Preparation method of aluminum foil current collector for growing vertical graphene at low temperature

The preparation method of aluminum foil current collectors through low-temperature growth of vertical graphene solves the problem of poor combination performance of aluminum foil current collectors and graphene, and achieves improved performance of the aluminum foil surface and battery performance in sodium-ion batteries.

CN118782807APending Publication Date: 2024-10-15JIANGSU MOGUI NEW MATERIAL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411066545.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The combination of aluminum foil current collector and graphene coating in existing sodium-ion batteries is poor, resulting in limited battery performance improvement, and the need for catalyst assistance affects battery slurry stability.

Method used

An aluminum foil current collector preparation method for low-temperature growth of vertical graphene is used. The PECVD deposition chamber is heated in a vacuum environment and bombarded with Ar gas for cleaning. Then, carbon source gas is introduced at 500-600°C to grow vertical graphene to avoid high-temperature damage. and improve bonding strength.

Benefits of technology

The vertical graphene grown in a low-temperature environment forms a good bonding force with the aluminum foil, which improves the surface roughness of the aluminum foil and the contact with active materials, reduces the resistance, and improves the performance of sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782807A_ABST
    Figure CN118782807A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of aluminum foil current collectors of sodium-ion batteries, and particularly relates to a preparation method of an aluminum foil current collector for growing vertical graphene at low temperature, which comprises the following steps: S1, carrying out surface pretreatment on the aluminum foil current collector; s2, placing the pretreated aluminum foil current collector in a PECVD deposition cavity, and heating the aluminum foil current collector to 500-600 DEG C in a vacuum environment; s3, introducing Ar gas, and performing bombardment cleaning on the surface of the aluminum foil current collector; s4, introducing a carbon source gas, and growing vertical graphene in an environment of 500-600 DEG C; and S5, introducing protective gas, and cooling to room temperature under low pressure to obtain the aluminum foil current collector with the vertical graphene grown at low temperature. According to the invention, a traditional graphene coating is changed into vertical graphene deposited and grown on the surface of the aluminum foil in a low-temperature environment, good binding force with the aluminum foil can be formed without assistance of a catalyst, and meanwhile, the vertical graphene has the characteristics of vertical orientation and non-stacking morphology, so that the performance of the sodium ion battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum foil current collectors for sodium ion batteries, and specifically relates to the selection of electrode materials, and in particular to a method for preparing an aluminum foil current collector for low-temperature growth of vertical graphene. Background Art

[0002] Since sodium resources are abundant in the earth's crust and widely distributed around the world, and the working principle and battery structure of sodium-ion batteries are basically similar to those of lithium-ion batteries, they are compatible with existing lithium-ion equipment, making sodium-ion batteries an important alternative or supplementary technology for lithium-ion batteries. In addition, with the deepening of sodium-ion battery research, the unique advantages of sodium-ion batteries, such as excellent high and low temperature performance and high safety, have also made sodium-ion battery technology one of the development focuses in the field of energy storage. Therefore, it is necessary to fully develop and improve the key components of sodium-ion batteries, strengthen their unique advantages, and improve the performance of sodium-ion battery products, so that they can occupy a favorable position in future market competition.

[0003] Unlike lithium-ion batteries, since aluminum does not undergo alloying reactions at low potentials, both the positive and negative electrodes of sodium-ion batteries can use inexpensive, lightweight aluminum foil as current collectors. Although aluminum foil current collectors have been widely used in multiple battery systems, some of its inherent shortcomings will also have an adverse effect on further improving battery performance. For example, the limited contact area between aluminum foil and the electrode material will increase the internal resistance of the positive electrode to a certain extent; the limited bonding strength between aluminum foil and the active material will cause the particulate matter to fall off during the cyclic charge and discharge process, thereby reducing the battery capacity and cycle life.

[0004] The existing process uses a method of coating the surface of aluminum foil with graphene to improve the surface performance. However, the surface treatment of graphene must be assisted by a catalyst, which affects the stability of the subsequent battery slurry coating. There is also the problem of insufficient adhesion between the graphene coating and the aluminum foil surface.

