High-conductivity polymer single ion conductor based on irradiation grafting and preparation method and application thereof
By using highly flexible polymer single-ion conductors prepared by radiation grafting in lithium-ion batteries, the problems of insufficient energy density, power density and safety performance of lithium-ion batteries are solved, achieving high conductivity and improved safety, and reducing Risk of side effects and thermal runaway.
Patent Information
- Application Number
- CN202310362800.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-15
AI Technical Summary
Existing lithium-ion batteries have problems with insufficient energy density, power density and safety performance in large-scale applications. In particular, the traditional separator electrolyte system is flammable and volatile, and the lithium ion migration number is low, leading to thermal runaway and side reactions. And now Some polymer single-ion conductors have low conductivity and are difficult to maintain the lithium ion transport rate.
The irradiation grafting method is used to directly graft the lithium salt that is difficult to self-polymerize on the polyether or polyester main chain to keep the length of the lithium salt side chain short, disperse the anionic groups, and improve the flexibility of the main chain, thereby obtaining high conductivity. Polymer single-ion conductor used in lithium-ion batteries.
It achieves high ion conductivity and improved safety at room temperature, reduces lithium metal interface side reactions, improves uniform deposition of lithium metal, enhances battery cycle performance and safety, and does not require the addition of small molecule plasticizers.
Smart Images

Figure CN118782896A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of new energy technology and is applied to batteries, supercapacitors, etc. Specifically, it relates to a polymer single ion conductor with high ionic conductivity without adding small molecule plasticizers. The present invention also relates to a preparation method of the polymer single ion conductor, namely, a radiation grafting method, and its application in chemical power supply systems such as lithium ion batteries and batteries based on the polymer single ion conductor. Background Art
[0002] Lithium-ion batteries have been widely used in portable devices due to their high energy density and good cycle performance. However, their application in larger-scale fields, especially in grid energy storage and power battery fields, places higher demands on the energy density, power density and safety performance of lithium-ion batteries.
[0003] At present, lithium batteries mainly use diaphragm electrolyte systems. Small molecule organic matter is used as solvent in the electrolyte, which has the disadvantages of being flammable and volatile. When the battery is punctured, impacted, or subjected to high temperature, thermal runaway may occur, causing accidents such as fire and explosion. At the same time, when the electrolyte system is charged and discharged, the number of lithium ion migration is low, and both anions and cations can migrate freely, which is easy to cause side reactions at the electrode interface (especially lithium metal electrodes), thereby reducing energy density and power density. Replacing the electrolyte with a polymer single ion conductor can solve this problem. Under the action of an electric field, only lithium ions can migrate in the polymer single ion conductor, which not only reduces side reactions, but also facilitates the uniform deposition of lithium metal. Polymer single ion conductors can be divided into sulfonic acid groups, borate esters, borane groups, and sulfonyl imide groups according to the anion groups. However, the conductivity of existing polymer single ion conductors is very low, and it is difficult to maintain the lithium ion transport rate required by the battery without adding a large amount of plasticizers. The reason is that in the single ion conductors prepared by traditional methods, 1. the anion groups are too close; 2. the main chain flexibility is low. The results of molecular dynamics simulations show that excessive concentration of anionic groups will greatly reduce the degree of ion dissociation, thereby reducing ionic conductivity. Therefore, it is necessary to further improve polymer single ion conductors. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a high conductivity polymer single ion conductor based on radiation grafting and a preparation method and application thereof. The present invention uses radiation grafting to directly graft a double-bond lithium salt that is not easy to self-polymerize onto a polyether or polyester main chain, and keeps the side chain as short as possible (close to 1 lithium salt unit). Because the anionic groups are dispersed and the main chain is highly flexible, the conductivity of the obtained polymer single ion conductor is greatly improved compared to traditional polymer single ion conductors. Even without adding small molecule plasticizers, it can operate at room temperature, which greatly improves the safety of the battery.
