Method for preparing spherical solid electrolyte
Through spray drying and heat treatment technology, the problem of particle size and shape control of sulfide-based solid electrolytes during the drying process was solved, and a sulfide-based solid electrolyte with a spherical shape and uniform particle size distribution was obtained, improving its density and lithium ion conductivity.
Patent Information
- Application Number
- CN202311677236.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-07
- Filing Date
- 2023-12-08
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult to control the particle size distribution and shape of existing sulfide-based solid electrolytes during the drying process, resulting in particle deformation, composition ratio changes and viscosity instability, which affects their dispersibility in production slurries.
The sulfide-based solid electrolyte is prepared using spray drying technology. The starting raw materials are sprayed into the spray dryer through a nozzle atomizer. The pressure and temperature inside the chamber are controlled to obtain an intermediate with a spherical shape and uniform particle size distribution, which is further optimized through heat treatment. its structure.
The spherical shape and uniform particle size distribution of the sulfide-based solid electrolyte are achieved, its tap density and particle compaction density are improved, and the lithium ion conductivity of the electrode and solid electrolyte layer is enhanced.
Smart Images

Figure CN118782889A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing a solid electrolyte having a uniform particle size distribution and a spherical shape. Background Art
[0002] The particle shape of sulfide-based solid electrolytes varies depending on drying time, temperature, and pressure. For example, since the evaporation amount of sulfur in the precursor solution increases with the increase of drying time, it may be difficult to control the particle size distribution and shape of the sulfide-based solid electrolyte. Therefore, it is necessary to design a method to minimize sulfur loss by drying in a short time within a suitable temperature range.
[0003] On the other hand, when the sulfide-based solid electrolyte comes into contact with moisture and / or oxygen, its oxidation reaction occurs very quickly, which causes deformation of particles of the sulfide-based solid electrolyte and changes in the composition ratio.
[0004] Therefore, in the sulfide-based solid electrolyte synthesized by the general method, there is a mixture of spherical particles and plate-shaped particles, and fine-grained powders and large-grained powders are also mixed. When a sulfide-based solid electrolyte whose particle size and shape are not controlled as described above is used to produce a slurry, the viscosity may change over time, which in turn may lead to poor dispersibility of the components. Summary of the invention
[0005] An object of the present invention is to provide a method for preparing a sulfide-based solid electrolyte having a spherical shape and a uniform particle size distribution.
[0006] The object of the present invention is not limited to the above-mentioned object. The object of the present invention will become more apparent from the following description and will be achieved by the means and combinations thereof described in the claims.
[0007] The method for preparing a solid electrolyte according to the present invention may include: preparing a raw material containing at least one selected from lithium (Li) element, phosphorus (P) element, sulfur (S) element and a combination thereof; preparing a starting material containing the raw material and a solvent; obtaining an intermediate in the form of a powder by spray drying the starting material; and obtaining a sulfide-based solid electrolyte by heat treating the intermediate.
[0008] The raw materials may include Li 2 S and P 2 S 5The raw material may further include a lithium compound containing a halogen element. The solvent may include tetrahydrofuran (THF). The starting raw material may have a solid content in an amount of 10 wt % to 30 wt %.
[0009] Obtaining the intermediate can include spraying the starting material into the chamber of the spray dryer by a nozzle atomizer. The evaporation amount of the chamber can be in the range of 1kg / hour to 4kg / hour. Obtaining the intermediate can include spraying the starting material into the chamber with a spray amount of 50ml / minute to 70ml / minute. The internal pressure of the chamber can be in the range of 1.3 atmospheric pressures (atm) to 1.5 atmospheric pressures (atm).
[0010] The spray dryer may include: a chamber defining an interior space of a particular size; a nozzle atomizer connected to the chamber to spray the starting material; a first compressor connected to the nozzle atomizer to supply a carrier gas; a second compressor connected to the chamber to supply a gas for adjusting the internal pressure of the chamber; a sensor installed in the chamber to measure the internal pressure of the chamber; an exhaust valve for exhausting the carrier gas in the chamber to the outside; and a controller connected to the second compressor and the exhaust valve to control whether to operate based on the internal pressure of the chamber measured by the sensor Second compressor and exhaust valve.
