By forming a coating layer containing Sn, Cu, Cr and Ni intermetallic compound crystals on the surface of the substrate, the problem of insufficient durability of a single precious metal coating layer at high temperatures is solved, and the durability in high temperature environments is improved.

CN118783153APending Publication Date: 2024-10-15NAPRA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311021951.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2023-08-15
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Precious metal single-coated terminals have insufficient durability in high-temperature environments and are difficult to meet the high-temperature operating requirements of electronic equipment.

Method used

A plating layer is formed on the surface of the base material. The plating layer contains intermetallic compound crystals of Sn, Cu, Cr and Ni dispersed in the mother phase of Sn and Sn-Cu alloy. It is produced by electrolytic plating electrodes and adopts an epitaxial joint structure to improve durability. sex.

Benefits of technology

Significantly improves the durability of the terminal in high temperature environments, avoids cracks and peeling of the coating at high temperatures, and maintains mechanical strength and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118783153A_ABST
    Figure CN118783153A_ABST
Patent Text Reader

Abstract

Precious metal, such as a silver-plated or tin-plated film, or a single-metal plated film has high conductivity, so that the plated film can be widely applied to a connector of an electronic device, a contact of a switch, a relay and the like, and a terminal component. However, when a terminal using such a noble metal or a single metal is operated in a high-temperature environment, there is a problem in durability. The problem is solved by a terminal in which a plating layer is formed on the surface of a base material, and the plating layer has a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a parent phase containing Sn and an Sn-Cu alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a terminal and a bump suitable for an electronic component connection portion, a bonding terminal, and the like. Background Art

[0002] Plating films of precious metals or single metals such as silver plating and tin plating are widely used in contacts or terminals of connectors, switches, relays, etc. of electronic devices due to their high conductivity. However, when terminals using such precious metals or single metals are operated in a high temperature environment, there is a problem of durability.

[0003] It should be noted that Patent Document 1 below discloses a tin-copper intermetallic compound dispersed tin contact terminal, which is characterized in that a tin plating layer in which a tin-copper intermetallic compound is dispersed is formed on the surface of a base material made of copper or a copper alloy.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2003-82499 Summary of the invention

[0007] Problems to be solved by the invention

[0008] An object of the present invention is to provide a terminal having excellent durability when operating in a high temperature environment.

[0009] Means for solving problems

[0010] The present invention provides a terminal having a plating layer formed on the surface of a substrate, wherein the plating layer has a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a matrix containing Sn and a Sn-Cu alloy.

[0011] Effects of the Invention

[0012] According to the present invention, it is possible to provide a terminal having excellent durability when operating in a high-temperature environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is an optical image of a cross section obtained by thinly cutting the electrode for electrolytic plating of the present invention obtained in Example 1 by FIB (focused ion beam).

[0014] Figure 2 This is a cross-sectional SEM image of the obtained electrode for electrolytic plating of Example 1.

[0015] Figure 3 This is a diagram showing the results of element mapping analysis of the electrode for electrolytic plating obtained in Example 1 by EDS.

[0016] Figure 4 This is a diagram for explaining an example of a production apparatus suitable for producing the metal particles of the present invention.

[0017] Figure 5 This is a microscope photograph showing the results of a 180-degree bending test of the contact terminal of Example 1.

[0018] Figure 6 This is a microscope photograph showing the results of a surface crack test on the contact terminal of Example 1.

[0019] Figure 7 This is a microscope photograph showing the test results of heat resistance of Example 1.

[0020] Figure 8 This is a microscope photograph showing the results of a 180-degree bending test of the contact terminal of Comparative Example 1.

[0021] Fig. 9 This is a microscope photograph showing the results of the surface crack test of Comparative Example 1.

[0022] Fig.10 This is a microscope photograph showing the results of the heat resistance test of Comparative Example 1.

