Heterogeneous palladium-palladium phosphide nanobelt oxygen reduction electrocatalyst and preparation method thereof
By preparing a heterogeneous palladium-palladium phosphide nanoribbon structure by combining ultrasonic and roasting methods, using polyvinylpyrrolidone and phosphorus atoms, the problem of poor catalytic activity of palladium-based nanostructures in fuel cells was solved, and efficient oxygen ionization was achieved. Improved reduction reaction performance and stability.
Patent Information
- Application Number
- CN202410768443.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-15
AI Technical Summary
Existing palladium-based nanostructures have poor catalytic activity in fuel cells, and due to excessive particle size, the specific surface area is reduced, making it difficult to be effectively used in oxygen reduction reactions.
It adopts a heterogeneous palladium-palladium phosphide nanoribbon structure, which is a combination of ribbon-shaped palladium metallocene and palladium phosphide metallocene. It is prepared by ultrasonic method and roasting method. Polyvinylpyrrolidone is used as a surfactant and phosphorus atoms are introduced to reduce oxygen content. The adsorption of intermediates improves catalytic performance.
It achieves the provision of highly active sites and improvement of catalytic activity, avoids the reduction of specific surface area caused by excessive palladium phosphide particle size, and significantly improves the electrochemical activity and stability of the oxygen reduction reaction.
Smart Images

Figure CN118782815A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a heterogeneous palladium-palladium phosphide nanobelt oxygen reduction electrocatalyst and a controllable preparation method thereof. The catalyst can be applied to electrocatalytic oxygen reduction reaction. Background Art
[0002] Fuel cells, as a relatively new type of energy conversion device, have attracted much attention due to their high energy density and clean and sustainable superior characteristics. In fuel cells, platinum-based nanostructures have high catalytic performance for anodic oxidation and cathode reduction reactions (such as oxygen reduction reactions). However, the high price of platinum-based materials limits their large-scale application in fuel cells. In addition, platinum-based materials are easy to poison and agglomerate, which leads to a reduction in their active sites and reduces their catalytic activity. Based on the above problems, a large number of researchers have conducted research. Using palladium-based nanostructures with stronger anti-poisoning ability and electronic structure similar to platinum to replace platinum as a catalyst is one of the effective ways to solve this problem. However, palladium-based nanostructures have strong adsorption of oxygen-containing intermediates, resulting in active sites being occupied and poor catalytic activity. Modification by introducing non-metallic elements into palladium-based nanostructures can effectively reduce adsorption and improve catalytic activity.
[0003] At present, a large number of palladium-based nanostructures have been successfully prepared. Metalloene is a new type of two-dimensional nanostructure with atomic-level thickness and special morphology (ribbon, sheet, petal, etc.), which has a high specific surface area and the number of active sites, greatly improving the catalytic activity. The introduction of non-metallic elements to modify palladium metalloene has also achieved many results, such as boron doping, nitrogen doping and phosphating. Generally, the solvothermal method is used to achieve the doping of non-metallic elements, and the calcination method is used to achieve the preparation of palladium-non-metallic element compounds. By introducing non-metallic elements, the electronic structure of palladium can be adjusted and the lattice expansion can be induced, the d-band center can be reduced, thereby promoting the desorption of oxygen-containing intermediates and improving the catalytic activity. For palladium phosphide prepared by calcination, the specific surface area may be reduced due to the increase in particle size. This situation can be avoided by preparing palladium-palladium phosphide heterostructure catalysts.
[0004] In summary, the preparation of palladium-based nanomaterials by combining the advantages of palladium metalloene, introduction of non-metallic elements and heterogeneous structures is a valuable and promising method, which can greatly improve the catalytic activity and utilization rate of palladium-based catalysts. It is reported that pure palladium phosphide nanostructured catalysts have a lower electrochemically active specific surface area relative to palladium black due to their large particle size, so it is urgent to develop a new approach to better design palladium-palladium phosphide catalysts with higher specific surface area and stronger activity. Summary of the invention
[0005] In order to overcome the shortcomings of the prior art, the present invention aims to provide a heterogeneous palladium-palladium phosphide nanobelt oxygen reduction electrocatalyst and its preparation method, and to study the electrocatalytic oxygen reduction reaction. The catalyst structure is composed of a band-shaped palladium metal olefin and a palladium phosphide metal olefin. The unique structure of the band metal olefin can provide a large number of active sites, and the introduced phosphorus atoms can reduce the adsorption of oxygen-containing intermediates, thereby enhancing the catalytic performance. This work provides a reference for embedding non-metallic elements into metal elements to develop promising oxygen reduction electrocatalysts.