[0011] Obtaining the intermediate may be performed at a temperature of 180° C. to 240° C. Obtaining the intermediate may include spray drying the starting material for 1 second to 5 seconds. Obtaining the sulfide-based solid electrolyte may include heat treating the intermediate at a temperature of 300° C. to 500° C. for 12 hours to 48 hours.
[0012] When the 50% cumulative mass particle size distribution diameter in the particle distribution of the sulfide-based solid electrolyte is referred to as D50, the D50 of the sulfide-based solid electrolyte may be 5 μm to 10 μm. When the 90% cumulative mass particle size distribution diameter, the 50% cumulative mass particle size distribution diameter, and the 10% cumulative mass particle size distribution diameter in the particle distribution of the sulfide-based solid electrolyte are referred to as D90, D50, and D10, respectively, the (D90-D10) / D50 of the sulfide-based solid electrolyte may be 1 to 3.
[0013] The tap density of the sulfide-based solid electrolyte may be in the range of 0.5 g / ml to 0.7 g / ml. Can be in the range of 1.65g / ml to 1.8g / ml.
[0014] According to the present invention, a sulfide-based solid electrolyte having a spherical shape and a uniform particle size distribution can be obtained.
[0015] The effects of the present invention are not limited to the aforementioned effects. It should be understood that the effects of the present invention include all effects that can be inferred from the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The above and other features of the present invention will now be described in detail with reference to specific illustrative examples of the invention shown in the accompanying drawings, which are hereinafter described by way of illustration only. The present invention is therefore not limited, and wherein:
[0017] Figure 1 An exemplary method for preparing a solid electrolyte according to the present invention is shown;
[0018] Figure 2 An embodiment of an exemplary spray dryer according to the present invention is shown;
[0019] Figure 3 An example nozzle atomizer embodiment of the present invention is shown.
[0020] Figure 4 The sulfide-based solid according to Example 1 was observed using a scanning electron microscope. Example results for electrolytes;
[0021] Figure 5 The sulfide-based solid according to Example 2 was observed using a scanning electron microscope. Example results for electrolytes;
[0022] Figure 6 The sulfide-based solid according to Example 3 was observed using a scanning electron microscope. Example results for electrolytes;
[0023] Figure 7 The sulfide-based solid according to Example 4 was observed using a scanning electron microscope. Example results for electrolytes;
[0024] Figure 8 The sulfide-based solid according to Comparative Example 1 was observed using a scanning electron microscope. Example results for electrolytes;
[0025] Fig. 9 An example showing the particle size distribution of the sulfide-based solid electrolyte according to Example 1 Measurement results;
[0026] Fig.10 An example showing the particle size distribution of the sulfide-based solid electrolyte according to Example 2 Measurement results;
[0027] Fig.11 An example showing the particle size distribution of the sulfide-based solid electrolyte according to Example 3 Measurement results;
[0028] Fig.12 An example showing the particle size distribution of the sulfide-based solid electrolyte according to Example 4 Measurement results;
[0029] Fig.13 An example showing the particle size distribution of the sulfide-based solid electrolyte according to Comparative Example 1 Measurement results;
[0030] Fig.14 are exemplary cyclic voltammetry evaluation results of the performance of all-solid-state batteries prepared using the sulfide-based solid electrolytes according to Example 1, Example 2, and Comparative Example 1;
[0031] Fig.15 Shows exemplary capacities measured when charging and discharging all-solid-state batteries prepared using the sulfide-based solid electrolytes according to Example 1, Example 2, and Comparative Example 1;
[0032] Fig.16 The sulfide-based solid electrode according to Comparative Example 5 was analyzed using a scanning electron microscope. The result of decomposition;
[0033] Fig.17 The sulfide-based solid according to Example 6 was analyzed using a scanning electron microscope. Example results for electrolytes;
[0034] Fig.18 An example showing the particle size distribution of the sulfide-based solid electrolyte according to Comparative Example 5 Measurement results;
[0035] Fig.19 Example measurement results of the particle size distribution of the sulfide-based solid electrolyte according to Comparative Example 6 are shown. DETAILED DESCRIPTION
[0036] The above-mentioned purpose, other purposes, features and advantages of the present invention will be easily understood through the following preferred embodiments in conjunction with the accompanying drawings. However, the present invention is not limited to the embodiments described herein, but can be embodied in other forms. More specifically, the embodiments introduced herein are provided to make the disclosed content thorough and complete, and to fully convey the technical ideas of the present invention to those skilled in the art.