[0023] Explanation of symbols

[0024] 1 Granulation chamber

[0025] 2 Cover

[0026] 3 Nozzles

[0027] 4 dish-shaped rotating disk

[0028] 5 Rotating disk support mechanism

[0029] 6 Particle discharge pipe

[0030] 7 Electric stove

[0031] 8 Mixed gas tank

[0032] 9Piping

[0033] 10Piping

[0034] 11 valves

[0035] 12 Exhaust

[0036] 13 Valve

[0037] 14 Exhaust

[0038] 15. Automatic Filter

[0039] 16 Particle recovery device DETAILED DESCRIPTION

[0040] Hereinafter, embodiments of the present invention will be described in further detail.

[0041] First, the terminology in this specification is based on the following unless otherwise specified.

[0042] (1) Metals may include not only simple metal elements but also alloys and intermetallic compound crystals containing multiple metal elements.

[0043] (2) When referring to a single metal element, it does not refer to a substance that is completely pure and only composed of the metal element, but also refers to the case where other substances are contained in trace amounts. In other words, it does not mean that substances containing trace amounts of impurities that have little effect on the properties of the metal element are excluded. For example, when referring to the parent phase, it does not mean that substances in which part of the atoms in the Sn crystal are replaced by other elements (such as Cu) are excluded. For example, the above-mentioned other substances or other elements may contain 0 to 0.1 mass % in the following electrode.

[0044] (3) Epitaxial bonding refers to the precipitation of intermetallic compound crystals in a substance that becomes a metal-alloy (the parent phase in the present invention), and the precipitation of the intermediate Sn-Cu alloy and the intermetallic compound crystals are bonded at the lattice level to form grains. The term epitaxial bonding is well known, for example, as described in the last paragraph of the left column of page 160 of Nature Chemistry 3(2):160-6, 2011.

[0045] The terminal of the present invention is a terminal formed by forming a plating layer on the surface of a substrate, and the plating layer has a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a matrix containing Sn and a Sn-Cu alloy.

[0046] The following electrolytic plating electrode is applied to the plating bath for forming the above-mentioned plating layer. Hereinafter, the above-mentioned electrolytic plating electrode may be referred to as "electrolytic plating electrode of the present invention".

[0047] The electrode for electrolytic plating of the present invention has a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are contained in a matrix containing Sn and a Sn-Cu alloy, and the composition of the structure is:

[0048] Cu: 0.7-15 mass %,

[0049] Cr: 0.001 to 1 mass %,

[0050] Ni: 0.01 to 5 mass %,

[0051] The remainder is Sn (which may contain unavoidable impurities in an amount of 0.1 mass % or less),

[0052] The composition of the parent phase is Cu: 5 mass % or less, Ni: 1 mass % or less, Cr: 1 mass % or less, and the remainder is Sn (which may contain unavoidable impurities of 0.1 mass % or less),

[0053] The intermetallic compound crystals are contained in the matrix phase.

[0054] Figure 1 This is an optical image of a cross section obtained by thinly cutting the electrode for electrolytic plating of the present invention obtained in Example 1 described below by FIB (focused ion beam).

[0055] The electrode for electrolytic plating of the present invention may be a soluble electrode, and can be produced by the following method.

[0056] First, metal particles described below (hereinafter, sometimes referred to as metal particles of the present invention) are produced.

[0057] Next, the obtained metal particles of the present invention are melted by high-frequency induction heating under vacuum, cast in a mold in a nitrogen atmosphere and under atmospheric pressure, cooled and solidified to form a rolled sheet, which is then stacked in multiple pieces as needed (hereinafter sometimes referred to as a block), thereby obtaining a rolled sheet.

[0058] The metal particles of the present invention can be produced from a raw material containing, for example, 8% by mass of Cu, 1% by mass of Cr, 1% by mass of Ni, and the remainder being Sn. For example, the raw material is melted, supplied to a dish-shaped disk rotating at high speed in a nitrogen atmosphere, the molten metal is dispersed in the form of droplets by centrifugal force, and cooled and solidified under reduced pressure to obtain the metal particles.

