

[0041] In some embodiments, the Dv50 of the positive electrode lithium supplement material is 5μm-15μm, for example, it can be 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, preferably 8μm-12μm. The smaller the Dv50 of the positive electrode lithium supplement material, the higher the reaction activity, the larger the specific surface area, and the more contact with the electrolyte, resulting in an increase in the gas production of the battery cell; the larger the Dv50 of the positive electrode lithium supplement material, the lower the reaction activity, resulting in insufficient lithium removal, low lithium supplement capacity, low battery cell capacity, and low energy density. On the basis of coating the surface of the lithium-rich ternary compound with the complex of the first organic matter and the second organic matter, when the Dv50 of the positive electrode lithium replenishing material is adjusted to the above range, the specific surface area of ​​the positive electrode lithium replenishing material is small, the surface residual alkali is low, and it is more conducive to processing during the ingredient preparation process. At the same time, it can avoid the problems of the positive electrode lithium replenishing material having too large Dv50, poor conductivity, low reaction activity, and high delithiation potential resulting in poor lithium replenishment effect.

[0042] The present invention also provides a method for preparing the above-mentioned positive electrode lithium supplement material, comprising the following steps:

[0043] (1) The metal oxide M x O y Mix evenly with lithium salt and sinter at high temperature to obtain transition metal oxide Li x MO y Kernel;

[0044] (2) weighing a second organic substance and a first organic substance according to a certain weight, dissolving them in an organic solvent, and mixing them to obtain a mixed solution;

[0045] (3) Weigh a certain amount of transition metal oxide Li x MO y , placed in the mixed solution obtained in step (2), mixed thoroughly, and then dried to obtain the positive electrode lithium supplement material.

[0046] In some embodiments, in step (1), the metal oxide M x O y Including but not limited to one or more of MnO, Fe2O3, Co3O4, NiO, MoO3 or CuO.

[0047] In some embodiments, in step (1), the lithium salt includes but is not limited to one or more of Li2O, LiOH·H2O, and Li2CO3.

[0048] In some embodiments, in step (1), the sintering temperature is 650-800° C., and the sintering time is 12-24 hours.

[0049] In some embodiments, in step (2), the mass ratio of the second organic matter to the first organic matter is 0.2-1. The mixing time is 0.5-1h. There is no particular limitation on the mixing method, as long as it can meet the purpose of the present application. For example, the mixing can be conventional mixing methods such as magnetic stirring, mechanical stirring and ultrasonic treatment. There is no particular limitation on the organic solvent, for example, it can be methanol, ethanol, isopropanol, etc.

[0050] In some embodiments, in step (3), there is no particular limitation on the drying method, as long as it can meet the purpose of the present application, for example, conventional drying methods such as spray drying or oven drying can be used. The drying temperature is 100-200°C, and the drying time is adjusted according to the needs.

[0051] The second aspect of the present invention provides a positive electrode sheet, which includes the positive electrode lithium replenishing material described in the first aspect of the present invention. The positive electrode lithium replenishing material is at least one of the positive electrode lithium replenishing materials provided by the present invention.

[0052] The positive electrode sheet provided by the present invention, due to the inclusion of the above-mentioned positive electrode lithium replenishing material, can improve the capacity of the positive electrode sheet, enhance the lithium replenishing effect of the cathode lithium replenisher, enhance the initial coulombic efficiency and energy density of the battery containing the positive electrode sheet, reduce the side reactions caused by the oxidation of the battery's electrolyte, enhance the stability of the battery, and reduce high-temperature storage gas production and circulation gas production.

[0053] In some embodiments, the positive electrode sheet further comprises a positive electrode active material; based on the total weight of the positive electrode active material, the mass proportion of the positive electrode lithium supplement material (lithium supplement agent) is 0.1-2wt%, for example, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.8wt%, 2.0wt%. On the basis that the positive electrode sheet contains the positive electrode lithium supplement agent of the present invention, when the mass proportion of the lithium supplement agent is within the above range, the active lithium lost due to the formation of SEI (solid electrolyte membrane) during the first cycle of battery charging and discharging can be effectively compensated, thereby improving the first cycle coulomb efficiency of the battery, increasing the number of lithium ions available inside the battery, and thus improving the total capacity and energy density of the battery.

