An epoxy resin-based electromagnetic shielding composite material with a layered gradient structure and a preparation method thereof
By adopting layered gradient structure and 3D printing technology in electromagnetic shielding materials, using the proportion and distribution of components of different functional fillers, the problems of high reflection coefficient and insufficient performance of existing electromagnetic shielding materials are solved, and efficient electromagnetic wave absorption and The effect of reducing secondary pollution.
Patent Information
- Application Number
- CN202411275166.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-12
AI Technical Summary
While the existing electromagnetic shielding materials improve electromagnetic shielding performance, the high reflection coefficient leads to secondary pollution of electromagnetic waves. The conductive and mechanical properties of polymer-based electromagnetic shielding materials are insufficient, making it difficult to meet the complex electromagnetic environment needs.
Using epoxy resin-based electromagnetic shielding composite material with a layered gradient structure, a multi-layer composite shielding layer is prepared through 3D printing technology, and the component proportions and distribution of different functional fillers can be used to achieve gradient changes in conductivity and magnetic permeability, forming " The multiple shielding effect of absorption-reflection-reabsorbing" reduces the reflection coefficient and improves electromagnetic shielding performance.
It realizes that while ensuring electromagnetic shielding performance, it reduces electromagnetic wave reflection, improves the absorption loss of electromagnetic energy, and reduces secondary pollution. The material has good shape memory performance and mechanical properties.
Smart Images

Figure CN118785684B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electromagnetic shielding composite materials, and in particular to an epoxy resin-based electromagnetic shielding composite material with a layered gradient structure and a preparation method thereof. Background Art
[0002] With the development of science and technology, more and more electronic products have entered our lives, and these electronic devices will generate a large amount of electromagnetic waves, which will not only cause electromagnetic interference (EMI) to other electronic devices, instruments, communication signals, etc., but also cause a lot of harm to the human body, such as dizziness, insomnia, memory loss, palpitations, etc. Electromagnetic waves have become another major source of pollution after water pollution, air pollution, and noise pollution. With the advent of the 5G era, it is imperative to develop electromagnetic shielding materials with excellent performance in response to the increasingly complex electromagnetic environment.
[0003] Electromagnetic shielding materials usually shield electromagnetic waves in the form of absorption or reflection to protect sensitive electronic devices. Metal materials have excellent electrical conductivity, can reflect most of the electromagnetic waves, and have excellent electromagnetic shielding performance. However, compared with polymers, metals have disadvantages such as high density, poor corrosion resistance and difficulty in processing, which limit their wide application in electromagnetic shielding materials; polymer-based electromagnetic shielding materials have the characteristics of light weight, good corrosion resistance and flexible preparation methods, making their application more extensive. Polymer-based electromagnetic shielding materials are mainly divided into two categories. One is directly prepared from intrinsic conductive polymers, such as polypyrrole, polythiophene, and polyacetylene. The conductivity and mechanical properties of these polymers are poor, which limits their development in the field of electromagnetic shielding; the other is polymer-based electromagnetic shielding composite materials prepared by polymer doping carbon and metal conductive fillers. By flexibly designing the structure of the composite material, the percolation threshold can be effectively reduced, the conductivity of the composite filler can be improved, and the influence of excessive filler content on the mechanical properties of the composite material can be avoided. However, shielding materials with too high conductivity will have impedance mismatch with the air, causing a large amount of electromagnetic wave reflection and secondary pollution. In order to reduce the reflection coefficient, some scholars have designed shielding materials that mainly absorb losses. In order to better adjust the various properties of shielding materials, a large amount of research is currently focused on the structural design of composite electromagnetic shielding materials. Summary of the invention
[0004] The present invention provides an epoxy resin-based electromagnetic shielding composite material with a layered gradient structure and a preparation method thereof. The composite material provided by the present invention has a positive electrical conductivity gradient and a reverse magnetic conductivity gradient along the incident direction of electromagnetic waves, and has good electromagnetic shielding performance while having a low reflection coefficient and shape memory performance.