[0037] Unless otherwise stated, all numbers, values and / or expressions used herein to represent the amount of components, reaction conditions, polymer compositions and compounds should be understood to be modified by the term "about" in all cases, because, among other things, these numbers are essentially approximations reflecting the various uncertainties of the measured values that occur when obtaining these values. Moreover, when a numerical range is disclosed in this specification, unless otherwise stated, such a range is continuous and includes all values between the minimum and maximum values (including the end values) of the range. In addition, when such a range involves integers, unless otherwise stated, all integers between the minimum and maximum values (including the end values) are also included.
[0038] Figure 1 The preparation method of the solid electrolyte according to the present invention is shown. Figure 1 , the preparation method may include: preparing a raw material containing at least one selected from lithium (Li) element, phosphorus (P) element, sulfur (S) element and a combination thereof (S10); preparing a starting material containing the raw material and a solvent (S20); obtaining an intermediate in the form of a powder by spray drying the starting material (S30); And by heat treating the intermediate, a sulfide-based solid electrolyte is obtained (S40).
[0039] Examples of sulfide-based solid electrolytes may include Li 3 PS 4 , Li 6 PS 5 Cl, Li 6 PS 5 Br, Li 6 PS 5 I etc.
[0040] The raw materials may be prepared according to the desired composition of the sulfide-based solid electrolyte (S10). For example, the raw materials may include Li 2 S and P 2 S 5 Alternatively, the raw material may further include a lithium compound containing a halogen element. Examples of the lithium compound may include LiCl, LiBr, LiI, and the like.
[0041] The starting material can be prepared by mixing the raw material with a solvent (S20).
[0042] Any solvent may be used as long as it can disperse the raw material without reacting therewith. For example, the solvent may include tetrahydrofuran (THF).
[0043] The starting raw material may have a solid content in an amount of 10 wt % to 30 wt %. If the solid content of the raw material is less than 10 wt %, the raw material may be ionized due to the polarity of the oxygen element contained in tetrahydrofuran, and thus the sulfide-based solid electrolyte as a final product may become a fine powder having a particle size of less than 1 μm and an uneven particle shape. If the solid content of the raw material exceeds 30 wt %, the amount of the solvent is reduced, and thus the dispersibility of the raw material may be reduced, and Aggregation may occur.
[0044] By spray-drying the raw material prepared as described above using a spray dryer, an intermediate in the form of powder can be obtained (S30).
[0045] Figure 2 An embodiment of a spray dryer according to the present invention is shown. The spray dryer may include: a chamber 10 having an inner space of a specific size; a tank 20 for storing starting materials; A nozzle atomizer 30 is used to spray the starting material supplied from the tank 20 into the chamber 10; a first compressor 40 is connected to the nozzle atomizer 30 to supply a carrier gas; a second compressor 50 is connected to the chamber 10 to supply a gas for adjusting the internal pressure of the chamber 10; a sensor 60 is installed on the chamber 10 to measure the internal pressure of the chamber 10; an exhaust valve 70 is used to discharge the carrier gas and the dried intermediate from the chamber 10 to the outside; a separator 80 is used to separate the raw materials discharged from the chamber 10 into the carrier gas and the intermediate; and a controller 90 is used to control whether to operate the second compressor 50 and the exhaust valve 70.
[0046] The technical feature of the present invention is that the nozzle atomizer 30 is used to prepare a sulfide-based solid electrolyte with uniform particle size. Figure 3 An embodiment of an exemplary nozzle atomizer 30 of the present invention is shown. The starting material is finely sprayed and injected into the chamber 10 from the distal end of the nozzle by a carrier gas. Since the nozzle atomizer 30 has higher dispersibility than other atomizers such as a disk atomizer, a sulfide-based solid electrolyte with uniform particle size can be obtained. In addition, in the nozzle atomizer 30, since the sprayed raw material falls vertically during the drying process, the drying time is short, and the loss of sulfur in the starting raw material can be minimized, so that a high-quality sulfide-based solid electrolyte can be obtained.
[0047] The carrier gas is not particularly limited, and examples thereof may include an inert gas such as argon.