[0054] In some embodiments, in the positive electrode sheet, the content of M element is 1,000ppm-20,000ppm, for example, 1,000ppm, 2,000ppm, 3,000ppm, 4,000ppm, 5,000ppm, 6,000ppm, 7,000ppm, 8,000ppm, 9,000ppm, 10,000ppm, 11,000ppm, 12,000ppm, 13,000ppm, 14,000ppm, 15,000ppm, 16,000ppm, 17,000ppm, 18,000ppm, 19,000ppm, 20,000ppm. On the basis that the positive electrode sheet contains the positive electrode lithium supplement agent of the present invention, when the content of M element in the positive electrode sheet is adjusted to the above range, it indicates that the addition amount of the positive electrode lithium supplement material (lithium supplement agent) is appropriate, which can improve the first week coulomb efficiency of the battery and improve the total capacity and energy density of the battery.

[0055] In some embodiments, the positive electrode sheet includes a positive electrode active material, a positive electrode lithium supplement material, a conductive agent, and a binder. The lithium supplement material, the positive electrode active material, the conductive agent, and the binder are mixed in a certain ratio and uniformly coated on the surface of a positive electrode current collector (e.g., an aluminum current collector) to prepare a positive electrode sheet.

[0056] There is no particular restriction on the positive electrode active material, for example, the positive electrode active material includes at least one of lithium cobalt oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium phosphate, lithium vanadate, lithium manganate, lithium nickel oxide, lithium nickel cobalt manganate, lithium-rich manganese-based materials or lithium nickel cobalt aluminum oxide. There is no particular restriction on the conductive agent, for example, the conductive agent includes one or more of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, metal powder, and carbon fiber; the binder is selected from one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyacrylic acid lithium (PAALi). There is no particular restriction on the binder, for example, the binder includes at least one of polypropylene, polyethylene, polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene, polytetrafluoroethylene or polyhexafluoropropylene.

[0057] In some embodiments, the positive electrode sheet satisfies at least one of the following conditions:

[0058] (i) The thickness of the positive electrode sheet is 80mm-170mm;

[0059] (ii) The surface density of the positive electrode is 15 mg / cm 2 -30 mg / cm 2 ;

[0060] (iii) The compaction density of the positive electrode is 4.1 g / cm 3 -4.3g / cm 3 .

[0061] In some embodiments, the thickness of the positive electrode sheet can be, for example, 80mm, 82mm, 84mm, 85mm, 86mm, 88mm, 90mm, 92mm, 94mm, 95mm, 96mm, 98mm, 100mm, 110mm, 120mm, 130mm, 140mm, 150mm, 160mm, 170mm. On the basis that the positive electrode sheet contains the positive electrode lithium supplement of the present invention, when the thickness of the positive electrode sheet is adjusted to the above range, during the charge and discharge process, lithium ions can be fully embedded and de-embedded in the positive electrode active material, thereby increasing the capacity of the battery; and the expansion and contraction caused by the embedding and de-embedding of lithium ions during the charge and discharge process can be reduced, thereby reducing the risk of loosening and cracking of the positive electrode sheet and extending the cycle life of the battery.

[0062] In some embodiments, the surface density of the positive electrode sheet is 15 mg / cm 2 、16mg / cm 2 、17mg / cm 2 、18mg / cm 2 、19mg / cm 2 , 20mg / cm 2 , 21mg / cm 2, 22mg / cm 2 , 23mg / cm 2 , 24mg / cm 2 , 25mg / cm 2 、26mg / cm 2 , 27mg / cm 2 、28mg / cm 2 , 29mg / cm 2 、30mg / cm 2 , preferably 16 mg / cm 2 -20mg / cm 2 On the basis that the positive electrode sheet contains the positive electrode lithium supplement agent of the present invention, when the surface density of the positive electrode sheet is adjusted within the above range, the distribution and arrangement of the positive electrode active material are more reasonable, which is conducive to the insertion and extraction of lithium ions, thereby maximizing the utilization rate of the active material and improving the energy density of the battery; and it is helpful to maintain the structural stability of the positive electrode sheet, reduce the structural changes caused by the insertion and extraction of lithium ions during the charge and discharge cycle, such as expansion, contraction, etc., thereby improving the cycle life of the battery.

