Cured, conformable porous composites and related devices, methods and uses
By using closed-circuit battery expandable microspheres in combination with thermally expandable polymer microspheres and inorganic particle filling materials to form a cured porous composite material, the problems of solvent use and insufficient performance in traditional lead-acid battery pack separator manufacturing are solved, and high porosity is achieved efficiency and good wettability, improving the cycle and recharge capabilities of the battery pack.
Patent Information
- Application Number
- CN202410735727.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2016-08-05
- Filing Date
- 2017-08-04
- Publication Date
- 2024-10-15
AI Technical Summary
The manufacturing process of traditional lead-acid battery pack separators uses dangerous and flammable solvents, resulting in low production efficiency and environmental pollution, and performs poorly in terms of high cycle and recharge capabilities, especially in 'start-stop' applications. High performance requirements.
Closed-circuit cell expandable microspheres are combined with thermally expanded polymer microspheres and inorganic particulate filler materials to form a cured, conformable porous composite that is compressed and heated to form a separator with interconnected pores, eliminating the use of processing oils and extractions Solvent to improve porosity and electrolyte wettability.
It is possible to create a separator with high porosity and good wettability without using dangerous solvents, which improves the cycleability and rechargeability of lead-acid battery packs and is suitable for 'start-stop' applications with high cycle requirements.
Smart Images

Figure CN118783031A_ABST
Abstract
Description
[0001] This application is a divisional application of a Chinese patent application filed on August 4, 2017, with Chinese patent application number 201780054041.0 and invention name “Solidified, conformable porous composite materials and related devices, methods and uses”, and this application claims priority to the U.S. application number 62 / 371,453.
[0002] Copyright Notice
[0003] Amtek Research International LLC. A portion of the disclosure of this patent document contains material that is subject to copyright protection. The copyright owner has no objection to the facsimile reproduction by anyone of the patent document or the patent disclosure, as it appears in the U.S. Patent and Trademark Office patent file or records, but otherwise reserves all copyright rights whatsoever. 37 CFR §1.71(d). Technical Field
[0004] The present invention relates to a cured, conformable porous composite material having interconnected pores and comprising thermally expanded polymer microspheres and a particulate filler material. The cured, conformable porous composite material (1) exhibits good porosity without the use of processing oils and accompanying extraction solvents, and (2) exhibits adequate electrolyte wettability. The cured, conformable porous composite material can be used as a separator to improve the manufacturability and performance of energy storage devices such as lead-acid batteries. Background Art
[0005] As technology has evolved, separators for lead-acid batteries have been formed from different materials. Over time, wood, paper, rubber, PVC, fiberglass, and silica-filled polyethylene have all been used. Currently, lead-acid batteries are found to be generally in two design modes, namely valve-regulated recombinant (valve-regulated lead acid (VRLA)) batteries and flooded batteries. Both modes include a positive electrode and a negative electrode separated from each other by a porous battery separator. The porous separator prevents the electrodes from physically contacting and provides a residence space for the electrolyte. This separator is formed from a material that is resistant to sulfuric acid electrolyte, is easily wetted in sulfuric acid, and has sufficient porosity to allow the electrolyte to be present in the pores of the separator material, thereby allowing ionic current to flow with low resistance between adjacent positive and negative plates.
[0006] Recently, enhanced flooded batteries (EFBs) have been developed to meet the high cycling requirements in "start-stop" or "micro-hybrid" vehicle applications. In such applications, the engine is shut down when the vehicle stops (e.g., at a traffic light) and restarted later. The advantage of the "start-stop" vehicle design is that it can reduce CO2 emissions and improve overall fuel efficiency. The main challenge of a "start-stop" vehicle is that the battery pack must continue to provide all electrical functions during the stop phase while being able to provide enough current to restart the engine at the required moment. In this case, the battery pack must show higher performance in terms of cycling and rechargeability compared to traditional flooded lead-acid battery designs.