[0005] The first object of the present invention is to provide an epoxy resin-based electromagnetic shielding composite material with a layered gradient structure, comprising a first shielding layer, a second shielding layer, a third shielding layer and a fourth shielding layer arranged in sequence from top to bottom, wherein the first shielding layer, the second shielding layer, the third shielding layer and the fourth shielding layer are all prepared by 3D printing, and the raw materials of the 3D printing ink used in each shielding layer are composed of the following components: epoxy resin, methyl hexahydrophthalic anhydride, N, N-dimethylbenzylamine, polyether polyol, acetylene carbon black and functional filler; wherein the functional filler of the fourth shielding layer is Flake silver powder, and the mass percentage of flaky silver powder in the raw material is 19-21%; the functional filler of the third shielding layer is multi-walled carbon nanotubes and nickel powder, and the mass percentage of the multi-walled carbon nanotubes and nickel powder in the raw material is 0.5-1.5% and 5-7%, respectively; the functional filler of the second shielding layer is multi-walled carbon nanotubes and nickel powder, and the mass percentage of the multi-walled carbon nanotubes and nickel powder in the raw material is 0.4-0.6% and 9-11%, respectively; the functional filler of the first shielding layer is nickel powder, and the mass percentage of nickel powder in the raw material is 13-15%.
[0006] Compared with the prior art, the present invention adopts 3D printing to prepare a multi-layer composite shielding layer, and adopts the above-mentioned four-layer shielding layer with different functional fillers and component proportions. This is because: the conductivity of different filler layers is different, and there will be a certain impedance mismatch between the layers, which will cause interlayer electromagnetic wave reflection. In order to make the surface layer impedance match as good as possible, avoid excessive surface layer reflection, and allow more electromagnetic waves to enter the interior of the composite material, the surface layer of the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure of the present invention selects a first shielding layer with low conductivity and high magnetic permeability, and the conductivity of the following three layers gradually increases, and the magnetic permeability gradually decreases. The bottom layer selects the fourth shielding layer with the highest conductivity, which can weaken the penetration of electromagnetic waves into the composite material, reflect the electromagnetic waves and enter the absorption layer again, and convert the electromagnetic waves into internal energy in the form of dielectric loss and magnetic loss. After the electromagnetic waves enter the composite material, they are reflected and absorbed multiple times between layers to form an "absorption-reflection-reabsorption" shielding effect, so that SE A There has been some improvement.
[0007] In some embodiments, in each shielding layer, the mass ratio of the epoxy resin to the polyether polyol is 100:(2-3), the mass ratio of the methylhexahydrophthalic anhydride to the epoxy resin is (80-90):185, the mass ratio of the N,N-dimethylbenzylamine to the epoxy resin is (0.5-1.5):100, and the mass ratio of the acetylene black to the epoxy resin is (11-13):100.
[0008] Compared with the prior art, the present invention prepares printing ink by mixing epoxy resin with metal, methylhexahydrophthalic anhydride, N,N-dimethylbenzylamine, polyether polyol, acetylene carbon black and functional filler. The preparation method is simple and quick, and the epoxy resin matrix used has good shape memory performance. The shape memory function can be realized through thermal, electrical, magnetic and other excitation methods. The shielding material can be better attached to complex surfaces through such excitation. When the equipment is damaged, the shielding material can be recycled by re-excitation to save manufacturing costs.
[0009] Further, the present invention adopts the component content of the above mass ratio, wherein epoxy resin is used as a matrix material to provide the basic structure and mechanical properties of the composite material, and polyether polyol is added at a smaller ratio to improve the flexibility of the epoxy resin, methyl hexahydrophthalic anhydride is used as a curing agent to chemically react with the epoxy resin to form a stable polymer network, and its optimal content is 85:185, N, N-dimethylbenzylamine is used as a curing accelerator or catalyst to accelerate the reaction rate between the epoxy resin and the curing agent, so its content is less, acetylene black is a key conductive filler in the composite material, providing the necessary electromagnetic shielding performance, but excessive acetylene black will affect the microstructure of the material, resulting in poor dispersion or agglomeration, thereby affecting the overall mechanical properties. In summary, the present invention adopts the component composition of the above ratio.
[0010] The second object of the present invention is to provide a method for preparing an epoxy resin-based electromagnetic shielding composite material having a layered gradient structure, the preparation method specifically comprising the following steps:
[0011] S1, preparing printing ink for the first shielding layer;
[0012] S2, preparing printing ink for the second shielding layer;
[0013] S3, preparing printing ink for the third shielding layer;
[0014] S4, preparing printing ink for the fourth shielding layer;
[0015] S5. Use 3D software to draw a 3D model, import it into a direct writing 3D printer and set the printer parameters. Place the prepared printing ink in the printing syringes respectively, and then use the direct writing 3D printer to print layer by layer in the order of the fourth shielding layer, the third shielding layer, the second shielding layer and the first shielding layer. After printing, place it in a drying oven to heat and cure.