[0048] The present invention is characterized in that the spray amount of the starting material is adjusted to prepare a spherical sulfide-based solid electrolyte. First, the starting material may have a solid content in a certain range represented by a specific numerical value as described above. In the case where the evaporation amount of the chamber 10 can be 1kg / hour to 4kg / hour, the raw material can be sprayed into the chamber 10 at a spray amount of 50ml / minute to 70ml / minute. If the spray amount exceeds 70ml / minute, the drying may not be fully completed, and residual solvent may remain. The residual solvent may be carbonized and become an impurity during the heat treatment process described later.
[0049] The present invention is characterized in that the internal pressure of the chamber 10 is kept constant to prepare a sulfide-based solid electrolyte with uniform particle size. In order to obtain an intermediate of uniform quality, the air flow rate and pressure should be kept constant throughout the spraying, drying and collection process. A positive pressure is generated in the chamber 10 by a carrier gas used to spray the starting material into the chamber 10, and when the dried intermediate is discharged through the exhaust valve 70, a negative pressure is generated inside the chamber 10. Therefore, unless the internal pressure of the chamber 10 is artificially adjusted, a sulfide-based solid electrolyte with uniform particle size cannot be obtained because the pressure conditions in the chamber 10 change at any time.
[0050] In the spray dryer according to the present invention, the controller 90 connected to the second compressor 50 and the exhaust valve 70 can operate the second compressor 50 and the exhaust valve 70 based on the internal pressure of the chamber 10 measured by the sensor 60, thereby adjusting the internal pressure of the chamber 10. Specifically, the controller 90 can adjust the internal pressure of the chamber 10 to between 1.3 atmospheres and 1.5 atmospheres. When a positive pressure greater than required is generated in the chamber 10, the controller 90 opens the exhaust valve 70 to reduce the internal pressure of the chamber 10. In addition, when a negative pressure greater than required is generated in the chamber 10, the controller 90 drives the second compressor 50 to supply gas to the chamber 10. The gas is not particularly limited, and the same gas as the carrier gas can be used.
[0051] The obtaining of the intermediate (S30) may be performed at a temperature of 180° C. to 240° C. The temperature may refer to the temperature within the chamber 10. If the temperature is lower than 180° C., the drying time may become longer, which may make it difficult (if not impossible) to obtain a sulfide-based solid electrolyte having a uniform particle size.
[0052] The obtaining of the intermediate (S30) may include spray drying the starting material for 1 second to 5 seconds. When the drying time falls within the above range, the loss of sulfur can be minimized.
[0053] The dried intermediate is discharged from the chamber 10 through the exhaust valve 70 together with the carrier gas, other gases, etc., and moves to the separator 80. Examples of the separator 80 may include any device capable of separating solids and gases. For example, the separator 80 may include a cyclone.
[0054] The intermediate separated by the separator 80 may be separately collected for heat treatment described later, and a carrier gas, other gases, etc. may be supplied to the second compressor 50 to be used as a gas for adjusting the internal pressure of the chamber 10 .
[0055] The sulfide-based solid electrolyte (S40) can be obtained by heat-treating the intermediate obtained as described above. The intermediate can be crystallized and impurities can be removed by heat treatment. Specifically, the sulfide-based solid electrolyte can be obtained by heat-treating the intermediate at a temperature of 300° C. to 500° C. for 12 to 48 hours.
[0056] Sulfide-based solid electrolytes are characterized by their uniform spherical particlesize.
[0057] When the 50% cumulative mass particle size distribution diameter in the particle distribution of the sulfide-based solid electrolyte is referred to as D50, the D50 of the sulfide-based solid electrolyte may range from 5 μm to 10 μm. D50 may refer to the particle size when the cumulative frequency reaches 50% as the number of particles accumulates from a smaller particle diameter. If D50 is less than 5 μm, the packing density of the sulfide-based solid electrolyte may be reduced when the electrode and / or solid electrolyte layer is prepared using a sulfide-based solid electrolyte. If D50 exceeds 10 μm, the specific surface area of the sulfide-based solid electrolyte is reduced, the interface with the active material, etc. is reduced, and therefore, the lithium ion conductivity of the electrode and / or solid electrolyte layer may be reduced.