[0007] In the case of "start-stop" applications, valve-regulated lead-acid (VRLA) batteries have shown good cyclability in the field, but they have relatively high costs and other issues. Therefore, there remains a need for mechanically strong, acid-resistant, high-porosity separators that can be used throughout the life cycle of lead-acid batteries used in "start-stop" applications.
[0008] For silica-filled polyethylene separators, the traditional manufacturing process includes extrusion, extraction, followed by drying, cutting and winding steps. Precipitated silica is typically combined with polyolefins, process oils and various minor ingredients to form a separator mixture, which is extruded through a sheet die at an elevated temperature to form an oil-filled sheet. The oil-filled sheet is calendered to its desired thickness and profile, and most of the process oil is extracted. The sheet is dried to form a microporous polyolefin separator and cut into appropriate widths for a specific battery pack design. In this manufacturing process, the extraction of the process oil and the drying of the extraction solvent are the limiting steps. The output of the production line depends on the speed at which the process oil can be removed and the speed at which the solvent dries, both of which depend on the thickness of the separator product. Trichloroethylene (TCE) and hexane are typically used as extraction solvents for the process oil, which present challenges in terms of health, safety and effective recycling.
[0009] Therefore, there is also a need for a battery separator that is manufactured without the use of hazardous and / or flammable solvents. The separator should have desirable properties, such as good wettability, good porosity, and allow for high cyclability and rechargeability of the battery. Summary of the invention
[0010] It has been found that closed circuit battery expandable microspheres can be combined with a particulate filler material to form a cured, conformable porous composite material having interconnected pores and containing thermally expandable polymer microspheres and particulate filler material. The cured, conformable porous composite material can form a battery separator with good wettability, good porosity, and allows for batteries with high cyclability and rechargeability.
[0011] The expandable microspheres are preferably expandable polymer microspheres, such as (AkzoNobel NV), Advancell EM (Sekisui Chemical Co., Ltd.), Kureha Microsphere (Kureha Corp.), (Chase Corp.), (PolyChem Alloy). Expancel microspheres are small spherical thermoplastic particles that consist of a polymer shell that encapsulates a gas. When heated, the internal pressure from the gas increases while the thermoplastic shell softens. Therefore, with the gas trapped inside the sphere, the volume of the microsphere increases.
[0012] The particulate filling material preferably comprises an inorganic material. The inorganic material preferably comprises an inorganic oxide, carbonate or hydroxide, such as alumina, silica, zirconium oxide, titanium dioxide, mica, boehmite or a mixture thereof. The inorganic material provides electrolyte wettability to the solidified, conformable porous composite material. The inorganic material can be porous or non-porous. The inorganic material can be in various forms, such as particles, fibers (e.g., microglass fibers), flakes or nanotubes in ground or unground form. The inorganic material is preferably insoluble in sulfuric acid, an electrolyte commonly used in lead-acid batteries. The inorganic material may be insoluble in potassium hydroxide, an electrolyte commonly used in alkaline batteries. The inorganic material is preferably about 30 wt % to about 90 wt % of the solidified, conformable porous composite material.
[0013] Compression and heating are preferably used to form a solidified, conformable porous composite material. The particulate filler material is preferably mixed with expandable microspheres and then heated in a defined volume space (e.g., a mold). The process can be performed in batches or continuously. Similarly, a solidified, conformable porous composite material can be formed in situ between the electrodes of a battery pack.
[0014] The porosity of the solidified, conformable porous composite material measured by water porosity is preferably 30% or more, such as about 40% or more, about 50% or more, about 60% or more, about 70% or more, or about 80% or more. For example, the porosity can be about 30% to about 90%, about 40% to about 90%, about 50% to about 90%, about 60% to about 90%, about 70% to about 90%, about 75% to about 90%, about 80% to about 90%, or about 85% to about 90%.