[0005] Therefore, how to overcome the poor bonding performance of graphene coating on the aluminum foil surface in lithium batteries is a technical problem that needs to be solved urgently in this field.

[0006] It should be noted that the above information disclosed in this background technology section is only for understanding the background technology of the present application concept, and therefore, it may contain information that does not constitute the prior art. Summary of the invention

[0007] The embodiments of the present disclosure at least provide a method for preparing an aluminum foil current collector for low-temperature growth of vertical graphene.

[0008] In a first aspect, an embodiment of the present disclosure provides a method for preparing an aluminum foil current collector for low-temperature growth of vertical graphene, comprising the following steps: step S1, performing surface pretreatment on the aluminum foil current collector; step S2, placing the pretreated aluminum foil current collector in a PECVD deposition chamber, and heating the PECVD deposition chamber to 500-600°C under a vacuum environment; step S3, introducing Ar gas at a flow rate of 2-5 ml / min, and turning on the plasma generator after the pressure in the PECVD deposition chamber is stable, and bombarding and cleaning the surface of the aluminum foil current collector; step S4, after stopping the introduction of Ar gas, introducing carbon source gas, and chemically vapor depositing and growing vertical graphene on the surface of the aluminum foil current collector at 500-600°C; step S5, stopping the introduction of carbon source gas, introducing protective gas, and cooling to room temperature under low pressure to obtain an aluminum foil current collector for low-temperature growth of vertical graphene.

[0009] In an optional embodiment, the surface pretreatment in step S1 is specifically repeated cleaning with acetone or ethanol, and drying in an inert atmosphere for standby use.

[0010] In an optional embodiment, the vacuum atmosphere in step S2 is less than 10 -3 Pa PECVD deposition chamber gas pressure environment.

[0011] In an optional embodiment, the radio frequency power of the plasma generator in step S3 is 300-400 W, and the bombardment cleaning time is 5-15 min.

[0012] In an optional embodiment, the carbon source gas in step S4 is any one of ethylene and propylene; the flow rate of the carbon source gas is 30-60 ml / min, the working gas pressure is 20-60 Pa, and the deposition time is 20-60 min.

[0013] In an optional embodiment, the protective gas in step S5 is any one of nitrogen and argon; the flow rate of the protective gas is 20-40 ml / min.

[0014] In a second aspect, the embodiments of the present disclosure also provide an aluminum foil current collector for low-temperature growth of vertical graphene, which is prepared by the method described above.

[0015] In an optional embodiment, the growth density of the vertical graphene is 0.002-0.008 g / cm 2 .

[0016] In an optional embodiment, the thickness of the vertical graphene is 400-800 nm.

[0017] In a third aspect, the embodiments of the present disclosure also provide an application of the aluminum foil current collector of low-temperature grown vertical graphene as described above in the field of sodium ion batteries.

[0018] The beneficial effect of the present invention is that the preparation method of the aluminum foil current collector for low-temperature grown vertical graphene of the present invention changes the traditional graphene coating to deposit and grow vertical graphene on the surface of the aluminum foil under a low-temperature environment, and can form a good bonding force with the aluminum foil without the assistance of a catalyst. At the same time, the vertical graphene has the characteristics of vertical orientation and non-stacking morphology. Its special non-stacking morphology can greatly increase the roughness of the aluminum foil surface, improve the contact between the active material and the aluminum foil, reduce the resistance of the aluminum foil, and improve the performance of the sodium ion battery.

[0019] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description, claims and drawings.

[0020] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 The SEM image of the vertical graphene on the surface of the aluminum foil of Example 1 provided in the embodiments of the present disclosure; Figure 2 A Raman spectrum of graphene perpendicular to the surface of the aluminum foil of Example 1 provided in the embodiments of the present disclosure; Figure 3 The SEM image of the vertical graphene on the surface of the aluminum foil of Example 2 provided in the embodiments of the present disclosure; Figure 4 A Raman spectrum of graphene perpendicular to the surface of the aluminum foil of Example 2 provided in the embodiments of the present disclosure; Figure 5 The SEM image of the vertical graphene on the surface of the aluminum foil of Example 3 provided in the embodiments of the present disclosure; Figure 6 A Raman spectrum of graphene perpendicular to the surface of the aluminum foil of Example 3 provided in the embodiments of the present disclosure; Figure 7The SEM image of the vertical graphene on the surface of the aluminum foil of Example 4 provided in the embodiments of the present disclosure; Figure 8 This is a Raman spectrum of the vertical graphene on the aluminum foil surface of Example 4 provided in the embodiments of the present disclosure. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Glossary PECVD Plasma Enhanced Chemical Vapor Deposition; SEM Scanning electron microscope.