[0063] In some embodiments, the compaction density of the positive electrode sheet is 4.10 g / cm 3 4.15g / cm 3 4.20g / cm 3 4.25g / cm 3 4.30g / cm 3 When the positive electrode sheet contains the positive electrode lithium supplement of the present invention and the compaction density of the positive electrode sheet is adjusted within the above range, the volume density of the active substance in the positive electrode material can be increased, so that more active substances can participate in the electrochemical reaction, thereby increasing the capacity of the battery; and the capacity attenuation caused by structural changes can be reduced, so that the battery can maintain a high capacity retention rate during long-term use.

[0064] The third aspect of the present invention provides a battery, comprising the positive electrode lithium supplement material described in the first aspect of the present invention, or comprising the positive electrode sheet described in the second aspect of the present invention.

[0065] The battery of the present invention, because it contains the above-mentioned positive electrode lithium supplement material or positive electrode sheet, has the advantages of less gas production, low battery cell expansion rate, high initial coulomb efficiency, long cycle life and high energy density.

[0066] In some embodiments, the battery further comprises a negative electrode sheet, the negative electrode sheet comprises a negative electrode active material, and the negative electrode active material comprises a silicon material. Preferably, the mass proportion of silicon material in the negative electrode active material is ≥ 2%. The silicon material in the negative electrode active material can provide a higher specific capacity and improve the energy density of the battery.

[0067] In some embodiments, the silicon material includes at least one of silicon carbon, silicon oxygen, silicon alone, and silicon alloy; more preferably silicon carbon.

[0068] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0069] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0070] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0071] Example A Group Preparation of Positive Electrode Lithium Supplement Material

[0072] Embodiment A1-1:

[0073] (1) Lithium oxide and ferric oxide were weighed according to a molar ratio of Li:Fe of 5.1:1, and mixed at high speed for 5 min using a mixer. The mixed material was placed in a crucible and sintered at 750°C for 24 h in a tube furnace filled with an inert atmosphere. After sintering, the mixture was further crushed by a jet mill to obtain a Li5FeO4 lithium supplement. Its XRD is as follows: Figure 2 shown.

[0074] (2) Triphenylamine (TPA) and lithium bis(oxalatoborate) (LiBOB) were mixed in a mass ratio of 3:7, dissolved in a methanol solution, and magnetically stirred for 30 minutes to obtain a mixed solution A.

[0075] (3) Weigh a certain amount of Li5FeO4 and dissolve it in the mixed solution A, stirring for 20 minutes. Finally, spray drying is performed at 120°C to obtain a composite lithium supplement (i.e., a surface layer of LiBOB and TPA complex coated on the surface of Li5FeO4). The final morphology is as follows: Figure 3 shown.

[0076] The positive electrode lithium supplement materials of Example A1-A6 and Comparative Examples A1-A3 are prepared with reference to Example 1-1, and the specific different technical features are shown in Table 1. In Example A1, the coated surface layer is a composite of a first organic matter and a second organic matter, and the type of the second organic matter is changed. In Example A2, only the surface layer of the first organic matter is coated, and the type of the first organic matter is changed. In Example A3, the mass ratio of the second organic matter to the first organic matter is changed, which is achieved by adjusting the mass ratio of the two in step (2). In Example A4, the mass proportion and thickness of the surface layer are changed, which is achieved by adjusting the concentration of the mixed solution of TPA and lithium bis(oxalatoborate) (LiBOB) in step (2). In Example A5, the particle size of the lithium supplement agent is changed, which is achieved by adjusting the pressure of the airflow crushing. In Example A6, the type of transition metal oxide is changed.

[0077] Referring to Example A1-1, the type of the second organic matter in Example A1 group was changed; the type of the first organic matter in Example A2 group was changed (the second organic matter was not added in Example A2-1); the mass ratio of the second organic matter to the first organic matter in Example A3 group was changed; the mass proportion and thickness of the surface layer in Example A4 group were changed; and the particle size of the lithium supplement agent in Example A5 group was changed. See Table 1 below for specific differences.

[0078] Table 1

[0079]

[0080]

[0081] Note: "*" indicates that the corresponding parameters in this example or comparative example are the same as those in Example A1-1. " / " indicates that the corresponding parameters were not tested or the corresponding organic matter was not added.

[0082] In Example A6 group, the core type of the lithium supplement agent is changed, wherein in Example A6-1, Li2CuO2 replaces Li5FeO4; in Example A6-2, Li2MoO3 replaces Li5FeO4.