[0015] Mechanical reinforcements can be added to increase the structural strength of the porous composite material that is cured, adapted. Mechanical reinforcements can be supports that are primarily formed on one or two major surfaces of the porous composite material that is cured, adapted, or at least partially embedded in the overall structure of the porous composite material that is cured, adapted. The example of support includes foam, sheet, film, mesh, membrane, woven or nonwoven mat, silk screen, or a combination thereof.
[0016] The cured, conformable porous composite material is preferably wettable by an electrolyte and has a porosity of about 30-90% as determined by water porosity determination (e.g., BCIS-03-6 test method for porosity (volume) and moisture content). The cured, conformable porous composite material as described above can be used to separate electrodes in energy storage devices (e.g., batteries, electrochemical double layer capacitors, supercapacitors, or fuel cells), wherein the pores can be filled with an electrolyte. Such a separator is advantageous for the manufacture of energy storage devices.
[0017] Other aspects and advantages will become apparent from the following detailed description of the preferred embodiments which proceeds with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 A picture showing the process steps from Example 3 is depicted.
[0019] Figure 2A A SEM fracture level view image of a sample obtained from Example 9 is depicted.
[0020] Figure 2B Depicted with Figure 2A SEM fracture vertical view image of the same sample.
[0021] Figure 3 A picture showing a single cell from Example 10 is depicted.
[0022] Figure 4 A sample prepared from Example 11 is depicted.
[0023] Figure 5A A SEM image of the top surface of the sample obtained from Example 12 is depicted.
[0024] Figure 5B Depicted with Figure 5A SEM image of a cross section of the same sample. DETAILED DESCRIPTION
[0025] By mixing expandable microspheres with a particulate filling material, a solidified, conformable porous composite material having interconnected pores and containing heat-expandable microspheres and particulate filling materials can be prepared. The microspheres can be dry powders or aqueous dispersions. Similarly, the particulate filling material can be dry powders or aqueous dispersions. The mixture can then be placed in a mold (or other volume-limited space) and heated for a sufficient time to bond the materials together. The expansion of the microspheres provides the necessary compression for bonding. The volume of the mold (which affects the pressure as the microspheres expand) and the temperature and duration of the heating can be used to cause at least a portion of the heat-expanded polymer microspheres to break due to the escape of the gas encapsulated in the microspheres. After expansion, the mold is slowly cooled. The microspheres remain in an expanded state and bond together. The solidified, conformable porous composite material is then removed from the mold. When there is an aqueous dispersion, water can be evaporated as part of the formation process. Before heating the mixture, a mechanical reinforcement material can be placed in the mold. As used herein, "cured, conformable porous composite material" means that the composite material is a solid that conforms to the shape of the volumetric defined space in which the expandable microspheres and particulate filler material are heated.
[0026] The mold patterning (or other volume-limited space) can be made to provide various ribbed patterns. In addition, the porous composite material of solidification, conformation can be further shaped after being taken out from the mold. The porous composite material of solidification, conformation can form a sheet or other required geometric shapes. For example, a sheet can be formed, which has at least one patterned major surface, has a thickness of about 0.3mm to about 0.6mm or about 0.4mm to about 0.5mm, and has a thickness of about 0.5mm to about 5mm or about 1mm to about 3mm.
[0027] The same process can be repeated in a battery or other energy storage device cell. The free-flowing mixture of expandable microspheres and particulate filler material can be placed between the electrodes of the cell, the cell capped, and then the cell heated. As the microspheres expand, the fixed cell volume provides the necessary compression. It is not necessary to remove the cured, conformable porous composite from the cell. After the cured, conformable porous composite is formed, the electrolyte can be added directly to the cell.
[0028] The cured, conformable porous composite (formed in situ or in a mold) was in good contact with the electrode, and no leaching of the Expancel microspheres swollen in acid was detected. The cured, conformable porous composite had good acid wettability, good porosity, and allowed for high cyclability and rechargeability of the battery.