[0006] The technical solution adopted by the present invention is:
[0007] A heterogeneous palladium-palladium phosphide nanobelt oxygen reduction electrocatalyst is prepared by the following method:
[0008] 1) Prepare sodium chloropalladate solutions with concentrations between 50 and 100 mM respectively;
[0009] 2) Mix 300-800 mg of polyvinyl pyrrolidone and 50-100 mg of ascorbic acid with 1-3 mL of ethylenediamine, and sonicate at 20-50° C. for 30-60 minutes until completely dissolved; add 30-100 mg of molybdenum hexacarbonyl, continue sonicating for 30-60 minutes until completely dissolved, add 0.1-0.2 mL of sodium chloropalladate solution, and sonicate until the system is uniform;
[0010] 3) reacting the solution obtained in step 2) at 100-150° C. for 5-10 hours, centrifuging and washing to obtain a ribbon-shaped palladium metal olefin precursor, and drying the product at room temperature for 12-36 hours;
[0011] 4) 5-20 mg of a ribbon-shaped palladium metal olefin precursor and 20-50 mg of sodium hypophosphite are placed in a porcelain boat, heated to 260-350° C. at a heating rate of 2-5° C. / min in a tube furnace, kept warm for 1-3 hours, and then cooled to obtain a heterogeneous palladium-palladium phosphide nanobelt.
[0012] Different reaction conditions have an important influence on the structure of the heterogeneous palladium-palladium phosphide nanobelts. The surfactant polyvinyl pyrrolidone plays a very important role in the preparation of heterogeneous palladium-palladium phosphide nanobelts. Different crystal faces of the palladium precursor have different adsorption capacities for polyvinyl pyrrolidone. Some crystal faces are not covered by the migrated palladium atoms due to the adsorption of more polyvinyl pyrrolidone. Therefore, during the addition of palladium atoms, it can effectively guide the synthesis of the palladium nanobelt structure.
[0013] The present invention also relates to a method for preparing heterogeneous palladium-palladium phosphide nanobelts, the method comprising the following steps:
[0014] 1) Prepare sodium chloropalladate solutions with concentrations between 50 and 100 mM respectively;
[0015] 2) Mix 300-800 mg of polyvinyl pyrrolidone and 50-100 mg of ascorbic acid with 1-3 mL of ethylenediamine, and sonicate at 20-50° C. for 30-60 minutes until completely dissolved; add 30-100 mg of molybdenum hexacarbonyl, continue sonicating for 30-60 minutes until completely dissolved, add 0.1-0.2 mL of sodium chloropalladate solution, and sonicate until the system is uniform;
[0016] 3) reacting the solution obtained in step 2) at 100-150° C. for 5-10 hours, centrifuging and washing to obtain a ribbon-shaped palladium metal olefin precursor, and drying the product at room temperature for 12-36 hours;
[0017] 4) 5-20 mg of a strip-shaped palladium metal olefin precursor and 20-50 mg of sodium hypophosphite are placed in a porcelain boat, heated to 260-350° C. at a heating rate of 2-5° C. / min in a tubular furnace, kept warm for 1-3 hours, and cooled to obtain heterogeneous palladium-palladium phosphide nanobelts. The concentration and volume of sodium chloropalladate and ascorbic acid, the type and volume of the surfactant, and the reaction time and temperature are further controlled to control the structure and morphology of the palladium catalyst.
[0018] The electrochemical catalytic oxygen reduction reaction is carried out under normal temperature and pressure conditions. The specific test operation process is as follows:
[0019] (1) 0.1 mL of Nafion solution (0.5 wt%), 0.2 mL of anhydrous ethanol, and 0.7 mL of ultrapure water were measured to prepare a mixed solution;
[0020] (2) Weigh 2-10 mg of sample and disperse it in the above mixed solution. Ultrasonicate for 40 minutes to obtain a uniform dispersion. Take 2-5 μL of the dispersion and evenly drop it on the surface of the rotating disk electrode. After completely drying at 45° C., it is made into a working electrode. Together with a silver / silver chloride electrode as a reference electrode and a platinum wire electrode as a counter electrode, a three-electrode system is formed to carry out an oxygen reduction reaction test.