[0083] Comparative Example A1 is carried out with reference to Example A1-1, but without coating, and only step (1) is carried out.

[0084] Comparative Example A2:

[0085] Lithium oxide and ferric oxide were weighed according to the molar ratio of Li:Fe being 5.1:1, and a certain amount of glucose (glucose accounts for 4% of the total mass ratio) was weighed at the same time, and mixed at high speed for 5 minutes using a mixer. The mixed materials were placed in a crucible and sintered at 700°C for 24 hours in a tubular furnace filled with an inert atmosphere to obtain a carbon-coated Li5FeO4 lithium supplement.

[0086] Comparative Example A3:

[0087] Lithium oxide and ferric oxide were weighed according to a Li:Fe molar ratio of 5.1:1, and mixed at high speed for 5 minutes using a mixer. The mixed materials were placed in a crucible and sintered at 700°C for 24 hours in a tubular furnace filled with an inert atmosphere to obtain a Li5FeO4 lithium supplement. Li5FeO4 and Al2O3 were further weighed, mixed at high speed for 3 minutes, and sintered at 650°C for 7 hours in a tubular furnace filled with an inert atmosphere to obtain an Al2O3-coated Li5FeO4 lithium supplement.

[0088] The positive electrode lithium supplement materials obtained in the above-mentioned Example A1-A6 groups and Comparative Examples A1-A3 were subjected to the following residual alkali test, and the test method is as follows:

[0089] ① Accurately weigh 1.0g±0.1g of lithium supplement into a 100ml clean and dry conical flask with a stopper, add 100ml methanol to the conical flask, and stir at 800rpm for 5 minutes (using a 3cm magnetic stirrer). After stirring, vacuum filter, select a 50mm diameter, 0.2μm pore size water-based microporous filter membrane, and collect the filtrate into a 100ml volumetric flask.

[0090] ②Pipette 1 mL of the filtrate into the titration cup and dilute it to 40 mL with pure water. Use 0.01 M HCl standard solution to perform a residual alkali test using an acid-base potentiometric titrator to obtain a titration curve and record the titration results R1, R2, and R3, R1+R2=V1, and R1+R2+R3=V2.

[0091] ③ Obtain LiOH and Li2CO3 contents by the following calculation method

[0092]

[0093] Total amount of residual alkali (wt%) = LiOH (wt%) + Li2CO3 (wt%)

[0094] 73.89: Molar mass of Li2CO3, M(Li2CO3);

[0095] 36.94: 1 / 2 molar mass of Li2CO3 M(1 / 2Li2CO3);

[0096] 23.94: molar mass of LiOH M(LiOH);

[0097] m: weigh the mass of the test sample;

[0098] c: concentration of HCl standard solution;

[0099] V3: volume of the filtrate;

[0100] V4: Volume of ultrapure water: 100ml

[0101] The residual alkali test results of Example A1-A6 and Comparative Examples A1-A3 are shown in Table 2.

[0102] Table 2

[0103]

[0104] It can be seen from Table 2 that the surface of the positive electrode lithium supplement material of the present invention is coated with the first organic matter and the second organic matter, which is helpful to reduce the residual alkali on the surface of the lithium supplement agent.

[0105] In Comparative Examples A2 and A3, the coating is uneven, and the exposed surface of the lithium supplementer is still in contact with CO2 and moisture in the air, resulting in high residual alkali, poor environmental stability, and severe gas production.

[0106] Example B Group Preparation of Button Cells

[0107] (1) The positive electrode lithium supplement material prepared in the above-mentioned Example A1-A6 group and Comparative Example A1-A3: conductive carbon black: PVDF = 90:5:5 were mixed evenly and coated on aluminum foil to make different positive electrode sheets. The thickness of the positive electrode sheet was 0.08 mm, and the surface density of the positive electrode sheet was 0.2835 mg / cm 2 The compaction density of the positive electrode is 4.05g / cm 3 .

[0108] The positive electrode lithium supplement material prepared in the above Example A1-1 was mixed with lithium cobalt oxide to obtain a positive electrode active material, which was evenly mixed according to the ratio of positive electrode active material: conductive carbon black: PVDF = 90:5:5 (the SEM morphology of the positive electrode sheet prepared after the lithium supplement material and lithium cobalt oxide were mixed is as shown in FIG. Figure 4 As shown in Table 3, different positive electrodes are made by coating on aluminum foil. By changing the mass proportion of lithium supplement, the content of M element changes at the same time.