[0025] Most current studies use modified aluminum foil to improve electrode performance. The main modification methods are: (1) Surface treatment, such as roughening the aluminum foil surface by chemical etching, oxidation, etc., and increasing the specific surface area of ​​the aluminum foil to increase the interfacial conductivity. (2) Conductive coating modification. By coating the aluminum foil surface with a highly conductive coating such as carbon black or graphene, the surface properties of the aluminum foil are changed to improve the battery cycle stability and rate performance. These modification methods can improve the performance of the electrode to a certain extent, but the surface-treated aluminum foil may affect the stability of the subsequent battery slurry coating, resulting in uneven distribution of the electrode material. Conductive coating modification may also have problems with the coating bonding to the aluminum foil surface.

[0026] The defects existing in the above solutions are the results obtained by the inventor after practice and careful research. Therefore, the discovery process of the above problems and the solutions proposed by the present disclosure for the above problems below should be the contributions made by the inventor to the present disclosure during the disclosure process.

[0027] Based on the above research, an embodiment of the present disclosure provides a method for preparing an aluminum foil current collector for low-temperature growth of vertical graphene, comprising the following steps: Step S1, performing surface pretreatment on the aluminum foil current collector; Step S2, placing the pretreated aluminum foil current collector in a PECVD deposition chamber, and heating the PECVD deposition chamber to 500-600°C under a vacuum environment; Step S3, introducing Ar gas at a flow rate of 2-5 ml / min, and turning on the plasma generator after the pressure in the PECVD deposition chamber is stable, and bombarding and cleaning the surface of the aluminum foil current collector; Step S4, after stopping the introduction of Ar gas, introducing carbon source gas, and chemically vapor depositing and growing vertical graphene on the surface of the aluminum foil current collector at 500-600°C; Step S5, stopping the introduction of carbon source gas, introducing protective gas, and cooling to room temperature under low pressure to obtain an aluminum foil current collector for low-temperature growth of vertical graphene.

[0028] Specifically, the low-temperature deposition process at 500-600°C effectively avoids the damage to the aluminum foil caused by high temperature, and the vertical graphene grown in a low-temperature environment does not affect the mechanical properties of the aluminum foil.

[0029] Specifically, compared with graphene coating, growing vertical graphene on the surface of aluminum foil current collector by PECVD deposition not only effectively improves the binding force and thus eliminates the need for catalyst assistance, but also utilizes the vertical orientation and non-stacking morphology unique to vertical graphene to achieve new effects in increasing the roughness of the aluminum foil surface, improving the contact between active substances and aluminum foil, reducing the resistance of aluminum foil, and improving the performance of sodium ion batteries.

[0030] In the embodiment of the present disclosure, specifically, the surface pretreatment in step S1 is to repeatedly clean the surface with acetone or ethanol, and dry the surface in an inert atmosphere for later use.

[0031] In the embodiment of the present disclosure, specifically, the vacuum atmosphere in step S2 is less than 10 -3 Pa PECVD deposition chamber gas pressure environment.

[0032] In the disclosed embodiment, specifically, in step S3, the radio frequency power of the plasma generator is 300-400 W, and the bombardment cleaning time is 5-15 min.

[0033] In the embodiment of the present disclosure, specifically, the carbon source gas in step S4 is any one of ethylene and propylene; the flow rate of the carbon source gas is 30-60 ml / min, the working gas pressure is 20-60 Pa, and the deposition time is 20-60 min.

[0034] In the embodiment of the present disclosure, specifically, the protective gas in step S5 is any one of nitrogen and argon; the flow rate of the protective gas is 20-40 ml / min.