[0029] The cured, conformable porous composite material can be used with many energy storage devices, such as alkaline batteries or lead-acid batteries. The cured, conformable porous composite material can constitute a separator or a portion thereof.
[0030] The particulate filling material of the solidified, conformable porous composite material may include additives. The solidified, conformable porous composite material may include additives that beneficially affect the performance of the energy storage device. Preferred additives include hydrogen evolution inhibitors, electrolyte-soluble pore formers, structural reinforcing agents, wettability enhancers, or combinations thereof. Certain additives may perform multiple functions.
[0031] Turning now to specific exemplary additives, an electrolyte-soluble pore former is dissolved in the electrolyte (typically sulfuric acid for lead-acid batteries and aqueous potassium hydroxide for alkaline batteries) after the battery is assembled and the electrolyte is added. The dissolution of the electrolyte-soluble pore former results in an increase in the porosity of the separator, a change in the interconnectivity (i.e., tortuosity) between adjacent pores of the separator, and an increase in the pore size distribution. After the electrolyte-soluble pore former is dissolved, the battery is optionally rinsed with fresh electrolyte. For lead-acid batteries, preferably, the electrolyte-soluble pore former is magnesium hydroxide, magnesium oxide, or a combination thereof. The electrolyte-soluble pore former may include sulfates of zinc, lithium, aluminum, magnesium, tin, potassium, or sodium. The electrolyte-soluble pore former may also include carbonates of lithium, magnesium, potassium, or sodium. The electrolyte-soluble pore former may be combined with the above-mentioned inorganic materials that provide electrolyte wettability to the cured, conformable porous composite material.
[0032] The hydrogen evolution inhibitor may be distributed throughout the pore structure of the cured, conformable porous composite material. Examples of hydrogen evolution inhibitors include benzaldehyde derivatives such as vanillin, o-anisaldehyde, 2-hydroxybenzaldehyde, 4-methoxybenzaldehyde, 2,4-dimethoxybenzaldehyde, 2,5-dimethoxybenzaldehyde, veratraldehyde (3,4-dimethoxybenzaldehyde) and 2,3,4-trimethoxybenzaldehyde.
[0033] The cured, conformable porous composite material may also include additives other than particulate filler materials, such as surface active molecules, such as sodium dodecylbenzene sulfonate or sodium dihexylsulfosuccinate.Other additives for non-energy storage devices include fragrances.
[0034] The ability to form a cured, conformable porous composite material in situ is beneficial for manufacturing. For example, a cured, conformable porous composite material can be manufactured during assembly of a battery pack. This can facilitate the manufacture of lead-acid batteries in a bipolar stack configuration with attendant benefits in energy density and uniform current density. Other manufacturing benefits of a cured, conformable porous composite material (formed in situ or in a mold) will be apparent to those skilled in the art.
[0035] In addition to separators, the cured, conformable porous composite material can be used to make other components of energy storage devices, such as flame arresters. In addition, the cured, conformable porous composite material can be used for non-energy storage device related applications, such as fragrance storage.
[0036] Example
[0037] For each example, a strong and stable cured, conformable porous composite material was formed by mixing the dry powders listed in Table 1.
[0038] For Examples 1-9, the thoroughly mixed dry powder was placed in a tightly sealed 4 oz plastic jar (see Figure 1 ) in an oven at the listed temperature for 1 hour, the plastic jar provides the required compression for the expanded microspheres, which causes the mixed powder to bind to form a strong and hard cured, conformable porous composite.
[0039] For Example 10, a cured, conformable porous composite material was formed by binding the listed mixed dry powder formulation in a single cell consisting of one positive electrode and one negative electrode obtained from a Deka YB16B dry-charged motorcycle battery pack (East Penn Manufacturing Co., Inc.). The cell was covered and placed in an oven and cured for 2 hours at the listed temperature. The cell showed high cycling and recharge capabilities.