[0016] Compared with the prior art, the present invention adopts direct writing 3D printing technology and controls the distribution of fillers by printing layer by layer. The prepared electromagnetic shielding material has a forward conductive gradient and a reverse magnetic conductive gradient along the incident direction of the electromagnetic wave. This gradient structure can form a multiple reflection and absorption loss effect of "absorption-reflection-reabsorption" for electromagnetic waves, which is beneficial to reduce the surface reflection of electromagnetic waves while ensuring good electromagnetic shielding performance, and convert more electromagnetic energy into internal energy dissipation.
[0017] In some embodiments, in step S1, the preparation method of the printing ink of the first shielding layer includes the following steps: placing an epoxy resin in a container, adding a polyether polyol according to a mass ratio, and then placing it in a drying oven and preheating it to 75-78°C to fully dissolve it, and then adding methyl hexahydrophthalic anhydride and N, N-dimethylbenzylamine in sequence, and then adding acetylene carbon black, after mechanically stirring for 50-60 min, adding nickel powder and stirring for 30-35 min, after stirring, filtering with a filter cloth with a pore size of 80-82 μm and vacuuming for 10-12 min to obtain the printing ink of the first shielding layer.
[0018] In some embodiments, in step S2, the preparation method of the printing ink for the second shielding layer includes the following steps: placing an epoxy resin in a container, adding a polyether polyol according to a mass ratio, and then placing it in a drying oven and preheating it to 75-78°C to fully dissolve it, adding multi-walled carbon nanotubes and ultrasonically vibrating it for 10-12 min, and then adding methyl hexahydrophthalic anhydride and N, N-dimethylbenzylamine in sequence, and then adding acetylene black, mechanically stirring for 50-60 min, then adding nickel powder and stirring for 30-35 min, after stirring, filtering with a filter cloth with a pore size of 80-82 μm and vacuuming for 10-12 min to obtain the printing ink for the second shielding layer.
[0019] In some embodiments, in the step S3, the preparation method of the printing ink of the third shielding layer includes the following steps: placing an epoxy resin in a container, adding a polyether polyol according to a mass ratio, and then placing it in a drying oven and preheating it to 75-78°C to fully dissolve it, adding multi-walled carbon nanotubes and ultrasonically vibrating it for 10-12 min, and then adding methyl hexahydrophthalic anhydride and N, N-dimethylbenzylamine in sequence, and then adding acetylene carbon black, mechanically stirring for 50-60 min, then adding nickel powder and stirring for 30-35 min, after stirring, filtering with a filter cloth with a pore size of 80-82 μm and vacuuming for 10-12 min to obtain the printing ink of the third shielding layer.
[0020] In some embodiments, in step S4, the preparation method of the printing ink of the fourth shielding layer includes the following steps: placing an epoxy resin in a container, adding a polyether polyol according to a mass ratio, and then placing it in a drying oven to preheat to 75-78°C to fully dissolve it, and then adding methyl hexahydrophthalic anhydride and N, N-dimethylbenzylamine in sequence, and then adding acetylene carbon black, after mechanically stirring for 50-60 minutes, adding flaky silver powder and stirring for 30-35 minutes, after stirring, filtering with a filter cloth with a pore size of 80-82 μm and vacuuming for 10-12 minutes to obtain the printing ink of the fourth shielding layer.
[0021] In some embodiments, in step S5, the parameters of printing using a direct writing 3D printer are as follows: the printing needle diameter is 0.41-0.42 mm, the layer height is set to 0.4-0.41 mm, each ink is printed one layer in sequence, the printing speed is 10-11 mm / s, the printing spacing is 0.4-0.5 mm, the printing air pressure is 0.1-0.2 MPa, the broken wire height is 2 mm, and the early wire ejection is 200-202 ms.