[0005] One of the technical solutions adopted by the present invention to solve the technical problem is:
[0006] A polymer single ion conductor, wherein a lithium salt containing a carbon-carbon double bond and being difficult to self-polymerize is directly grafted onto the main chain of a polyether or polyester, or a lithium salt containing a carbon-carbon double bond and being difficult to self-polymerize and a highly polar monomer containing a carbon-carbon double bond are grafted simultaneously. At the same time, the length of the grafted side chain of the lithium salt is relatively short (close to 1 structural unit) to ensure the dispersibility of the lithium salt.
[0007] Preferably, the chemical formula of the polymer single ion conductor is as shown below:
[0008]
[0009] Wherein, R1 and R2 are polyester or polyether segments, R1 and R2 may be the same or different, R3 is a lithium salt side chain, and R4 is H or a polymer side chain formed by a highly polar monomer.
[0010] In some specific embodiments, the polymer single ion conductor is selected from the following A or B or C:
[0011] Polymer single ion conductor A: Where m1 is a natural number from 5 to 20, and m2 is a natural number from 50 to 1000;
[0012] Polymer single ion conductor B: Where m1 is a natural number between 10 and 40, and m2 is a natural number between 50 and 3000;
[0013] Polymer single ion conductor C: Among them, m1 is a natural number between 5 and 20, m2 is a natural number between 100 and 5000, and m3 is a natural number between 1000 and 10000.
[0014] The main chain of the polymer single ion conductor of the present invention is a polyether chain or polyester chain with good flexibility. The lithium salt group is directly grafted on the flexible polymer main chain, and the length of the grafted side chain is relatively short (close to 1 lithium salt unit). The polymer single ion conductor of this specific structure needs to be prepared by irradiation grafting combined with a specific double bond-containing monomer. The high-conductivity all-polymer single ion conductor provided by the present invention has a higher lithium ion conductivity (3×10 -4 S / cm) and migration number (0.99). The polymer single ion conductor can be used in lithium batteries to effectively improve the cycle efficiency of lithium metal negative electrodes and inhibit fire and explosion caused by short circuits in batteries, greatly improving safety.
[0015] The second technical solution adopted by the present invention to solve its technical problem is:
[0016] The present invention provides a method for preparing the polymer single ion conductor. Radiation is used to directly generate free radical active sites on a polymer main chain with good lithium ion conductivity, and lithium salt groups are grafted onto these sites. Since the selected lithium salt monomer is difficult to self-polymerize, the grafted chain is ensured to be as short as possible.
[0017] Specifically, a method for preparing a polymer single ion conductor comprises:
[0018] 1) Dissolving a flexible polymer with high ion conductivity, i.e., polyether or polyester, and a lithium salt containing carbon-carbon double bonds and difficult to self-polymerize in a good solvent;
[0019] 2) irradiating the solution obtained in step 1) with a radiation source, so that the lithium salt containing carbon-carbon double bonds and difficult to self-polymerize is grafted onto the chain of the flexible polymer, i.e., polyether or polyester, to generate a polymer single ion conductor;
[0020] 3) Add a poor solvent to the product obtained in step 2) to precipitate the polymer single ion conductor, and separate and wash to obtain.
[0021] Furthermore, a highly polar monomer containing a carbon-carbon double bond can be added to the solution obtained in step 1) according to specific circumstances; in step 2), the lithium salt containing a carbon-carbon double bond and being difficult to self-polymerize is grafted onto the chain of the polyether or polyester together with the highly polar monomer containing a carbon-carbon double bond by irradiation to generate a polymer single ion conductor.
[0022] Preferably, the flexible polymer polyether or polyester includes but is not limited to: polyether polymers such as polyethylene oxide, polytetrahydrofuran, polydioxolane, or polyester polymers such as polyvinyl carbonate and polyethylene carbonate condensate, that is, the main chain of the polymer single ion conductor is a polyether chain or a polyester chain.
[0023] Preferably, the lithium salt containing carbon-carbon double bonds and difficult to self-polymerize includes but is not limited to the following substances: one or more of lithium vinyl sulfonate, lithium [(trifluoromethyl)(vinyl)]sulfonyl imide, lithium vinyl borate, etc. The characteristics of these structures are that the carbon-carbon double bonds are directly connected to the anion group, and it is difficult to self-polymerize due to the electrostatic repulsion of the anion.