[0021] (3) Before the test, add 0.1M potassium hydroxide solution into the electrolytic cell, and continue to pass oxygen for 30 minutes to saturate the solution with oxygen. Debug and select the programs of linear sweep voltammetry and cyclic voltammetry, and use a computer to monitor the current data of the working electrode at different scan rates in real time. Based on the measured data and related formulas, calculate the Tafel slope and electron transfer number to evaluate the oxygen reduction performance of the catalyst.
[0022] The beneficial effects of the heterogeneous palladium-palladium phosphide nano-charged catalyst and the preparation method thereof provided by the present invention are mainly reflected in:
[0023] (1) The preparation process is simple and clear. Polyvinyl pyrrolidone surfactant is rationally used as a soft template. Carbon monoxide provided by molybdenum hexacarbonyl guides the growth of palladium atoms. The synthesized palladium metal olefin has a uniform morphology and a yield of nearly 100%.
[0024] (2) The palladium metal olefin is partially phosphated, thereby avoiding the problem of excessively large particle size of palladium phosphide and optimizing the catalytic activity of the catalyst.
[0025] (3) The synthesized heterogeneous palladium-palladium phosphide nanobelt electrocatalyst showed excellent activity and stability in the oxygen reduction reaction. Palladium-based materials have broad application prospects as electrocatalysts for oxygen reduction reactions. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 These are SEM images of heterogeneous palladium-palladium phosphide nanobelts according to specific embodiment 1 of the present invention, wherein (a) represents the SEM image of the heterogeneous palladium-palladium phosphide nanobelt, and (b) represents the SEM image of the heterogeneous palladium-palladium phosphide nanobelt in another area.
[0027] Figure 2 These are the TEM and HRTEM images of the heterogeneous palladium-palladium phosphide nanobelt according to the specific embodiment 1 of the present invention, wherein (a) represents the HRTEM image of the heterogeneous palladium-palladium phosphide nanobelt, and (b) represents the TEM image of the heterogeneous palladium-palladium phosphide nanobelt.
[0028] Figure 3 This is the XPS graph of the heterogeneous palladium-palladium phosphide nanobelt according to the specific embodiment 1 of the present invention, wherein (a) represents the XPS graph of the Pd element, and (b) represents the XPS graph of the P element.
[0029] Figure 4 This is the XRD diagram of the heterogeneous palladium-palladium phosphide nanobelt according to specific embodiment 1 of the present invention.
[0030] Figure 5 The linear sweep voltammetry curve of the heterogeneous palladium-palladium phosphide nanobelt at 1600 rpm and the Tafel slope diagram of the specific embodiment 1 of the present invention, wherein (a) represents the linear sweep voltammetry curve of the heterogeneous palladium-palladium phosphide nanobelt at 1600 rpm, and (b) represents the Tafel slope diagram of the heterogeneous palladium-palladium phosphide nanobelt.
[0031] Figure 6 This is the linear scanning voltammetry curve of the heterogeneous palladium-palladium phosphide nanobelt at different rotational speeds and the transfer electron number diagram of the specific embodiment 1 of the present invention, wherein (a) represents the linear scanning voltammetry curve of the heterogeneous palladium-palladium phosphide nanobelt at different rotational speeds, and (b) represents the transfer electron number diagram of the heterogeneous palladium-palladium phosphide nanobelt.
[0032] Figure 7The linear sweep voltammetry curve of the heterogeneous palladium-palladium phosphide nanobelt before and after 5000 cycles and the polarographic current-time curve diagram of the specific embodiment 1 of the present invention, wherein (a) represents the linear sweep voltammetry curve of the heterogeneous palladium-palladium phosphide nanobelt before and after 5000 cycles, and (b) represents the polarographic current-time curve diagram of the heterogeneous palladium-palladium phosphide nanobelt.
[0033] Figure 8 This is a SEM image of dendritic palladium-palladium phosphide according to specific embodiment 2 of the present invention.