[0109] (2) In a dry room, button cells were assembled with lithium metal sheets, diaphragms, and electrolytes (the diaphragms were made of polypropylene (PP) diaphragms. The electrolytes were made of lithium hexafluorophosphate (LiPF6) with a concentration of 1 mol / L dissolved in a mixture solution of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1) and were respectively labeled as Example B1-B6 Group, Example B7 Group, and Comparative Examples B1-B3.

[0110] Table 3

[0111]

[0112]

[0113] The positive electrode lithium supplement material containing the above-mentioned Example B1-B7 groups and Comparative Examples B1-B3 was subjected to the following performance test, and the test conditions were: voltage range 3-4.6V, 0.1C constant current to 4.6V, 4.6V constant voltage charging with a cut-off current of 0.05C, recording the first charge gram capacity (mAh / g), the first discharge gram capacity (mAh / g) and calculating the first coulombic efficiency (first coulombic efficiency = first discharge gram capacity / first charge gram capacity).

[0114] The results of the tests of Example B1-B7 and Comparative Examples B1-B3 are recorded in Table 4.

[0115] Table 4

[0116]

[0117]

[0118] It can be seen from Table 4 that the positive electrode lithium supplement material provided by the present invention can improve the capacity of the positive electrode sheet and enhance the initial coulombic efficiency and energy density of the battery containing the positive electrode sheet.

[0119] Example C Group Preparation of Lithium Batteries

[0120] (1) The positive electrode lithium supplement material prepared in the above-mentioned Example A1-A6 group and Comparative Example A1-A3 is mixed with commercial lithium cobalt oxide, and (lithium supplement agent + lithium cobalt oxide): conductive carbon black: polyvinylidene fluoride are mixed evenly at a weight ratio of 98.2:1:0.8, and then coated on the positive electrode collector to prepare a positive electrode plate, and the lithium supplement agent accounts for 1wt% in the active material.

[0121] (2) Mix them evenly in a weight ratio of (graphite + 5% silicon carbon): conductive carbon black: polyacrylic acid = 97.2:1.45:1.35, and then apply them on the negative electrode collector to prepare a negative electrode sheet.

[0122] (3) The positive electrode sheets prepared above and the positive electrode sheets prepared in Example B7 group, as well as the negative electrode sheets, separators, and electrolytes (the separator is a PP / PE / PP composite film with a thickness of 8 μm and a porosity of 42%. The electrolyte uses lithium hexafluorophosphate (LiPF6) as the lithium salt, and the solvent is a mixture solution of ethylene carbonate (EC) and diethyl carbonate (DEC)) are assembled into lithium-ion batteries, which are respectively recorded as Example C1-C7 groups and Comparative Examples C1-C3.

[0123] The lithium ion batteries containing the above C1-C7 groups and comparative examples C1-C3 were subjected to the following performance tests:

[0124] (1) Capacity test: The above battery was left to stand for 5 minutes, and then charged to 4.53V at 0.5C constant current and constant voltage, with a cut-off current of 0.025C. After standing for 5 minutes, it was discharged to 3V at 0.2C constant current, and the capacity Q1 at this time was recorded. Energy density = Q1 × platform voltage / battery volume. The corresponding results are shown in Table 5.

[0125] (2) 25℃ cycle performance test: The battery was placed in a (25±2)℃ environment and allowed to stand for 10 min. The battery was charged to 4.53 V at 1.2C constant current and constant voltage, with a cut-off current of 0.05C. After the battery was fully charged, it was left for 5 min and then discharged at 0.5C constant current to a cut-off voltage of 3.0 V. The highest discharge capacity of the first three cycles was recorded as the initial capacity Q2. When the number of cycles reached 200, the last discharge capacity of the battery was recorded as Q3. The cycle retention rate = Q3 / Q2. The recorded results are shown in Table 5.