[0022] Compared with the prior art, the present invention further limits the parameters of direct writing 3D printer printing, mainly because: 1. A larger needle diameter results in less fine details, while a smaller needle diameter can result in slower printing speed; 2. A thinner layer height can improve printing accuracy, but will increase printing time; a thicker layer height can shorten printing time, but may affect the surface quality and details of the print; 3. The printing speed is selected to be 10-11 mm / s, because this is a relatively moderate printing speed, which can ensure good deposition and curing of materials during printing, while avoiding printing quality problems caused by too fast speed; 4. 0.4-0.5 The spacing of 2mm can ensure the continuity of the material and a good coverage area, and it also matches the layer height, which helps to improve printing efficiency and quality; 5. The setting of the air pressure directly affects the extrusion amount of the material and the stability of the printing process. Lower air pressure can reduce the extrusion of the material and is suitable for printing fine structures; higher air pressure can increase the extrusion amount and increase the printing speed. Within the range of 0.1~0.2MPa, the air pressure can be adjusted according to actual needs to obtain the best printing effect; 6. When the needle needs to be raised during printing to avoid collision with the already printed structure, the 2mm lifting distance can ensure sufficient space to avoid damage to the already printed part; 7. During the printing process, early filament extraction is to ensure that the material has begun to extrude before moving to the next printing position, which helps to maintain the continuity of the material and avoid gaps or breakpoints.
[0023] In some embodiments, in step S5, the specific steps of heating and curing are: heating at 90-92°C for 30-32 minutes, heating to 118-120°C for 1-1.2 hours, then heating to 140-145°C for 30-32 minutes, and finally heating to 150-160°C for 2-2.5 hours.
[0024] Compared with the prior art, the curing process of the present invention adopts a gradual temperature increase method, which can reduce the accumulation of internal stress of the material and prevent the material from cracking during the curing process. The timing of each stage is to ensure that the material has enough reaction time at the temperature to achieve sufficient curing. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a physical picture of the printing effect of the first two layers of the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5 of the present invention;
[0026] Figure 2 1 to 4 are filler dispersion diagrams of embodiments 1 to 4 of the present invention; wherein a is the filler dispersion diagram of embodiment 1; b is the filler dispersion diagram of embodiment 2; c is the filler dispersion diagram of embodiment 3; d is the filler dispersion diagram of embodiment 4;
[0027] Figure 3 This is a cross-sectional SEM image of the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5 of the present invention;
[0028] Figure 4 The silver element in the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5 of the present invention is Figure 3 Element mapping at ;
[0029] Figure 5 The nickel element in the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5 of the present invention is Figure 3 Element mapping at ;
[0030] Figure 6 Schematic diagram of the conductivity of the electromagnetic shielding materials prepared in Examples 1-4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0031] Figure 7 Schematic diagram of the real part of the complex dielectric constant of the electromagnetic shielding materials prepared in Examples 1-4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0032] Figure 8Schematic diagram of the imaginary part of the complex dielectric constant of the electromagnetic shielding materials prepared in Examples 1-4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0033] Fig. 9 Schematic diagram of the complex dielectric constant and dielectric loss factor of the electromagnetic shielding materials prepared in Examples 1-4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0034] Fig.10 A schematic diagram of the hysteresis loop of the electromagnetic shielding material prepared in Examples 1-3 of the present invention;
[0035] Fig.11 Schematic diagram of the real part of the complex magnetic permeability of the electromagnetic shielding materials prepared in Examples 1-3 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0036] Fig.12 Schematic diagram of the imaginary part of the complex magnetic permeability of the electromagnetic shielding materials prepared in Examples 1-3 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0037] Fig.13 A schematic diagram of the magnetic loss tangent values of the electromagnetic shielding materials prepared in Examples 1-3 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0038] Fig.14 The overall performance diagram of the electromagnetic shielding materials prepared in Examples 1 to 4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0039] Fig.15 The reflection efficiency diagram of the electromagnetic shielding materials prepared in Examples 1 to 4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0040] Fig.16 Absorption efficiency diagram of the electromagnetic shielding materials prepared in Examples 1-4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0041] Fig.17 Reflection coefficient diagrams of the electromagnetic shielding materials prepared in Examples 1-4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5;
[0042] Fig.18 A schematic diagram of the electromagnetic shielding mechanism of the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5 of the present invention;
[0043] Fig.19 This is the S parameter test schematic. DETAILED DESCRIPTION
[0044] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. It should be noted that the following embodiments are only used to illustrate the implementation method and typical parameters of the present invention, and are not used to limit the parameter range described in the present invention. Reasonable changes derived therefrom are still within the scope of protection of the claims of the present invention.
[0045] It should be noted that the endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this article.