[0034] Fig. 9 This is a TEM image of dendritic palladium-palladium phosphide according to specific embodiment 2 of the present invention.
[0035] Fig.10 The linear sweep voltammetry curve of dendritic palladium-palladium phosphide at 1600 revolutions and the Tafel slope diagram of specific embodiment 2 of the present invention, wherein (a) represents the linear sweep voltammetry curve of dendritic palladium-palladium phosphide at 1600 revolutions, and (b) represents the Tafel slope diagram of dendritic palladium-palladium phosphide.
[0036] Fig.11 This is a SEM image of the palladium-palladium phosphide flake according to the specific embodiment 3 of the present invention.
[0037] Fig.12 This is a TEM image of the palladium-palladium phosphide flake according to the specific embodiment 3 of the present invention.
[0038] Fig.13 The present invention is a specific embodiment 3 of the present invention, the linear sweep voltammetry curve of flake palladium-palladium phosphide at 1600 revolutions, and the Tafel slope diagram, wherein (a) represents the linear sweep voltammetry curve of flake palladium-palladium phosphide at 1600 revolutions, and (b) represents the Tafel slope diagram of flake palladium-palladium phosphide. DETAILED DESCRIPTION
[0039] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:
[0040] Reference Figures 1 to 10 In this embodiment, the oxygen reduction reaction performance test of the palladium nanobelt material is carried out on a CHI760D electrochemical workstation, and the operation process is as follows:
[0041] In the first step, 0.1 mL of Nafion solution (0.5 wt%), 0.2 mL of anhydrous ethanol and 0.7 mL of ultrapure water were measured to prepare a mixed solution;
[0042] In the second step, 5 mg of the sample was weighed and dispersed in the above-mentioned mixed solution, and a uniform dispersion was obtained by ultrasonication for 40 minutes. 2.5 μL of the dispersion was evenly dropped on the surface of the rotating disk electrode, and completely dried at 45°C to form a working electrode, which was combined with a silver / silver chloride electrode as a reference electrode and a platinum wire electrode as a counter electrode to form a three-electrode system for oxygen reduction reaction testing.
[0043] The third step is to add 0.1M potassium hydroxide solution to the electrolytic cell before the test begins, and continue to pass oxygen for 30 minutes to saturate the solution with oxygen. Then, the linear sweep voltammetry and cyclic voltammetry programs are debugged and selected, and the current data of the working electrode at different scan rates is monitored in real time by a computer. Based on the measured data and related formulas, the Tafel slope and electron transfer number are calculated to evaluate the oxygen reduction performance of the catalyst.
[0044] Embodiment 1:
[0045] A method for preparing a heterogeneous palladium-palladium phosphide nanobelt, the method comprising the following steps:
[0046] 1) Prepare a sodium chloropalladate solution with a concentration of 80 mM;
[0047] 2) Mix 600 mg of polyvinyl pyrrolidone and 80 mg of ascorbic acid with 2 mL of ethylenediamine, and sonicate at 30° C. for 40 minutes until completely dissolved; add 50 mg of molybdenum hexacarbonyl, continue sonicating for 40 minutes until completely dissolved, add 0.15 mL of sodium chloropalladate solution, and sonicate until the system is uniform;
[0048] 3) reacting the solution obtained in step 2) at 120° C. for 6 hours, centrifuging and washing to obtain a strip-shaped palladium metal olefin precursor, and drying the product at room temperature for 24 hours;
[0049] 4) 10 mg of palladium metal olefin precursor and 30 mg of sodium hypophosphite were placed in a porcelain boat, heated to 300° C. at a heating rate of 3° C. / min in a tube furnace, kept at this temperature for 2 hours, and cooled to obtain the final product, heterogeneous palladium-palladium phosphide nanobelt catalyst.
[0050] The SEM images of the heterogeneous palladium-palladium phosphide nanobelts obtained are shown in Figure 1 The obtained TEM and HRTEM images of heterogeneous Pd-PdP nanobelts are shown in Figure 2 The XPS images of heterogeneous palladium-palladium phosphide nanobelts are shown in Figure 3 The XRD pattern of the heterogeneous palladium-palladium phosphide nanobelts obtained is shown in Figure 4 The obtained linear sweep voltammetric curve of heterogeneous Pd-PdP nanobelt at 1600 rpm, the Tafel slope is shown in Figure 5 The linear sweep voltammetry curves and electron transfer numbers at different speeds can be found in Figure 6. The linear sweep voltammetric curve before and after 5000 revolutions, and the polarographic current-time curve refer to Figure 7 .