[0059] Reference Figure 4An example of a manufacturing device suitable for manufacturing the metal particles of the present invention is described. The upper part of the granulation chamber 1 is cylindrical, the lower part is conical, and a cover 2 is provided on the upper part. A nozzle 3 is vertically inserted into the center of the cover 2, and a dish-shaped rotating disk 4 is provided directly below the nozzle 3. Symbol 5 is a mechanism for supporting the dish-shaped rotating disk 4 so as to be movable up and down. In addition, a discharge pipe 6 for the generated particles is connected to the lower end of the conical part of the granulation chamber 1. The upper part of the nozzle 3 is connected to an electric furnace (high frequency furnace: a ceramic crucible was used in the past, but a carbon crucible is used in the present invention) 7 for melting the granulated metal. The atmospheric gas adjusted to a prescribed composition by a mixed gas tank 8 is supplied to the inside of the granulation chamber 1 and the upper part of the electric furnace 7 through pipes 9 and 10, respectively. The pressure in the granulation chamber 1 is controlled by a valve 11 and an exhaust device 12, and the pressure in the electric furnace 7 is controlled by a valve 13 and an exhaust device 14. The molten metal supplied from the nozzle 3 to the dish-shaped rotating disk 4 is dispersed in the form of fine droplets by the centrifugal force generated by the dish-shaped rotating disk 4, and is cooled under reduced pressure to become solid particles. The generated solid particles are supplied from the discharge pipe 6 to the automatic filter 15 and classified. Reference numeral 16 is a particle recovery device.

[0060] The process of cooling and solidifying the molten metal from high temperature is important for forming the metal particles of the present invention.

[0061] For example, the following conditions can be mentioned.

[0062] The melting temperature of the metal in the melting furnace 7 is set to 800° C. to 1000° C., and the molten metal is supplied from the nozzle 3 to the dish-shaped rotating disk 4 while maintaining the temperature.

[0063] As the dish-shaped rotating disk 4, a dish-shaped disk with an inner diameter of 35 mm and a rotating body thickness of 5 mm was used, and the rotation speed was set to 80,000 to 100,000 revolutions per minute.

[0064] As the granulation chamber 1, a granulation chamber having a reduced pressure of 9×10 -2 After the pressure in the vacuum tank with a performance of about 100 Pa was reduced, nitrogen gas at 15 to 50° C. was supplied and exhausted at the same time, and the pressure in the granulation chamber 1 was set to 1×10 -1 Below Pa.

[0065] The metal particles of the present invention are obtained in the above manner. The particle size of the metal particles of the present invention is approximately 5 μm, but the particle size of the metal particles of the present invention is preferably in the range of 1 μm to 50 μm, for example.

[0066] Next, the obtained metal particles of the present invention are melted by high-frequency induction heating in a vacuum, cast in a mold in a nitrogen atmosphere at atmospheric pressure, cooled and solidified to form a rolled sheet, and a plurality of sheets are stacked as needed to obtain a block.

[0067] The above-mentioned high-frequency induction heating and cooling and solidification conditions are important for forming the electrode for electrolytic plating of the present invention.

[0068] For example, the following conditions can be mentioned.

[0069] High frequency induction heating: can reduce the pressure to 9×10 -2 A crucible for high-frequency dissolution is set in a vacuum tank with a performance of about 1.447 Pa, and the metal particles of the present invention are introduced into the crucible. The metal particles of the present invention are subjected to high-frequency induction heating while the pressure is reduced to the above-mentioned reduced pressure level. The heating temperature is set to 800°C to 1000°C to melt the metal particles of the present invention, and the temperature is maintained for 5 minutes to 15 minutes.

[0070] Cooling and solidification: Next, nitrogen gas at 15 to 50° C. is flowed in the tank, and the heating temperature is set to about 400° C. or higher under atmospheric pressure, and mold casting is performed, followed by cooling and solidification at 30° C. or lower.