[0046] Unless otherwise defined, all terms, symbols and other scientific terms used herein are intended to have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. In some cases, terms with conventionally understood meanings are defined herein for the purpose of clarification or ease of reference, and such definitions herein should not be construed as indicating significant differences from conventional understandings in the art. The technical methods described or cited herein are generally well understood by those skilled in the art and are adopted by conventional methods. Unless otherwise stated, the use of commercially available kits, reagents and instruments is carried out in accordance with the protocols and parameters given by the manufacturer.
[0047] The technical effects of the present invention are described below in conjunction with specific embodiments.
[0048] In this embodiment, Examples 1-4 use inks A, B, C, and D to print four layers respectively, and Example 5 uses each ink to print one layer in sequence.
[0049] Example 1
[0050] This embodiment provides an electromagnetic shielding material, which is prepared by the following method:
[0051] S1. Preparation of printing ink: weigh 20g of epoxy resin in a mixing cup, add 0.6g of polyether polyol at a mass ratio of 100:3, place in a drying oven and preheat to 78°C to fully dissolve, then add 9.2g of methyl hexahydrophthalic anhydride and 0.2g of N, N-dimethylbenzylamine at a mass ratio of 185:85 and 100:1, respectively, and then add 2.4g of acetylene black, use a stirrer to mechanically stir at a speed of 800 rpm for 60 min, then add 2.8g of nickel powder and stir for 30 min, after stirring, filter with a filter cloth with a pore size of 80 μm and evacuate for 10 min, transfer the prepared ink to the printing syringe, and record the ink as A;
[0052] S2. Preparation of electromagnetic shielding materials: Use 3D software to draw a 3D model, import it into a direct writing 3D printer of model Bio-Printer-ws (China) and set the printer parameters. Place the prepared printing ink in the printing syringe and use the direct writing 3D printer to print layer by layer in sequence. After printing, place it in a drying oven for heating and curing. Among them, the printing parameters of the direct writing 3D printer are as follows: the printing needle diameter is 0.41mm, the layer height is set to 0.4 mm, the number of layers is 4, the printing speed is 10 mm / s, the printing spacing is 0.4mm, the printing pressure is 0.1~0.2 MPa, the broken wire height is 2mm, and the early wire is 200ms; the specific steps of heating and curing are: heating at 90℃ for 30 min, heating to 120℃ for 1 h, then heating to 140℃ for 30 min, and finally heating to 160℃ for 2 h.
[0053] Example 2
[0054] This embodiment provides an electromagnetic shielding material, which is prepared by the following method:
[0055] S1. Preparation of printing ink: weigh 20g of epoxy resin in a mixing cup, add 0.6g of polyether polyol at a mass ratio of 100:3, place in a drying oven and preheat to 78°C to fully dissolve, add 0.1g of multi-walled carbon nanotubes and ultrasonically disperse for 10min, then add 9.2g of methyl hexahydrophthalic anhydride and 0.2g of N,N-dimethylbenzylamine at a mass ratio of 185:85 and 100:1, respectively, and then add 2.4g of acetylene black, use a stirrer to mechanically stir at a speed of 800 rpm for 60min, then add 2g of Ni powder and stir for 30min, after stirring, filter with a filter cloth with a pore size of 80 μm and evacuate for 10min, transfer the prepared ink to the printing syringe, and record the ink as B;
[0056] S2. Preparation of electromagnetic shielding materials: Use 3D software to draw a 3D model, import it into a direct writing 3D printer of model Bio-Printer-ws (China) and set the printer parameters. Place the prepared printing ink in the printing syringe and use the direct writing 3D printer to print layer by layer in sequence. After printing, place it in a drying oven for heating and curing. Among them, the printing parameters of the direct writing 3D printer are as follows: the printing needle diameter is 0.41mm, the layer height is set to 0.4 mm, the number of layers is 4, the printing speed is 10 mm / s, the printing spacing is 0.4mm, the printing pressure is 0.1~0.2 MPa, the broken wire height is 2mm, and the early wire is 200ms; the specific steps of heating and curing are: heating at 90℃ for 30 min, heating to 120℃ for 1 h, then heating to 140℃ for 30 min, and finally heating to 160℃ for 2 h.