[0024] Preferably, the highly polar monomer containing a carbon-carbon double bond includes, but is not limited to, one or more of acrylonitrile, maleic anhydride, vinyl acetate or vinyl fluoride.
[0025] Preferably, the good solvent includes, but is not limited to, one or more of acetonitrile, ethyl acetate, acetone, methanol, dimethyl sulfoxide, N,N-dimethylformamide, etc.
[0026] Preferably, the radiation source includes but is not limited to X-rays, γ-rays, β-rays, short-wave ultraviolet rays, high-energy electron beams, and the like.
[0027] Preferably, the poor solvent includes, but is not limited to, one or more of diethyl ether, dichloromethane, chloroform, n-hexane, cyclohexane, xylene, and the like.
[0028] The polymer single ion conductor prepared by the preparation method provided by the present invention has the structural characteristics that the lithium salt group is directly grafted on the flexible polymer main chain, and the length of the grafted side chain is relatively short (close to 1 structural unit). The short length of the grafted side chain is due to the difficulty in chain growth from the polylithium salt monomer chain, which makes chain transfer more likely to occur.
[0029] The third technical solution adopted by the present invention to solve its technical problem is:
[0030] The present invention provides application of the polymer single ion conductor in a chemical power source system, especially in a battery, especially in a lithium ion battery and the like.
[0031] The fourth technical solution adopted by the present invention to solve its technical problem is:
[0032] A lithium ion battery comprises the above-mentioned polymer single ion conductor.
[0033] Unless otherwise specified, the equipment, reagents, processes, parameters, etc. involved in the present invention are conventional equipment, reagents, processes, parameters, etc. and are not given as embodiments.
[0034] All ranges recited herein include all point values within the range.
[0035] The terms “approximately”, “about” or “around” as used herein refer to within ±20% of the range or value.
[0036] In the present invention, the "normal temperature" refers to the normal ambient temperature, which may be 10 to 30°C.
[0037] Compared with the background technology, this technical solution has the following advantages:
[0038] The present invention constructs a grafted single ion conductor structure and ensures that the intervals between anion groups are large, thereby increasing the degree of dissociation and the conductivity. It can have high ion conductivity without adding small molecule plasticizers, and the safety is greatly improved. The high migration number and fixed anions reduce the side reactions on the lithium metal interface, reduce the lithium ion concentration polarization, are conducive to the uniform deposition and stripping of lithium metal, and improve the cycle performance of the battery. The prepared polymer electrolyte has good mechanical properties and is self-supporting. The preparation yield is high, and the preferred product yield can reach 91.3%. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1The radiation grafting reaction principle and the free energy change obtained by theoretical calculation of the embodiment of the present invention, the theoretical calculation level is B3LYP-D3 / def2-TZVP / / B3LYP-D3 / def2-SVP+SMD (CH3CN solvent).
[0040] Figure 2 The results of hydrogen nuclear magnetic resonance spectra before and after irradiation, sample a is a pure sample of lithium [(trifluoromethyl)(vinyl)]sulfonyl imide (hereinafter referred to as LiTVI); sample b is an acetonitrile solution of LiTVI irradiated with a gamma ray dose of 50 kGy; sample c is a mixture of LiTVI and polyethylene oxide dissolved in acetonitrile (Example 2); sample d is sample c irradiated with a gamma ray dose of 50 kGy.
[0041] Figure 3 is the conductivity-temperature curve of each electrolyte membrane.
[0042] Figure 4 The cyclic voltage curves of the lithium symmetric batteries of Comparative Example 3 and Example 4 are shown. DETAILED DESCRIPTION
[0043] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0044] Example 1
[0045] 1) 5.4 g of polyvinyl carbonate and 2.7 g of lithium [(trifluoromethyl)(vinyl)]sulfonyl imide were dissolved in 100 mL of acetonitrile, heated to 60° C. and stirred for 4 hours until the mixture was uniformly dispersed.
[0046] 2) Use 60 The solution obtained in step 1) was irradiated with Coγ-rays at a dose of 50 kGy.