[0071] The electrode for electrolytic plating of the present invention may be composed of:

[0072] Cu: 0.7-15 mass %,

[0073] Cr: 0.001 to 1 mass %,

[0074] Ni: 0.01-5% by mass

[0075] The remainder is Sn (which may contain unavoidable impurities in an amount of 0.1 mass % or less).

[0076] The above composition is the same as that of the metal particles of the present invention.

[0077] In addition, the composition of the parent phase in the electrode for electrolytic plating can be Cu: 5 mass% or less (e.g. 0.1-5 mass%), Ni: 1 mass% or less (e.g. 0.01-1 mass%), Cr: 1 mass% or less (e.g. 0.01-1 mass%), and the remainder is Sn.

[0078] The composition of the above-mentioned parent phase is the same as that of the metal particles of the present invention.

[0079] Furthermore, the composition of the intermetallic compound crystals in the electrode for electrolytic plating of the present invention is preferably:

[0080] Sn: 50-70 mass %,

[0081] Cu: 30-50 mass %,

[0082] Cr: 0.001 to 3 mass %,

[0083] Ni: 0.01 to 6.5 mass %.

[0084] The ratio of the intermetallic compound crystals in the electrode for electrolytic plating of the present invention is, for example, 20 to 60 mass %, or preferably 30 to 40 mass % based on the entire electrode for electrolytic plating.

[0085] The intermetallic compound crystals are contained and present in the matrix phase.

[0086] The composition and ratio of the parent phase and the intermetallic compound crystals in the electrode for electrolytic plating of the present invention can be satisfied by following the manufacturing conditions of the electrode for electrolytic plating. It should be noted that the inventors have confirmed that the structure of the electrode for electrolytic plating of the present invention can be maintained even if rolled sheets and blocks are formed.

[0087] The electrode for electrolytic plating of the present invention is preferably formed by epitaxially bonding the above-mentioned parent phase and at least one part of the above-mentioned intermetallic compound crystal. As described above, the so-called epitaxial bonding is to precipitate intermetallic compound crystals in the substance that becomes the metal-alloy (the parent phase in the present invention), and the precipitated intermediate Sn-Cu alloy is bonded to the intermetallic compound crystal at the lattice level to form grains. By forming the epitaxial bonding, the problem of the brittleness of the intermetallic compound crystal can be solved, and the reduction in mechanical strength caused by the change in the crystal structure of Sn can also be suppressed, and a contact terminal with excellent durability can be provided.

[0088] The epitaxial bonding of the electrode for electrolytic plating of the present invention can be formed according to the manufacturing conditions of the electrode for electrolytic plating described above.

[0089] In addition, regarding epitaxial bonding, when the entire bonding surface of the Sn-Cu alloy in the matrix and the intermetallic compound crystal is set to 100%, it is preferably 30% or more, and more preferably 60% or more. The ratio of epitaxial bonding can be calculated, for example, as follows.

[0090] An electron microscope photograph was taken of the cross section of the electrolytic plating electrode, and the bonding surface between the Sn-Cu alloy and the intermetallic compound crystal was randomly sampled at 50 locations. Next, the bonding surface was image analyzed to investigate the extent to which the epitaxial bonding described in the following examples existed on the sampled bonding surface.

[0091] In addition, the electrode for electrolytic plating of the present invention is useful as an electrode for electrolytic plating (anode) for forming the above-mentioned coating. Regarding the electrode for electrolytic plating of the present invention, the intermetallic compound crystals contained in the electrode for electrolytic plating are dispersed in a plating bath in nanometer size (less than 1 μm), and are plated on the surface of the substrate together with the parent phase along with being charged to form a coating. The formed coating preferably has a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a parent phase containing a Sn-Cu alloy, and at least one part of the parent phase and the intermetallic compound crystals are epitaxially bonded. In addition, epitaxial bonding is preferably performed between the substrate.

[0092] The plating bath for forming the above-mentioned plating layer may have, for example, the following composition in addition to comprising the electrode for electrolytic plating of the present invention.