[0126] (3) Battery swelling test after 8h storage at 85℃: First, the initial thickness H1 of the above battery was tested, and then the above battery was placed in an environment of (25±2)℃, left to stand for 10min, discharged to 3V at 0.2C, left to stand for 10min, and then charged to 4.53V at 0.7C. The battery was further placed in an oven at 85℃±2℃ for 8H. After the storage, the sample was taken out and immediately tested for the thermal thickness H2, and the battery swelling rate was calculated (swelling rate = (H2-H1) / H1). The results are shown in Table 5.

[0127] The results of the tests of Example C1-C7 and Comparative Examples C1-C3 are recorded in Table 5.

[0128] Table 5

[0129]

[0130]

[0131] It can be seen from Table 5 that coating the first organic matter and the second organic matter composite on the surface of the positive electrode lithium supplement agent can reduce the oxidation of oxygen on the electrolyte, slow down the expansion of the battery cell caused by gas release, and improve the cycle performance and energy density of the battery.

[0132] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A positive electrode lithium supplement material, characterized in that: The positive electrode lithium supplement material includes a transition metal oxide Li x MO y A core, and a surface layer covering the core; Wherein, 2≤x≤6, 0<y≤5, and the M element includes one or more of Mn, Fe, Co, Ni, Mo or Cu; The surface layer includes a first organic substance, which is an organic lithium salt containing a B element.

2. The positive electrode lithium supplement material according to claim 1, characterized in that: The surface layer further includes a second organic substance, and the chemical formula of the second organic substance is shown in the following formula I: Wherein, R1, R2, and R3 are independently selected from H, halogen, substituted or unsubstituted straight or branched C1-C10 alkyl, and the substituents include halogen.

3. The positive electrode lithium supplement material according to claim 2, characterized in that: The surface layer includes a composite of a first organic substance and a second organic substance; Preferably, in the composite, the mass ratio of the second organic matter to the first organic matter is 0.2-1; Preferably, the transition metal oxide Li x MO y According to the total weight of the surface layer, the mass proportion of the surface layer is 0.2wt%-3wt%.

4. The positive electrode lithium supplement material according to claim 2, characterized in that: The first organic substance includes one or more of lithium dioxalatoborate, lithium difluorooxalatoborate, lithium (2-fluoromalonate) difluoroborate, and lithium difluoro(1,2-dihydroxyethane-1,1,2,2-tetracarbonitrile)borate; Preferably, the second organic matter comprises a compound as shown below:

5. The positive electrode lithium supplement material according to any one of claims 1 to 4, characterized in that: The thickness of the surface layer is 1nm-30nm; Preferably, the Dv50 of the positive electrode lithium supplement material is 5 μm-15 μm; Preferably, the core comprises Li5FeO 4、 One or more of Li2NiO2, Li6CoO4, Li2MnO4, Li2CuO2 and Li2MoO3.

6. A positive electrode sheet, characterized in that: The invention comprises the positive electrode lithium supplement material according to any one of claims 1 to 5.

7. The positive electrode sheet according to claim 6, characterized in that: The positive electrode sheet also includes a positive electrode active material; based on the total mass of the positive electrode active material, the mass proportion of the positive electrode lithium supplement material is 0.1 to 2 wt%; Preferably, in the positive electrode sheet, the content of the M element is 1,000ppm-20,000ppm.

8. The positive electrode sheet according to claim 6, characterized in that: The positive electrode sheet satisfies at least one of the following conditions: (i) The thickness of the positive electrode sheet is 80mm-170mm; (ii) The surface density of the positive electrode is 15 mg / cm 2 -30 mg / cm 2 ; (iii) The compaction density of the positive electrode is 4.1 g / cm 3 -4.3g / cm 3 .

9. A battery, characterized in that: The positive electrode lithium supplement material comprises any one of claims 1 to 5, or the positive electrode sheet comprises any one of claims 6 to 8.

10. The battery according to claim 9, characterized in that The battery further comprises a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, and the negative electrode active material comprises a silicon material; Preferably, in the negative electrode active material, the mass proportion of silicon material is ≥ 2%; Preferably, the silicon material includes at least one of silicon carbon, silicon oxygen, silicon alone, and silicon alloy; more preferably silicon carbon.

Citation Information

Cited By

  • Lithium supplement agent and preparation method thereof, positive plate, battery and electric equipment

    CN120048906A

  • Lithium supplement, preparation method thereof, positive electrode sheet, battery and electrical equipment

    CN120048906B

  • Battery monomer, battery device, power utilization device and energy storage device

    CN120600796A