[0058] When the 90% cumulative mass particle size distribution diameter, the 50% cumulative mass particle size distribution diameter, and the 10% cumulative mass particle size distribution diameter in the particle distribution of the sulfide-based solid electrolyte are referred to as D90, D50, and D10, respectively, the range of (D90-D10) / D50 of the sulfide-based solid electrolyte may be 1 to 3. D10 may refer to the particle size when the cumulative frequency reaches 10% as the number of particles accumulates from a smaller particle size. D90 may refer to the particle size when the cumulative frequency reaches 90% as the number of particles accumulates from a smaller particle size. (D90-D10) / D50 is an indicator for determining the width of the particle size distribution, and the closer it is to 0, the narrower the particle size distribution width is considered to be.
[0059] The means for obtaining the D50, D90 or D10 is not particularly limited, but can be obtained, for example, from an integrated volume value measured with a laser beam diffraction scattering type particle size analyzer.
[0060] The tap density of the sulfide-based solid electrolyte may be in the range of 0.5 g / ml to 0.7 g / ml. The tap density may refer to a density value measured by the volume after 10 g of the sulfide-based solid electrolyte is loaded into a 25 ml measuring cylinder, the measuring cylinder is fixed, and then tapped and rotated 3000 times at the same time.
[0061] The particle compaction density of the sulfide-based solid electrolyte may be in the range of 1.65 g / ml to 1.8 g / ml. The particle compaction density may refer to the particle compaction density calculated based on the difference between the height of the initial empty pelletizer and the height of the pelletizer at this time when a pressure of 3 Mt is applied to the pelletizer for 10 seconds after 1 g of the sulfide-based solid electrolyte is injected into a cylindrical pelletizer with a diameter of 13 mm.
[0062] Other forms of the present invention will be described in more detail by the following examples. The following examples are merely examples to help understand the present invention, and the scope of the present invention is not limited thereto.
[0063] Example 1
[0064] Li was prepared by the following method 6 PS 5 Sulfide-based solid electrolytes for Cl.
[0065] Weigh Li according to the mass ratio of 5:1:2 2 S.P. 2 S 5 and LiCl to prepare the raw materials.
[0066] The raw materials were added so that the solid content of the starting raw materials was about 20%. First, 3 L of tetrahydrofuran was placed in a 5 L glass flask and a stirrer was operated. It was confirmed that by adding Li 2 S and P 2 S 5 , the color changes from transparent orange to green. When the solution is green, LiCl is added and the starting material is prepared by stirring for about 12 hours.
[0067] Use as Figure 2 The spray dryer shown spray-dries the starting material. First, The chamber is adjusted to about 180°C. The interior of the chamber is filled with argon, and the internal pressure of the chamber is adjusted to about 1.3 atmospheres. Under the above state, the starting material is sprayed into the chamber using a nozzle atomizer. The injection amount of the raw material is adjusted to about 70 ml / min. Spray drying is performed for about 1.5 seconds to obtain an intermediate in the form of a white powder.
[0068] After the heat treatment furnace is heated to about 400° C. at a temperature increase rate of about 100° C. / hour, the intermediate is put in while maintaining the temperature. The intermediate is heat treated for about 12 hours to produce a sulfide-based solid electrolyte.
[0069] Example 2
[0070] A sulfide-based solid electrolyte was prepared in the same manner as in Example 1 except that the spray drying temperature was changed to 200°C.
[0071] Example 3
[0072] A sulfide-based solid electrolyte was prepared in the same manner as in Example 1 except that the spray drying temperature was changed to 220°C.
[0073] Example 4
[0074] A sulfide-based solid electrolyte was prepared in the same manner as in Example 1 except that the spray drying temperature was changed to 240°C.
[0075] Comparative Example 1
[0076] The intermediate was obtained by drying the same starting material as in Example 1 using a heating mantle at about 180°C until the starting material became a white powder form.
[0077] By subjecting the intermediate to heat treatment in the same manner as in Example 1, a sulfide-based solid electrolyte was prepared.
[0078] Comparative Example 2
[0079] A sulfide-based solid electrolyte was prepared in the same manner as in Comparative Example 1, except that the temperature of the heating mantle was set to 200°C.
[0080] Comparative Example 3
[0081] A sulfide-based solid electrolyte was prepared in the same manner as in Comparative Example 1, except that the temperature of the heating mantle was set to 220°C.