[0035] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0036] The disclosed embodiment also provides an aluminum foil current collector for low-temperature growth of vertical graphene, which is prepared by the method described above.

[0037] In the embodiment of the present disclosure, specifically, the growth density of the vertical graphene is 0.002-0.008 g / cm 2 .

[0038] In the embodiments of the present disclosure, specifically, the thickness of the vertical graphene is 400-800 nm.

[0039] The disclosed embodiments also provide an application of the aluminum foil current collector of low-temperature grown vertical graphene as described above in the field of sodium ion batteries.

[0040] Embodiment 1: This embodiment provides a method for preparing an aluminum foil current collector for low-temperature growth of vertical graphene, comprising the following steps: The aluminum foil current collector with a thickness of 10 μm was ultrasonically cleaned with acetone solution for 15 min, repeated three times, and then blown dry with a nitrogen flow.

[0041] Place the dried aluminum foil in the PECVD deposition chamber, start the mechanical pump group, slowly open the vacuum system, pump the pressure in the chamber to below 0 Pa, turn off the mechanical pump, and introduce nitrogen (50 ml / min). After repeating the operation three times, raise the temperature of the deposition chamber to 600 ℃ at a rate of 10 ℃ / min and keep it warm for 10 min. Turn on the RF power supply, adjust the RF power to 350 W, control the working pressure to 50 Pa, bombard the surface of the aluminum foil with plasma discharge for 10 min, then stop introducing nitrogen, introduce ethylene, control the flow rate to 50 ml / min, the working pressure is 50 Pa, and the deposition time is 60 min. After the deposition is completed, stop introducing ethylene, introduce nitrogen, the flow rate is 20 ml / min, turn off the heating system and RF power supply, maintain the pressure in the tube, and cool down to room temperature.

[0042] The surface coating of the aluminum foil prepared in Example 1 was analyzed by SEM and Raman spectroscopy. Figure 1 and Figure 2 As shown, the surface of the aluminum foil current collector on which the low-temperature grown vertical graphene is prepared has a clean vertical graphene structure and exhibits clear characteristic peaks.

[0043] Embodiment 2: This embodiment provides a method for preparing an aluminum foil current collector for low-temperature growth of vertical graphene, comprising the following steps: The aluminum foil current collector with a thickness of 16 μm was ultrasonically cleaned with ethanol solution for 15 min, repeated three times, and then blown dry with a nitrogen flow.

[0044] Place the dried aluminum foil in the PECVD deposition chamber, start the mechanical pump group, slowly open the vacuum system, pump the pressure in the chamber to below 0 Pa, turn off the mechanical pump, and introduce nitrogen (50 ml / min). After repeating the operation three times, raise the temperature of the deposition chamber to 500°C at a rate of 10°C / min and keep it warm for 10 min. Turn on the RF power supply, adjust the RF power to 350 W, control the working pressure to 50 Pa, bombard the surface of the aluminum foil with plasma discharge for 10 min, then stop introducing nitrogen, introduce ethylene, control the flow rate to 50 ml / min, the working pressure is 50 Pa, and the deposition time is 20 min. After the deposition is completed, stop introducing ethylene, introduce nitrogen, the flow rate is 20 ml / min, turn off the heating system and RF power supply, maintain the pressure in the tube, and cool down to room temperature.

[0045] The surface coating of the aluminum foil prepared in Example 2 was analyzed by SEM and Raman spectroscopy. Figure 3 and Figure 4 As shown, the surface of the aluminum foil current collector on which the low-temperature grown vertical graphene is prepared has a clean vertical graphene structure and exhibits clear characteristic peaks.

[0046] Embodiment 3, this embodiment provides a method for preparing an aluminum foil current collector for low-temperature growth of vertical graphene, comprising the following steps: The aluminum foil current collector with a thickness of 20 μm was ultrasonically cleaned with acetone solution for 15 min, repeated three times, and then blown dry with a nitrogen flow.