[0047] 3) After the irradiated solution in step 2) is concentrated to 20 mL, an excess of low-temperature ether is added and stirred thoroughly. The precipitated light yellow solid is separated and washed with ether for 3 times. The polymer single ion conductor A is obtained, and the product is 6.2 g with a yield of 76.5%. After being dissolved in acetonitrile, it can be cast into a film. The film is light yellow and has a hard texture.
[0048] The synthesis reaction equation of polymer single ion conductor A is as shown in the figure below, where n is a natural number of 500 to 10000, m1 is a natural number of 5 to 20, and m2 is a natural number of 50 to 1000.
[0049]
[0050] Example 2
[0051] 1) Dissolve 7.2 g of polyethylene oxide and 2.0 g of lithium [(trifluoromethyl)(vinyl)]sulfonyl imide in 100 mL of acetonitrile, heat to 60° C. and stir for 4 hours until the mixture is evenly dispersed.
[0052] 2) Use 60 The solution obtained in step 1) was irradiated with Coγ-rays at a dose of 50 kGy.
[0053] 3) After the irradiated solution in step 2) is concentrated to 20 mL, an excess of low-temperature ether is added and stirred thoroughly. The precipitated light yellow solid is separated and washed with ether for 3 times. The polymer single ion conductor B is obtained, and the product is 8.4 g with a yield of 91.3%. After being dissolved in acetonitrile, it can be cast into a film, which is light yellow and has a tough and elastic texture.
[0054] The synthetic reaction equation of polymer single ion conductor B is shown in the figure below. Where n is a natural number between 1000 and 50000, m1 is a natural number between 10 and 40, and m2 is a natural number between 50 and 3000.
[0055]
[0056] Example 3
[0057] 1) Dissolve 3.6 g of polyethylene oxide, 2.0 g of lithium vinyl sulfonate and 4.0 g of acrylonitrile in 100 mL of acetonitrile, heat to 60° C. and stir for 4 hours until the mixture is evenly dispersed.
[0058] 2) Use 60 The solution obtained in step 1) was irradiated with Co γ-rays at a dose of 50 kgy.
[0059] 3) After the irradiated solution in step 2) is concentrated to 20 mL, an excess of low-temperature ether is added and stirred thoroughly. The precipitated yellow solid is separated and washed with ether for 3 times. The polymer single ion conductor C is obtained, and the product is 7.1 g with a yield of 74.0%. After being dissolved in acetonitrile, it can be cast into a film. The film is dark yellow and has a tough texture. tLi = 0.99.
[0060] The synthetic reaction equation of polymer single ion conductor C is shown in the figure below. Where n is a natural number between 1000 and 50000, m1 is a natural number between 5 and 20, m2 is a natural number between 100 and 5000, and m3 is a natural number between 1000 and 10000.
[0061]
[0062] Example 4
[0063] A battery comprises a positive electrode material and a negative electrode material, wherein the polymer single ion conductor A prepared in Example 1 is provided between the positive electrode material and the negative electrode material as an electrolyte.
[0064] Example 5
[0065] A battery comprises a positive electrode material and a negative electrode material, wherein the polymer single ion conductor B prepared in Example 2 is provided between the positive electrode material and the negative electrode material as an electrolyte.
[0066] Example 6
[0067] A battery comprises a positive electrode material and a negative electrode material, wherein the polymer single ion conductor C prepared in Example 3 is provided between the positive electrode material and the negative electrode material as an electrolyte.
[0068] Comparative Example 1
[0069] A conventional plasticized polymer electrolyte, PEO (Mw = 600000) and lithium salt lithium bis(trifluoromethylsulfonyl)imide are mixed and dissolved in a sufficient amount of acetonitrile, and the acetonitrile is dried and molded, and then an equal amount of plasticizer propylene carbonate is added to obtain a comparative plasticized polymer electrolyte D. The crystallization temperature of the plasticized polymer electrolyte D is about 60°C. The lithium ion migration number is 0.21.