[0051] It can be seen from the SEM image that the heterogeneous palladium-palladium phosphide nanobelt is a uniform ribbon structure, and the yield of the heterogeneous palladium-palladium phosphide nanobelt is close to 100%. Through the fast Fourier transform analysis of the TEM image, lattice fringes with different spacing can be found. Through HRTEM, XPS and XRD analysis, it is proved that there are face-centered cubic palladium nanobelt structure and palladium-palladium phosphide heterostructure. The existence of zero-valent palladium and divalent palladium through XPS analysis proves that the sodium chloropalladate precursor input has been reduced to a metallic state, and the presence of phosphorus is also determined, confirming the successful introduction of the phosphorus element. It can be seen from the linear scanning voltammetry curve that in the catalytic oxygen reduction reaction, the heterogeneous palladium-palladium phosphide nanobelt has a higher starting potential (1.05V vs.RHE) and half-wave potential (0.96Vvs.RHE). The Tafel slope calculated according to the above curve is 45.3mV dec -1 , proving that the transfer of the first electron in the oxygen reduction process is the rate-controlling step. The number of transferred electrons was calculated based on the linear sweep voltammetry curves at different speeds, and the two confirmed that the reaction was four-electron. The linear sweep voltammetry curves before and after 5000 cycles confirmed that the heterogeneous palladium-palladium phosphide nanobelts have high stability.
[0052] Embodiment 2:
[0053] A method for preparing a dendritic palladium-palladium phosphide oxygen reduction catalyst, the method comprising the following steps:
[0054] 1) Prepare a 50 mM sodium chloropalladate solution;
[0055] 2) Mix 300 mg of polyvinyl pyrrolidone and 50 mg of ascorbic acid with 1 mL of ethylenediamine, and sonicate at 20° C. for 30 minutes until completely dissolved; add 30 mg of molybdenum hexacarbonyl, continue sonicating for 30 minutes until completely dissolved, add 0.1 mL of sodium chloropalladate solution, and sonicate until the system is uniform;
[0056] 3) reacting the solution obtained in step 2) at 100° C. for 5 hours, centrifuging and washing to obtain a palladium precursor, and drying the product at room temperature for 12 hours;
[0057] 4) 5 mg of palladium precursor and 20 mg of sodium hypophosphite were placed in a porcelain boat, heated to 260° C. at a heating rate of 2° C. / min in a tube furnace, kept at this temperature for 1 hour, and cooled to obtain the final product, a dendritic palladium-palladium phosphide catalyst.
[0058] The SEM image of the obtained dendritic palladium-palladium phosphide is shown in Figure 8 The TEM image of the obtained dendritic palladium-palladium phosphide is shown in Fig. 9 The linear sweep voltammetric curve and Tafel slope of the dendritic palladium-palladium phosphide at 1600 rpm are shown in Fig.10 .
[0059] From the SEM and TEM images, it can be seen that the catalyst has a dendritic structure. From the linear scanning voltammetry curve, it can be seen that the dendritic palladium-phosphide palladium has a higher starting potential (1.03V vs. RHE) and half-wave potential (0.95V vs. RHE) in the catalytic oxygen reduction reaction. The Tafel slope calculated from the above curve is 63.1mV dec. -1 , demonstrating that the transfer of the first electron is the rate-determining step in the oxygen reduction process.