[0057] Example 3
[0058] This embodiment provides an electromagnetic shielding material, which is prepared by the following method:
[0059] S1. Preparation of printing ink: weigh 20g of epoxy resin in a mixing cup, add 0.6g of polyether polyol at a mass ratio of 100:3, place in a drying oven and preheat to 78°C to fully dissolve, add 0.2g of multi-walled carbon nanotubes and ultrasonically disperse for 10min, then add 9.2g of methyl hexahydrophthalic anhydride and 0.2g of N,N-dimethylbenzylamine at a mass ratio of 185:85 and 100:1 in sequence, and then add 2.4g of acetylene black, use a stirrer to mechanically stir at a speed of 800 rpm for 60min, then add 1.2g of nickel powder and stir for 30min, after stirring, filter with a filter cloth with a pore size of 80 μm and evacuate for 10min, transfer the prepared ink to the printing syringe, and record the ink as C;
[0060] S2. Preparation of electromagnetic shielding materials: Use 3D software to draw a 3D model, import it into a direct writing 3D printer of model Bio-Printer-ws (China) and set the printer parameters. Place the prepared printing ink in the printing syringe and use the direct writing 3D printer to print layer by layer in sequence. After printing, place it in a drying oven for heating and curing. Among them, the printing parameters of the direct writing 3D printer are as follows: the printing needle diameter is 0.41mm, the layer height is set to 0.4 mm, the number of layers is 4, the printing speed is 10 mm / s, the printing spacing is 0.4mm, the printing pressure is 0.1~0.2 MPa, the broken wire height is 2mm, and the early wire is 200ms; the specific steps of heating and curing are: heating at 90℃ for 30 min, heating to 120℃ for 1 h, then heating to 140℃ for 30 min, and finally heating to 160℃ for 2 h.
[0061] Example 4
[0062] This embodiment provides an electromagnetic shielding material, which is prepared by the following method:
[0063] S1. Preparation of printing ink: weigh 20g of epoxy resin in a mixing cup, add 0.6g of polyether polyol at a mass ratio of 100:3, place in a drying oven and preheat to 78°C to fully dissolve, then add 9.2g of methylhexahydrophthalic anhydride and 0.2g of N,N-dimethylbenzylamine at a mass ratio of 185:85 and 100:1, respectively, and then add 2.4g of acetylene carbon black, use a stirrer to mechanically stir at a speed of 800 rpm for 60 min, then add 4g of flaky silver powder and stir for 30 min, after stirring, filter with a filter cloth with a pore size of 80μm and evacuate for 10 min, transfer the prepared ink to the printing syringe, and record the ink as D;
[0064] S2. Preparation of electromagnetic shielding materials: Use 3D software to draw a 3D model, import it into a direct writing 3D printer of model Bio-Printer-ws (China) and set the printer parameters. Place the prepared printing ink in the printing syringe and use the direct writing 3D printer to print layer by layer in sequence. After printing, place it in a drying oven for heating and curing. Among them, the printing parameters of the direct writing 3D printer are as follows: the printing needle diameter is 0.41mm, the layer height is set to 0.4 mm, the number of layers is 4, the printing speed is 10 mm / s, the printing spacing is 0.4mm, the printing pressure is 0.1~0.2 MPa, the broken wire height is 2mm, and the early wire is 200ms; the specific steps of heating and curing are: heating at 90℃ for 30 min, heating to 120℃ for 1 h, then heating to 140℃ for 30 min, and finally heating to 160℃ for 2 h.
[0065] Example 5
[0066] This embodiment provides an epoxy resin-based electromagnetic shielding composite material with a layered gradient structure, which is prepared by the following preparation method: using 3D software to draw a 3D model, importing it into a direct writing 3D printer and setting printer parameters, printing the printing ink prepared in Examples 1-4 layer by layer, as shown in the attached Figure 1 As shown, from bottom to top, the first shielding layer is printed with ink A, the second shielding layer is printed with ink B, the third shielding layer is printed with ink C, and the fourth shielding layer is printed with ink D. The printing effects of the third and fourth shielding layers are shown in the attached figure. Figure 1As shown, after printing is completed, it is placed in a drying oven for heating and curing; the parameters of the direct writing 3D printer are as follows: the printing needle diameter is 0.41mm, the layer height is set to 0.4 mm, each ink is printed one layer in sequence, the printing speed is 10 mm / s, the printing spacing is 0.4mm, the printing air pressure is 0.1~0.2 MPa, the broken wire height is 2mm, and the early wire is 200ms; the specific steps of heating and curing are: heating at 90℃ for 30 min, heating to 120℃ for 1 h, then heating to 140℃ for 30 min, and finally heating to 160℃ for 2 h.