[0070] Comparative Example 2
[0071] A conventional self-polymerized polymer single ion conductor is prepared by dissolving 2 g of lithium p-phenylenesulfonyl imide and 0.01 g of AIBN in sufficient acetonitrile, and refluxing at 80°C for 8 h to fully polymerize the lithium salt. 7.2 g of PEO (Mw = 600,000) is added to the mixture, and after mixing evenly, the mixture is fully dried in acetonitrile for molding to obtain a comparative polymer single ion conductor E. The lithium ion transference number of the polymer single ion conductor E is 0.91.
[0072] Comparative Example 3
[0073] A battery comprises a positive electrode material and a negative electrode material, wherein the plasticized polymer electrolyte D in Comparative Example 1 is provided between the positive electrode material and the negative electrode material as an electrolyte.
[0074] Comparative Example 4
[0075] A conventional diaphragm electrolyte system battery comprises a positive electrode material and a negative electrode material, wherein a PP diaphragm and an LB-301 electrolyte (constituents are lithium hexafluorophosphate, ethylene carbonate and dimethyl carbonate) are arranged between the positive electrode material and the negative electrode material.
[0076] The preparation principle of the radiation grafted single ion conductor according to one embodiment of the present invention is shown in Figure 1As shown, high-energy rays destroy the CH bond and form a free radical site on the C atom. This site can attack the carbon-carbon double bond to cause a chain initiation reaction. The free energy change ΔG of this reaction is -27.6 kJ / mol. After that, there is a competition between chain growth and chain transfer. The ΔG of the chain growth reaction is -5.5 kJ / mol. Compared with the chain initiation, the spontaneity decreases. The reason for the decrease in spontaneity is the huge electrostatic repulsion energy between anionic monomers. Therefore, the system is more inclined to undergo a chain transfer reaction and then a new chain initiation reaction. The ΔG of this process is -32.0 kJ / mol, which is more advantageous than the chain growth reaction. Nuclear magnetic resonance hydrogen spectrum testing also verified this mechanism. The results are shown in Figure 2 As shown, the difficult-to-polymerize lithium salt alone did not undergo polymerization after irradiation in a solvent, but when the difficult-to-polymerize lithium salt was mixed with polymer PEO and dissolved in a solution and irradiated, the double bonds disappeared, indicating that a grafting reaction occurred.
[0077] The comparison of Li ion migration numbers of the products of Examples 1, 2, 3 and Comparative Examples 1 and 2 at 60°C is shown in Table 1. The comparison of conductivity is shown in Table 1. Figure 3 , combined with Table 1 and Figure 3 It can be seen that, relative to the dual ion conductor in Comparative Example 1, the migration numbers of Examples 1, 2, and 3 are increased from 0.21 to 0.98, 0.96, and 0.99, respectively. Because the anions are immobilized, the conductivity is slightly reduced, but the reduction is no more than one order of magnitude, and below the melting temperature of Comparative Example 1 of 60°C, the conductivity of the three embodiments is higher than that of Comparative Example 1. Compared with the self-polymerized single ion conductor in Comparative Example 2, the conductivity of the three embodiments is significantly improved, and it is increased by one order of magnitude or more above 60°C. The migration number is also further improved.
[0078] Table 1 Comparison of Li ion migration numbers of electrolytes of Examples 1, 2, 3 and Comparative Examples 1 and 2 at 60°C
[0079]
[0080] The key parameters of mechanical properties of Examples 1, 2, 3 and Comparative Example 1 are listed in Table 2. It can be seen from the table that the key mechanical indicators of Examples 1, 2, 3 are not inferior to those of Comparative Example 1 which can achieve self-support, and some of the examples even have a slight advantage, indicating that the examples have good mechanical properties and can achieve self-support.