[0060] Embodiment 3:
[0061] A method for preparing a flaky palladium-palladium phosphide oxygen reduction catalyst, the method comprising the following steps:
[0062] 1) Prepare a 100 mM sodium chloropalladate solution;
[0063] 2) 800 mg of polyvinyl pyrrolidone and 100 mg of ascorbic acid were mixed with 3 mL of ethylenediamine, and ultrasonicated at 50° C. for 60 minutes until completely dissolved; 100 mg of molybdenum hexacarbonyl was added, and ultrasonicated for another 60 minutes until completely dissolved; 0.2 mL of sodium chloropalladate solution was added, and ultrasonicated until the system was uniform;
[0064] 3) reacting the solution obtained in step 2) at 150° C. for 10 hours, centrifuging and washing to obtain a palladium precursor, and drying the product at room temperature for 36 hours;
[0065] 4) 20 mg of palladium precursor and 50 mg of sodium hypophosphite were placed in a porcelain boat, heated to 350° C. at a heating rate of 5° C. / min in a tube furnace, kept at this temperature for 3 hours, and cooled to obtain the final product, a palladium-palladium phosphide catalyst in the form of a flake.
[0066] The SEM image of the obtained palladium-phosphide flakes is shown in Fig.11 The TEM image of the obtained palladium-palladium phosphide flakes is shown in Fig.12 The linear sweep voltammetric curve and Tafel slope of the obtained flake palladium-palladium phosphide at 1600 rpm are shown in Fig.13 .
[0067] From the SEM and TEM images, it can be seen that the obtained catalyst has a flake structure. From the linear scanning voltammetry curve, it can be seen that in the catalytic oxygen reduction reaction, the flake palladium-palladium phosphide has a higher starting potential (1.01V vs.RHE) and half-wave potential (0.92V vs.RHE). The Tafel slope calculated from the above curve is 55.1mV dec -1, demonstrating that the transfer of the first electron is the rate-determining step in the oxygen reduction process.
Claims
1. A heterogeneous palladium-palladium phosphide nanobelt oxygen reduction electrocatalyst prepared by the following method: 1) Prepare sodium chloropalladate solutions with concentrations between 50 and 100 mM respectively; 2) Mix 300-800 mg of polyvinyl pyrrolidone and 50-100 mg of ascorbic acid with 1-3 mL of ethylenediamine, and sonicate at 20-50° C. for 30-60 minutes until completely dissolved; add 30-100 mg of molybdenum hexacarbonyl, continue sonicating for 30-60 minutes until completely dissolved, add 0.1-0.2 mL of sodium chloropalladate solution, and sonicate until the system is uniform; 3) reacting the solution obtained in step 2) at 100-150° C. for 5-10 hours, centrifuging and washing to obtain a ribbon-shaped palladium metal olefin precursor, and drying the product at room temperature for 12-36 hours; 4) 5-20 mg of a ribbon-shaped palladium metal olefin precursor and 20-50 mg of sodium hypophosphite are placed in a porcelain boat, heated to 260-350° C. at a heating rate of 2-5° C. / min in a tube furnace, kept warm for 1-3 hours, and then cooled to obtain a heterogeneous palladium-palladium phosphide nanobelt.
2. A method for preparing the heterogeneous palladium-palladium phosphide nanobelt oxygen reduction electrocatalyst as claimed in claim 1, characterized in that: The method comprises the following steps: 1) Prepare sodium chloropalladate solutions with concentrations between 50 and 100 mM respectively; 2) Mix 300-800 mg of polyvinyl pyrrolidone and 50-100 mg of ascorbic acid with 1-3 mL of ethylenediamine, and sonicate at 20-50° C. for 30-60 minutes until completely dissolved; add 30-100 mg of molybdenum hexacarbonyl, continue sonicating for 30-60 minutes until completely dissolved, add 0.1-0.2 mL of sodium chloropalladate solution, and sonicate until the system is uniform; 3) reacting the solution obtained in step 2) at 100-150° C. for 5-10 hours, centrifuging and washing to obtain a ribbon-shaped palladium metal olefin precursor, and drying the product at room temperature for 12-36 hours; 4) 5-20 mg of a ribbon-shaped palladium metal olefin precursor and 20-50 mg of sodium hypophosphite are placed in a porcelain boat, heated to 260-350° C. at a heating rate of 2-5° C. / min in a tube furnace, kept warm for 1-3 hours, and then cooled to obtain a heterogeneous palladium-palladium phosphide nanobelt.
3. The preparation method according to claim 2, characterized in that: The morphology and structure of the heterogeneous palladium-palladium phosphide nanobelt oxygen reduction electrocatalyst can be controlled by controlling the concentration and volume of sodium chloropalladate, ascorbic acid and polyvinyl pyrrolidone, as well as the temperature and time of the reaction.