[0067] Performance testing: To verify the microstructure of the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared by the present invention, the cross-section of the electromagnetic shielding materials prepared in Examples 1-4 was characterized using a scanning electron microscope (SEM) of model SU-70 (Japan) and an energy dispersive spectrometer of model APOLLO X (USA) to characterize the cross-section of the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5 and perform elemental analysis. The results are as follows: Figure 2-Figure 5 As shown, Figure 2 The SEM images of Examples 1-4, specifically, (a) is the SEM image of Example 1; (b) is the SEM image of Example 2; (c) is the SEM image of Example 3; and (d) is the SEM image of Example 4. Figure 3 is a SEM image of the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure of Example 5, Figure 4 for Figure 3 Silver element mapping image at Figure 5 for Figure 3 Nickel element mapping image at . Figure 2 It can be seen that the filler is evenly dispersed in the epoxy resin matrix. The one-dimensional multi-walled carbon nanotubes and the two-dimensional flaky silver powder have a higher bonding efficiency than the zero-dimensional nickel powder and are more likely to form a complete conductive path, which is beneficial to improving the conductivity of the composite material. Figure 3 It can be seen that after the composite materials printed with different inks are cured, the epoxy resin matrix is completely fused. Figure 4-5 It can be seen that the flaky silver powder is concentrated in the bottom layer, the nickel powder is distributed in the upper three layers, and the content gradually decreases from the top to the bottom.
[0068] Secondly, the conductive gradient of the composite material proposed in the present invention was verified. The resistance of the electromagnetic shielding materials prepared in Examples 1-4 and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5 was tested using a four-probe digital multimeter (DMM6500, USA). The conductivity was calculated according to formula (1). The results are shown in FIG. Figure 6As shown. Since good electrical conductivity is a prerequisite for effective shielding of electromagnetic waves, and since Ni powder and ACB are both zero-dimensional fillers, in Example 1 without MWCNT, the conductive path overlap efficiency is low, and the conductivity is 0.65 S / m. The one-dimensional carbon filler MWCNT can effectively improve the conductivity by forming a conductive path. In Example 2 and Example 3, 0.5 wt% and 1 wt% of MWCNT were added, respectively, and the Ni powder content was reduced from 14wt% to 10wt% and 6wt%, respectively. The conductive path overlap efficiency was increased, and the conductivity was significantly improved, which was 2.28 S / m and 6.18 S / m, respectively. On the basis of 12wt% ACB, 1.5 wt% of MWCNT was added to prepare a shielding layer. The length of MWCNT was between 20 and 30 μm, which was much smaller than the needle diameter (410 μm). The distribution of MWCNT was not affected by the printing path; while the conductivity of the composite material with 1.5wt% MWCNT added was only 6.80 S / m, at this time, MWCNT agglomerates, MWCNT dispersion is poor, the conductive path overlap efficiency is reduced, resulting in an insignificant improvement in conductivity. In order to improve the conductivity of the bottom shielding layer, flaky Ag powder is selected as a conductive filler, and 10 wt%, 20 wt%, and 30 wt% of Ag powder are added to 12 wt% ACB, respectively. The conductivity is 4.37 S / m, 12.80 S / m, and 15.27 S / m, respectively. By comparison, it is found that the conductivity of the composite material with 30 wt% Ag powder added is only 2.47 S / m higher than that of the composite material with 20 wt% Ag powder added. At this time, the amount of Ag powder added exceeds the percolation threshold, and the conductive path is relatively complete. Therefore, the bottom layer finally selects the composite material with 20 wt% Ag powder added as Example 4, as the shielding layer, to construct a positive conductive gradient. The conductivity of the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure obtained in Example 5 is 5.44 S / m, the conductivity of Example 5 with gradient structure is smaller than that of Example 4 with uniform structure. This is because the composite materials of uniform structure and gradient structure are both printed with 4 layers. Except for the shielding layer of Example 5 which uses the same ink as that of Example 4, the resistance of the other layers is greater than that of the single-layer Example 4. Therefore, the overall resistance is larger and the conductivity is smaller.
[0069]
[0070] In the formula is the conductivity, unit is S / m; L is the length of the sample, in m; S is the cross-sectional area of the sample, in m 2 ; R is the measured resistance value, unit is Ω.