[0081] Table 2 Comparison of mechanical properties of electrolytes of Examples 1, 2, 3 and Comparative Example 1
[0082]
[0083] Compared with Comparative Examples 3 and 4, Examples 4, 5 and 6 have significantly improved battery safety. The battery safety test results are listed in Table 3. In the puncture test, Comparative Example 4 caught fire after puncture, and the temperature rose sharply to 320°C in a short time. Because the main body of Examples 4, 5 and 6 is a polymer and no combustion occurs after puncture, the puncture temperature is significantly reduced compared with Comparative Example 3. The thermal runaway temperature was measured by adiabatic calorimetry, and Comparative Example 4 had the lowest thermal runaway temperature of 150°C. The thermal runaway temperature of Comparative Example 3 is slightly higher, at 232°C. The thermal runaway temperatures of Examples 4, 5 and 6 are 350, 392, and 310°C, respectively. The reason for the high thermal runaway temperature of the examples is that they are completely free of volatile components, thereby suppressing the thermal runaway caused by the volatilization and ignition of combustibles. The experimental results show that Examples 4, 5, and 6 have superior safety performance compared to the comparative examples.
[0084] Table 3 Comparison of soft pack battery safety of Examples 4, 5, 6 and Comparative Examples 3, 4
[0085]
[0086] Figure 4 The lithium symmetric battery cycle diagram of Example 4 and Comparative Example 3 shows that Comparative Example 3 short-circuited after 300 hours of cycling, while Example 4 can still cycle stably after 1000 hours of cycling. This shows that the single ion conductor can inhibit the growth of lithium dendrites and thus improve the cycling performance of the lithium negative electrode.
[0087] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. A method for preparing a polymer single ion conductor, characterized in that: include: 1) dissolving polyether or polyester and lithium salt containing carbon-carbon double bonds and difficult to self-polymerize in a good solvent; 2) irradiating the solution obtained in step 1) to graft the lithium salt containing carbon-carbon double bonds and difficult to self-polymerize onto the chain of the polyether or polyester to generate a polymer single ion conductor; 3) Adding a poor solvent to the product obtained in step 2) to precipitate the polymer single ion conductor to obtain the product.
2. The preparation method according to claim 1, characterized in that: A highly polar monomer containing a carbon-carbon double bond is added to the solution obtained in step 1); in step 2), the lithium salt containing a carbon-carbon double bond and being difficult to self-polymerize is grafted onto the chain of the polyether or polyester together with the highly polar monomer containing a carbon-carbon double bond by irradiation to generate a polymer single ion conductor.
3. The preparation method according to claim 1, characterized in that: The polyether includes at least one of polyethylene oxide, polytetrahydrofuran or polydioxolane; the polyester includes at least one of polyethylene carbonate or polyethylene carbonate condensate.
4. The preparation method according to claim 1, characterized in that: The lithium salt containing a carbon-carbon double bond and being difficult to self-polymerize includes at least one of lithium vinyl sulfonate, lithium [(trifluoromethyl)(vinyl)]sulfonyl imide or lithium vinyl borate.
5. The preparation method according to claim 2, characterized in that: The highly polar monomer containing a carbon-carbon double bond includes at least one of acrylonitrile, maleic anhydride, vinyl acetate or vinyl fluoride.
6. The preparation method according to claim 1, characterized in that: The good solvent includes at least one of acetonitrile, ethyl acetate, acetone, methanol, dimethyl sulfoxide or N,N-dimethylformamide; the poor solvent includes at least one of ether, dichloromethane, chloroform, n-hexane, cyclohexane or xylene; the radiation source used for the irradiation includes X-rays, γ-rays, β-rays, short-wave ultraviolet rays, or high-energy electron beams.
7. A polymer single ion conductor prepared by the preparation method according to any one of claims 1 to 6.
8. The polymer single ion conductor according to claim 7, characterized in that: The polymer single ion conductor is selected from the following A or B or C: A: Where m1 is a natural number from 5 to 20, and m2 is a natural number from 50 to 1000; B: Where m1 is a natural number between 10 and 40, and m2 is a natural number between 50 and 3000; C: Among them, m1 is a natural number between 5 and 20, m2 is a natural number between 100 and 5000, and m3 is a natural number between 1000 and 10000.
9. Use of the polymer single ion conductor according to claim 7 in a chemical power source system.
10. A lithium ion battery, characterized in that: The lithium ion battery comprises the polymer single ion conductor according to claim 7.
Citation Information
Cited By
Quasi-solid electrolyte of sodium metal battery, preparation method of quasi-solid electrolyte and quasi-solid sodium battery
CN121484223A