[0093] Copper sulfate: 180~250g / L

[0094] Stannous sulfate: 30~50g / L

[0095] Sulfuric acid: 80~120g / L

[0096] Various additives, etc. (adhesion inhibitors, interface complexation forming materials, film forming materials, electric field diffusion consumption forming materials)

[0097] In addition to the above-mentioned examples of the components of the plating bath, known dispersants, brighteners, antioxidants, etc. may be appropriately added as needed. For example, dispersants such as polyoxyethylene cumylphenyl ether and polyoxyethylene lauryl ether, brighteners such as cresol sulfonic acid, acetaldehyde, and acetylacetone, and antioxidants such as formalin, catechol, and hydroquinone may be mentioned.

[0098] The plating temperature is, for example, 30°C or lower, preferably 15 to 20°C.

[0099] The current density can be, for example, 1 to 10 A / dm 2 Adjust appropriately within the range.

[0100] The composition of the intermetallic compound crystals contained in the above-mentioned plating layer is the same as that of the electrode for electrolytic plating of the present invention. That is, for example:

[0101] Sn: 50-70 mass %,

[0102] Cu: 30-50 mass %,

[0103] Cr: 0.001 to 3 mass %,

[0104] Ni: 0.01 to 6.5 mass %.

[0105] In addition, the amount of intermetallic compound crystals contained in the above-mentioned plating layer is, for example, 20 to 60% by mass. The composition of the parent phase is also the same as the composition of the electrode for electrolytic plating of the present invention. That is, the composition of the parent phase is Cu: 5% by mass or less, Ni: 1% by mass or less, Cr: 1% by mass or less, and the remainder is Sn (which may contain unavoidable impurities of 0.1% by mass or less).

[0106] The above-mentioned composition and structure of the entire plating layer, the matrix phase, and the intermetallic compound can be formed by the above-mentioned plating conditions using the electrode for electrolytic plating of the present invention.

[0107] The plated substrate is then subjected to a heat treatment, and the heat treatment conditions include, for example, a temperature of 100 to 300° C. and a heating time of about 5 to 30 seconds.

[0108] Through the above operation, a plating layer is formed on the surface of the base material. The thickness of the plating layer is, for example, 2 μm to 10 μm.

[0109] It should be noted that, as the base material, aluminum, aluminum alloy, copper, copper alloy or stainless steel can be listed, and they can be selected from known materials without particular limitation. For example, as the copper alloy, brass, phosphor bronze, etc. can be listed.

[0110] Furthermore, when the terminal of the present invention is used as a micro bump, Si, SiC, or GaN is suitable as the base material.

[0111] In addition, as another embodiment, the present invention provides a bump. The bump of the present invention has the same composition as the terminal of the present invention described above. That is, the bump of the present invention is formed by forming a plating layer on the surface of the substrate, and the plating layer has a structure in which intermetallic compound crystals containing Sn, Cu, Cr and Ni are dispersed in a parent phase containing Sn and Sn-Cu alloy. The details of the plating layer of the bump of the present invention are the same as the plating layer of the terminal of the present invention described above, so the detailed description is omitted.

[0112] It should be noted that a titanium, nickel or nickel alloy layer may be formed in the base of the plated layer to further improve heat resistance. As the nickel alloy, one or two nickel alloys containing iron, tin, zinc, copper, cobalt, phosphorus, silver, boron, etc. may be used. The thickness of the base layer is preferably about 0.1 μm to 1.5 μm, for example.

[0113] Example

[0114] Hereinafter, the present invention will be further described with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0115] Example 1

[0116] As a raw material, a raw material containing 8 mass % of Cu, 1 mass % of Cr, 1 mass % of Ni and the remainder of Sn was used. Figure 4 The manufacturing apparatus shown in , manufactures metal particles 1 having a diameter of about 3 to 50 μm.

[0117] At this time, the following conditions were adopted.

[0118] A melting crucible is provided in the melting furnace 7, and the above raw materials are put into the crucible to be melted at 900°C. While the temperature is maintained, the molten metal is supplied from the nozzle 3 to the pan-shaped rotating disk 4.