[0040] For Examples 11-48, the listed well-mixed dry powder formulations and glass fiber mats were pressed between molds with washers and heated at the listed temperatures at constant pressure for 15 minutes. The molds were allowed to cool slowly before removing the samples. The templates were designed to have grooves therein so that the finished samples had a ribbed surface. The total thickness of Examples 11-48 ranged from about 0.5 mm to about 3 mm.
[0041] The resistance of Example 26 was evaluated using a DC pulse technique. The sample was soaked in sulfuric acid and then placed in a test bath. This example showed sufficiently low resistance, indicating good electrolyte wettability.
[0042] Table 1
[0043]
[0044]
[0045]
[0046]
[0047]
[0048]
[0049] It will be apparent to those skilled in the art that many changes may be made to the details of the above-described embodiments without departing from the underlying principles of the invention.
Claims
1. A solidified porous composite material, the solidified porous composite material comprising: a heat-expandable polymer matrix and a particulate fill material distributed in the polymer matrix, wherein the heat-expandable polymer matrix comprises compressed and thermally bonded polymer microspheres that have been heat-expanded to fill fixed-volume cavities of a volumetric space; and in, The cured porous composite material comprises interconnected pores extending through the polymer matrix and a porosity of 30% or greater.
2. The cured porous composite material according to claim 1, wherein at least a portion of the polymer microspheres are ruptured due to the escape of encapsulated gas during thermal expansion of the polymer microspheres.
3. The cured porous composite material of claim 1, wherein the porous composite material is free of mechanical reinforcement materials comprising woven or non-woven mats.
4. The cured porous composite material of claim 1, wherein the particulate filler material comprises an inorganic material comprising alumina, silica, zirconia, titania, mica, boehmite, or a mixture of any of the foregoing.
5. The cured porous composite material of claim 1, wherein the cured porous composite material is wettable by an electrolyte and has a porosity of 30-90% as measured by water porosity.
6. The cured porous composite material of claim 1, wherein the polymer microspheres and the particulate filler material comprise a bound dry powder or a bound aqueous dispersion.
7. The cured porous composite material of claim 1, wherein the particulate filler material comprises from 30% to 90% by weight of the cured porous composite material.
8. The cured porous composite material according to claim 1, wherein the particulate filling material further comprises an additive, the additive comprising a hydrogen evolution inhibitor, an electrolyte-soluble pore former, a structural reinforcing agent, a wettability enhancing agent, a fragrance, or a combination thereof.
9. The cured porous composite material of claim 8, wherein the additive comprises a fragrance.
10. The cured porous composite material of claim 1, wherein the cured porous composite material is formed into a sheet having a planar major surface, a patterned major surface, or a combination thereof.
11. The cured porous composite material of claim 10, wherein the sheet has at least one patterned major surface, has a region having a thickness of 0.3 mm to 0.6 mm, and has a region having a thickness of 0.5 mm to 5 mm.
12. The cured porous composite material of claim 11, wherein the sheet has at least one patterned major surface, has a region having a thickness of 0.4 mm to 0.5 mm, and has a region having a thickness of 1 mm to 3 mm.
13. An energy storage device comprising the cured porous composite material of claim 1.
14. A fragrance storage device comprising the cured porous composite material of claim 1.
15. A method of preparing a cured porous composite material according to claim 1, wherein no solvent is introduced into the composite material and removed from the composite material during the formation of the pores, said method include: A mixture of polymer microspheres and a particulate filler material is placed in a cavity of fixed volume; and The mixture is heated and compressed in the fixed-volume cavity to sufficiently expand the polymer microspheres to fill and conform to the fixed-volume cavity, to combine the heat-expanded polymer microspheres with the particulate filling material within the fixed-volume cavity, to cause at least a portion of the polymer microspheres to rupture due to the escape of encapsulated gas during the thermal expansion of the polymer microspheres, and to form a solidified porous composite material having interconnected pores.
16. The method of claim 15, further comprising slowly cooling the thermally expanded microspheres.