[0082] Comparative Example 4
[0083] A sulfide-based solid electrolyte was prepared in the same manner as in Comparative Example 1, except that the temperature of the heating mantle was set to 240°C.
[0084] Figure 4 Observation results of the sulfide-based solid electrolyte according to Example 1 using a scanning electron microscope. Figure 5 Observation results of the sulfide-based solid electrolyte according to Example 2 using a scanning electron microscope. Figure 6 These are the results of observing the sulfide-based solid electrolyte according to Example 3 using a scanning electron microscope. Figure 7 These are the results of observing the sulfide-based solid electrolyte according to Example 4 using a scanning electron microscope. Figure 8 This is the result of observing the sulfide-based solid electrolyte according to Comparative Example 1 using a scanning electron microscope. Figures 4 to 8 , it can be seen that the sulfide-based solid electrolytes according to Examples 1 to 4 have a substantially uniform spherical particle size, whereas the sulfide-based solid electrolyte according to Comparative Example 1 has an uneven particle size distribution and is a mixture of spherical particles and plate-like particles.
[0085] Fig. 9 These are the measurement results of the particle size distribution of the sulfide-based solid electrolyte of Example 1. Fig.10 These are the measurement results of the particle size distribution of the sulfide-based solid electrolyte of Example 2. Fig.11 These are the measurement results of the particle size distribution of the sulfide-based solid electrolyte of Example 3. Fig.12 These are the measurement results of the particle size distribution of the sulfide-based solid electrolyte of Example 4. Fig.13 This is the measurement result of the particle size distribution of the sulfide-based solid electrolyte of Comparative Example 1. Based on the above results, D50 and (D90-D10) / D50 of each sulfide-based solid electrolyte were calculated and shown in Table 1 below.
[0086]
Table 1
[0087] Reference Figures 9 to 13 From Table 1, it can be seen that since the sulfide-based solid electrolytes according to Examples 1 to 4 exhibit lower (D90-D10) / D50 values than the sulfide-based solid electrolyte according to Comparative Example 1, a sulfide-based solid electrolyte having a uniform particle size distribution can be obtained according to the present invention.
[0088] Table 2 shows the measurement results of the tap density of the sulfide-based solid electrolytes according to Examples 1, 2, and 4 and Comparative Examples 1 to 4. For each sulfide-based solid electrolyte, the tap density was measured twice and an average value was taken.
[0089]
Table 2
[0090] Table 3 shows the results of Example 1, Example 2, Example 4 and Comparative Examples 1 to 4. The particle compaction density of each sulfide-based solid electrolyte was measured twice and the average value was taken.
[0091]
Table 3
[0092] Referring to Table 2 and Table 3, it can be seen that the sulfide-based solid electrolyte according to the embodiment has a higher tap density and a higher particle compaction density than the sulfide-based solid electrolyte according to the comparative example.
[0093] Fig.14 It is the cyclic voltammetry evaluation result of the performance of the all-solid-state battery prepared using the sulfide-based solid electrolyte according to Example 1, Example 2 and Comparative Example 1. The evaluation conditions were adjusted to 0.1C and 2.5-4.2V. The charging capacity of the all-solid-state battery according to Example 1 is about 221mAh / g, and its discharge capacity is about 205mAh / g. The charging capacity of the all-solid-state battery according to Example 2 is about 223mAh / g, and its discharge capacity is about 202mAh / g. The charging capacity of the all-solid-state battery according to Comparative Example 1 is about 220mAh / g, and its discharge capacity is about 183mAh / g. Example 1 and Example 2 are superior to Comparative Example 1 in both charging capacity and discharge capacity.
[0094] Fig.15 The capacities measured when charging and discharging the all-solid-state batteries prepared using the sulfide-based solid electrolytes according to Example 1, Example 2, and Comparative Example 1 are shown. The measurements were performed while adjusting the C rate to 0.1C, 0.33C, 0.5C, 1C, and then 0.5C. It can be seen that both Example 1 and Example 2 showed excellent results compared to Comparative Example 1.
[0095] Comparative Example 5
[0096] A sulfide-based solid electrolyte was prepared in the same manner as in Example 1 above, except that the solid content of the starting material was adjusted to less than 10 wt %.
[0097] Comparative Example 6
[0098] A sulfide-based solid electrolyte was prepared in the same manner as in Example 1 above, except that the solid content of the starting material was adjusted to be greater than 30% by weight.