[0119] As the dish-shaped rotating disk 4, a dish-shaped disk with a diameter of 35 mm and a rotating disk thickness of 3 to 5 mm was used, and the rotation speed was set to 80,000 to 100,000 revolutions per minute.

[0120] As the granulation chamber 1, a granulation chamber having a reduced pressure of 9×10 -2 After the pressure was reduced by a vacuum tank with a performance of about 10 Pa, nitrogen gas at 15 to 50° C. was supplied and exhausted at the same time, and the pressure in the granulation chamber 1 was set to 1×10 -1 Below Pa.

[0121] The obtained metal powder 1 is used to produce the electrode for electrolytic plating of the present invention.

[0122] At this time, the following conditions were adopted.

[0123] High frequency induction heating: can reduce the pressure to 9×10 -2 A high-frequency melting crucible is set in a vacuum tank with a performance of about 0.04 Pa, and the metal particles of the present invention are introduced into the crucible. The metal particles of the present invention are subjected to high-frequency induction heating under a state of reduced pressure to the above-mentioned reduced pressure degree. The heating temperature is set to 900°C to melt the metal particles of the present invention, and the temperature is maintained for 5 minutes.

[0124] Cooling and solidification: Next, nitrogen gas at 15 to 50° C. was flowed in the tank for 10 minutes, and the raw material was heated to about 400° C. under atmospheric pressure, cast in a mold, and cooled and solidified at room temperature.

[0125] The obtained material was rolled into sheets, put into a cutting machine heated to 150° C., and cut into 1 cm to 3 cm squares to obtain the electrode for electrolytic plating of Example 1, which was placed in the following plating bath.

[0126] The obtained electrode for electrolytic plating of Example 1 has the above Figure 1 In addition, Figure 2This is a cross-sectional SEM image of the obtained electrode for electrolytic plating of Example 1, and it is confirmed that intermetallic compound crystals (dark color) are contained in the matrix (light color).

[0127] In addition, element mapping analysis was performed on a cross section of the electrolytic plating electrode using EDS (see Figure 3 ), and the results showed that its composition was Cu: 8 mass%, Cr: 1 mass%, Ni: 1 mass%, and the remainder Sn.

[0128] Furthermore, it was found that the electrode for electrolytic plating of Example 1 contained intermetallic compound crystals in the matrix phase, and at least one part of the matrix phase and the intermetallic compound crystals were epitaxially bonded.

[0129] It should be noted that the composition including the intermetallic compound crystal and the epitaxial bonding portion was found to be:

[0130] Sn: 50-70 mass %,

[0131] Cu: 30-50 mass %,

[0132] Cr: 0.001 to 3 mass %,

[0133] Ni: 0.01 to 6.5 mass %.

[0134] Furthermore, the intermetallic compound crystals in the above-mentioned electrode for electrolytic plating account for 30 to 35% by mass.

[0135] (Contact terminal preparation)

[0136] As a substrate (cathode), a phosphor bronze or brass plate (thickness: 0.30 mm) was used.

[0137] The substrate was subjected to electrolytic plating under the following conditions using the electrode for electrolytic plating of the present invention as an electrode for electrolytic plating to obtain a plated sheet.

[0138] Plating bath composition (concentration relative to 1 liter of water):

[0139] Copper sulfate: 180~250g / L

[0140] Stannous sulfate: 30~50g / L

[0141] Sulfuric acid: 80~120g / L

[0142] In addition, a known reference electrode is used and an appropriate amount of additives is added.

[0143] Plating temperature: 70℃

[0144] Current density: 3A / dm 2

[0145] Heat treatment temperature of the plated substrate: 200°C

[0146] Heat treatment time of the plated substrate: 300 seconds (under nitrogen atmosphere)

[0147] The composition of the obtained contact terminal is the same as the composition of the electrode for electrolytic plating of the present invention described above.

[0148] The durability of the contact terminal obtained in the above-mentioned Example 1 was investigated by the following experiment.