[0047] Place the dried aluminum foil in the PECVD deposition chamber, start the mechanical pump group, slowly open the vacuum system, pump the pressure in the chamber to below 0 Pa, turn off the mechanical pump, and introduce nitrogen (50 ml / min). After repeating the operation three times, raise the temperature of the deposition chamber to 600 °C at a rate of 10 °C / min and keep it warm for 10 min. Turn on the RF power supply, adjust the RF power to 350 W, control the working pressure to 50 Pa, bombard the surface of the aluminum foil with plasma discharge for 10 min, then stop introducing nitrogen, introduce ethylene, control the flow rate to 50 ml / min, the working pressure is 50 Pa, and the deposition time is 20 min. After the deposition is completed, stop introducing ethylene, introduce nitrogen, the flow rate is 20 ml / min, turn off the heating system and RF power supply, maintain the pressure in the tube, and cool down to room temperature.

[0048] The surface coating of the aluminum foil prepared in Example 3 was analyzed by SEM and Raman spectroscopy. Figure 5 and Figure 6 As shown, the surface of the aluminum foil current collector on which the low-temperature grown vertical graphene is prepared has a clean vertical graphene structure and exhibits clear characteristic peaks.

[0049] Embodiment 4: This embodiment provides a method for preparing an aluminum foil current collector for low-temperature growth of vertical graphene, comprising the following steps: The aluminum foil current collector with a thickness of 10 μm was ultrasonically cleaned with acetone solution for 15 min, repeated three times, and then blown dry with a nitrogen flow.

[0050] Place the dried aluminum foil in the PECVD deposition chamber, start the mechanical pump group, slowly open the vacuum system, pump the pressure in the chamber to below 0 Pa, turn off the mechanical pump, and introduce nitrogen (50 ml / min). After repeating the operation three times, raise the temperature of the deposition chamber to 600 °C at a rate of 10 °C / min and keep it warm for 10 min. Turn on the RF power supply, adjust the RF power to 350 W, control the working pressure to 50 Pa, bombard the surface of the aluminum foil with plasma discharge for 10 min, then stop introducing nitrogen, introduce propylene, control the flow rate to 50 ml / min, the working pressure is 50 Pa, and the deposition time is 60 min. After the deposition is completed, stop introducing propylene, introduce nitrogen, the flow rate is 20 ml / min, turn off the heating system and RF power supply, maintain the pressure in the tube, and cool down to room temperature.

[0051] The surface coating of the aluminum foil prepared in Example 4 was analyzed by SEM and Raman spectroscopy. Figure 7 and Figure 8 As shown, the surface of the aluminum foil current collector on which the low-temperature grown vertical graphene is prepared has a clean vertical graphene structure and exhibits clear characteristic peaks.

[0052] Comparative Example The aluminum foil deposition in this comparative example was carried out under conventional chemical vapor deposition conditions, without plasma assistance during the deposition process, and the deposition temperature was correspondingly increased to 800° C. The specific operation steps are as follows: The aluminum foil current collector with a thickness of 20 μm was ultrasonically cleaned with acetone solution for 15 min, repeated three times, and then blown dry with a nitrogen flow.

[0053] Place the dried aluminum foil in the PECVD deposition chamber, start the mechanical pump group, slowly open the vacuum system, pump the pressure in the chamber to below 0 Pa, turn off the mechanical pump, and introduce nitrogen (50 ml / min). After repeating the operation three times, raise the temperature of the deposition chamber to 800 °C at a rate of 10 °C / min, stop introducing nitrogen, introduce ethylene, and control the flow rate to 50 ml / min. The working pressure is 500 Pa, and the deposition time is 20 min. After the deposition is completed, stop introducing ethylene, introduce nitrogen, and the flow rate is 20 ml / min. Turn off the heating system, maintain the pressure in the tube, and cool it down to room temperature.

[0054] Since the deposition temperature of 800 °C is higher than the melting point of aluminum foil, the aluminum foil breaks and differentiates during the deposition process, and the deposition cannot be completed.