[0099] Fig.16 This is the result of analyzing the sulfide-based solid electrolyte according to Comparative Example 5 using a scanning electron microscope. Fig.16 It can be seen that Comparative Example 5 is not spherical, and The shape is very heterogeneous due to the low solid content of the starting material.
[0100] Fig.17 This is the result of analyzing the sulfide-based solid electrolyte according to Comparative Example 6 using a scanning electron microscope. Fig.17 It can be seen that Comparative Example 6 has larger particle size and lumped particles because of the higher solid content of the starting material.
[0101] Fig.18 These are the measurement results of the particle size distribution of the sulfide-based solid electrolyte of Comparative Example 5. Fig.19 This is the measurement result of the particle size distribution of the sulfide-based solid electrolyte of Comparative Example 6. Based on the above results, D50 of each sulfide-based solid electrolyte was calculated and shown in Table 4 together with the result of Example 1.
[0102]
Table 4
[0103] Reference Fig. 9 , Fig.18 and Fig.19 , it can be seen that the sulfide-based solid electrolyte according to Example 1 has a more uniform particle size distribution than those of Comparative Examples 5 and 6.
[0104] Although the experimental examples and implementation modes of the present invention are described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the appended claims also fall within the scope of the present invention.
Claims
1. A method for preparing a solid electrolyte, the method comprising: include: preparing a raw material, wherein the raw material comprises one or more of lithium element (Li element), phosphorus element (P element) and sulfur element (S element); preparing a starting material comprising the raw material and a solvent; obtaining an intermediate in powder form by spray drying the starting material; and By subjecting the intermediate to heat treatment, a sulfide-based solid electrolyte is obtained.
2. The method according to claim 1, in, The raw material includes Li 2 S and P 2 S 5 .
3. The method according to claim 1, in, The raw materials also include lithium compounds containing halogen elements.
4. The method according to claim 1, in, The solvent includes tetrahydrofuran, namely THF.
5. The method according to claim 1, in, The starting material has a solid content in an amount of 10 wt % to 30 wt %.
6. The method according to claim 1, in, Obtaining the intermediate includes: spraying the starting material into the chamber of a spray dryer through a nozzle atomizer.
7. The method according to claim 6, in, The evaporation capacity of the chamber is 1 kg / hour to 4 kg / hour.
8. The method according to claim 6, in, The starting material was sprayed into the chamber at a spray rate of 50 ml / min to 70 ml / min.
9. The method according to claim 6, in, The internal pressure of the chamber ranges from 1.3 atmospheres to 1.5 atmospheres.
10. The method according to claim 6, in, The spray dryer comprises: a chamber defining an interior space of a predetermined size; a nozzle atomizer connected to the chamber and configured to spray the starting material; a first compressor connected to the nozzle atomizer and configured to supply a carrier gas; a second compressor connected to the chamber and configured to supply gas to adjust an internal pressure of the chamber; a sensor mounted within the chamber and configured to measure an internal pressure of the chamber; an exhaust valve for exhausting the carrier gas in the chamber to the outside of the chamber; and A controller is connected to the second compressor and the exhaust valve and is configured to control whether to operate the second compressor and the exhaust valve based on the internal pressure of the chamber measured by the sensor.
11. The method according to claim 1, in, The obtaining of the intermediate is carried out at a temperature of 180°C to 240°C.
12. The method according to claim 1, in, The obtaining of the intermediate comprises: spray drying the starting material for 1 second to 5 seconds.
13. The method according to claim 1, in, Obtaining the sulfide-based solid electrolyte includes heat-treating the intermediate at a temperature of 300° C. to 500° C. for 12 hours to 48 hours.
14. The method according to claim 1, in, The D50 of the sulfide-based solid electrolyte is in the range of 5 μm to 10 μm.
15. The method according to claim 1, in, The range of (D90-D10) / D50 of the sulfide-based solid electrolyte is 1 to 3.
16. The method according to claim 1, in, The tap density of the sulfide-based solid electrolyte ranges from 0.5 g / ml to 0.7 g / ml.
17. The method according to claim 1, in, The particle compaction density of the sulfide-based solid electrolyte is in the range of 1.65 g / ml to 1.8 g / ml.