[0149] <Durability test method>

[0150] (180℃ bending test)

[0151] The contact terminal using a brass plate as a base material was subjected to a 180-degree bending test to observe the presence or absence of cracks in the plating layer. The thickness of the plating layer was 5 μm. Figure 5 The following are microscope photographs showing the results of a 180-degree bending test of the contact terminal of Example 1 (a is a photograph of the entire contact terminal, and b is an enlarged photograph of the bent portion). As a result, no cracks were observed in the plating layer of the contact terminal of Example 1.

[0152] (Surface crack test)

[0153] The obtained contact terminal was punched from the back side and subjected to a surface crack test. Figure 6 1 is a micrograph showing the results of a surface crack test of the contact terminal of Example 1. As a result, no surface cracks due to punching were observed in the plating layer of the contact terminal of Example 1.

[0154] (Heat resistance test)

[0155] The obtained contact terminal was left to stand at a temperature of 250° C. for 500 hours, and the state of the surface of the plating layer was observed with a microscope. Figure 7 This is a microscopic photograph showing the results of the heat resistance test of Example 1. No change was observed in the plating layer of the contact terminal of Example 1 before and after the heat resistance test.

[0156] Comparative Example 1

[0157] In Example 1, Example 1 was repeated except that the electrolytic plating electrode was changed to tin metal, and the 180° C. bending test, surface crack test, and heat resistance test were performed.

[0158] Figure 8 : is a microscope photograph showing the result of the 180 degree bending test of the contact terminal of Comparative Example 1. As a result, in the 180 degree bending test, cracks occurred in the plating layer, and separation between the plating layer and the base material occurred.

[0159] Fig. 9 : is a microscope photograph showing the result of the surface crack test of Comparative Example 1. As a result, in the plating layer of the contact terminal of Comparative Example 1, surface cracks caused by punching were confirmed.

[0160] Fig.10 : is a micrograph showing the result of the heat resistance test of Comparative Example 1. As a result, it was confirmed that the plating layer of the contact terminal of Comparative Example 1 was partially melted under the heating condition of standing at 250° C. for 500 hours.

[0161] As mentioned above, the present invention has been described in detail with reference to the accompanying drawings, but the present invention is not limited to these drawings, and a person skilled in the art can of course conceive various modifications based on the basic technical concept and teachings thereof.

Claims

1. A terminal having a plated layer formed on the surface of a substrate, The plating layer has a structure in which intermetallic compound crystals containing Sn, Cu, Cr, and Ni are dispersed in a matrix containing Sn and a Sn-Cu alloy.

2. The terminal according to claim 1, wherein: The composition of the coating is: Cu: 0.7-15 mass %, Cr: 0.001 to 1 mass %, Ni: 0.01 to 5 mass %, The remainder is Sn, which may contain unavoidable impurities in an amount of 0.1 mass % or less. The composition of the parent phase is Cu: 5 mass % or less, Ni: 1 mass % or less, Cr: 1 mass % or less, and the remainder is Sn, wherein unavoidable impurities of 0.1 mass % or less may be contained.

3. The terminal according to claim 1, wherein: The composition of the intermetallic compound crystal is: Sn: 50-70 mass %, Cu: 30-50 mass %, Cr: 0.001 to 3 mass %, Ni: 0.01 to 6.5 mass %.

4. The terminal according to claim 1, wherein: A titanium, nickel or nickel alloy layer is formed in the base of the plated layer.

5. The terminal according to claim 1, wherein The substrate is made of aluminum, aluminum alloy, copper, copper alloy or stainless steel.

6. The terminal according to claim 1, wherein The substrate is made of Si, SiC or GaN.

7. A bump, which is a bump formed by forming a plating layer on the surface of a substrate, The plating layer has a structure in which intermetallic compound crystals containing Sn, Cu, Cr, and Ni are dispersed in a matrix containing Sn and a Sn-Cu alloy.

Citation Information

Patent Citations

  • Tin-copper intermetallic compound-dispersed tinned terminal

    JP2003082499A