[0055] In summary, the preparation method of the aluminum foil current collector for low-temperature grown vertical graphene of the present invention changes the traditional graphene coating to deposit and grow vertical graphene on the surface of the aluminum foil under a low-temperature environment, and can form a good bonding force with the aluminum foil without the assistance of a catalyst. At the same time, the vertical graphene has the characteristics of vertical orientation and non-stacking morphology. Its special non-stacking morphology can greatly increase the roughness of the aluminum foil surface, improve the contact between the active material and the aluminum foil, reduce the resistance of the aluminum foil, and improve the performance of the sodium ion battery.

[0056] Although this patent document contains many details, they should not be construed as limitations on the scope of any invention or claim, but rather as descriptions of features of particular embodiments of particular inventions. Certain features described in this patent document in the context of separate embodiments may also be implemented in combination in a single embodiment. Conversely, various features described in the context of a single embodiment may also be implemented in multiple embodiments separately or in any suitable subcombination.

[0057] Furthermore, while the features described above may be described as acting in certain combinations, or even initially claimed as such, in certain cases one or more features of the claimed combinations may be removed from the combination, and the claimed combinations may be directed to sub-combinations or variations of sub-combinations.

[0058] This patent document describes only some implementations and examples, and other implementations, enhancements, and variations may be made based on what is described and illustrated in this patent document.

Claims

1. A method for preparing an aluminum foil current collector for low-temperature growth of vertical graphene, characterized in that: The following steps are involved: Step S1, performing surface pretreatment on the aluminum foil current collector; Step S2, placing the pretreated aluminum foil current collector in a PECVD deposition chamber, and heating the PECVD deposition chamber to 500-600° C. in a vacuum environment; Step S3, introducing Ar gas at a flow rate of 2-5 ml / min, and turning on the plasma generator after the pressure in the PECVD deposition chamber is stabilized to bombard and clean the surface of the aluminum foil current collector; Step S4, after stopping the introduction of Ar gas, introducing a carbon source gas, and growing vertical graphene on the surface of the aluminum foil current collector by chemical vapor deposition at 500-600° C.; Step S5, stop introducing the carbon source gas, introduce the protective gas, cool down to room temperature under low pressure, and obtain an aluminum foil current collector for low-temperature growth of vertical graphene.

2. The method for preparing the aluminum foil current collector for low temperature growth of vertical graphene according to claim 1, characterized in that: The surface pretreatment in step S1 is specifically to use acetone or ethanol to repeatedly clean the surface, and then dry it in an inert atmosphere for later use.

3. The method for preparing the aluminum foil current collector for low temperature growth of vertical graphene according to claim 1, characterized in that: The vacuum atmosphere in step S2 is less than 10 -3 Pa PECVD deposition chamber gas pressure environment.

4. The method for preparing an aluminum foil current collector for low temperature growth of vertical graphene according to claim 1, characterized in that: In step S3, the radio frequency power of the plasma generator is 300-400 W, and the bombardment cleaning time is 5-15 min.

5. The method for preparing the aluminum foil current collector for low temperature growth of vertical graphene according to claim 1, characterized in that: In step S4, the carbon source gas is any one of ethylene and propylene; The flow rate of the carbon source gas is 30-60 ml / min, the working gas pressure is 20-60 Pa, and the deposition time is 20-60 min.

6. The method for preparing an aluminum foil current collector for low temperature growth of vertical graphene according to claim 1, characterized in that: The protective gas in step S5 is any one of nitrogen and argon; The flow rate of the protective gas is 20-40 ml / min.

7. An aluminum foil current collector for low-temperature growth of vertical graphene, characterized in that: The method is prepared by the method according to any one of claims 1 to 6.

8. The method for preparing an aluminum foil current collector for low temperature growth of vertical graphene according to claim 7, characterized in that: The growth density of the vertical graphene is 0.002-0.008 g / cm 2 .

9. The method for preparing an aluminum foil current collector for low temperature growth of vertical graphene according to claim 7, characterized in that: The thickness of the vertical graphene is 400-800 nm.

10. Application of the aluminum foil current collector of low temperature grown vertical graphene as claimed in any one of claims 7 to 9 in the field of sodium ion batteries.

Citation Information

Cited By

  • High-texture oriented aluminum foil current collector material and preparation method thereof

    CN121601556A

  • A high texture oriented aluminum foil current collector material and a method of making the same

    CN121601556B