[0071] The complex dielectric constants of the electromagnetic shielding materials prepared in Examples 1-4 and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5 were tested using a vector network analyzer model N5234A (USA). Figure 7 , Figure 8 and Fig. 9 are the real part of the complex dielectric constant of Ni-MWCNT / Ag / EP composite materials , imaginary part and dielectric loss tangent ,in . Reflects the ability of shielding materials to store electrical energy. Reflects its dielectric loss capacity. Dielectric loss can be divided into conductivity loss and polarization relaxation loss, usually expressed as To measure the dielectric loss capability of shielding materials. Figure 6 It can be found that As the conductivity of the composite material increases, it increases. This is because the higher the conductivity, the more conducive it is to electronic polarization, and the greater the polarization intensity, The larger the conductivity, the larger the Proportional, As the conductivity of the composite material increases. In addition, the high conductivity of the dielectric leads to high More electric dipoles can be provided. The electric dipoles move under the action of the alternating electric field and reach a certain polarization intensity after a period of time. This process is polarization relaxation. When the frequency of the electric field increases to a certain extent, the movement of these electric dipoles cannot keep up with the change of frequency and lags behind. In this process, the electric dipoles repeatedly turn to cause dielectric loss to the incident electromagnetic wave. More electric dipoles can also cause greater dielectric loss. The epoxy resin-based electromagnetic shielding composite material with a layered gradient structure of the present invention has a layered gradient structure and will also cause a certain interface polarization. The interface polarization will enhance the composite material's loss of electromagnetic wave energy, and its strength is mainly determined by the number of interfaces. Therefore, the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure of the present invention Larger.
[0072]
[0073] In the formula is the conductivity, The free space dielectric constant, is the polarization relaxation loss.
[0074] Again, the magnetic conductivity gradient of the composite material proposed in the present invention is verified. The hysteresis loop of the composite material is tested using a vibrating sample magnetometer of model VSM EZ-7. Fig.10The hysteresis loops of the electromagnetic shielding materials prepared in Examples 1-3, with the decrease of Ni powder content, the magnetic saturation intensity decreases from 0.335 emu / g in Example 1 to 0.168 emu / g in Example 3, indicating that Example 5 has a good reverse magnetic conductivity gradient, and the hysteresis loops of Examples 1, 2 and 3 have no obvious remanence and coercive force, and Ni powder has good paramagnetism, which is beneficial for the composite material to respond quickly to the alternating magnetic field, thereby absorbing electromagnetic waves and converting them into heat energy dissipation.
[0075] The complex magnetic permeabilities of the electromagnetic shielding materials prepared in Examples 1-3 and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5 were tested using a vector network analyzer of model N5234A (USA). Fig.11 , Fig.12 and Fig.13 are the real part of complex magnetic permeability , imaginary part and the magnetic loss tangent The frequency variation curve, where . Reflects the ability of shielding materials to store magnetic energy. It reflects its magnetic loss capacity. The magnetic loss mainly includes hysteresis loss, eddy current loss, magnetization relaxation, natural resonance and other forms. Different magnetic field frequencies and amplitudes correspond to different magnetic loss forms. To measure the magnetic loss capacity of shielding materials. The energy loss caused by the magnetic medium in the alternating magnetic field per unit time and unit volume is defined as the magnetic loss power density. P , and The relationship between satisfies formula (3), from Fig.11 It can be seen that As the Ni powder content increases, The larger the value, the stronger the composite material's loss capacity for electromagnetic waves. In addition, as the frequency increases, the curve fluctuates. This is due to the magnetic dispersion phenomenon generated by the magnetic medium during the magnetization relaxation process under the action of the external dynamic magnetic field. The frequency range in the experiment is 8.0~12.0 GHz (X band), mainly near the ultra-high frequency stage (10 8 ~10 10 Hz), in this frequency range, magnetic dispersion is mainly caused by natural resonance.
[0076]
[0077] In the formula f is the frequency of the applied alternating magnetic field, is the vacuum permeability, is the imaginary part of the complex magnetic permeability, is the amplitude of the applied alternating magnetic field.
[0078] Finally, the electromagnetic shielding performance of the layered gradient structure epoxy resin-based composite material prepared by the method proposed in the present invention was verified. The scattering parameters of the composite material were tested using a vector network analyzer model N5234A (USA), and the electromagnetic shielding effectiveness of the composite material was calculated according to formulas (4) to (9). Figure 14-17 The electromagnetic shielding performance of Ni-MWCNT / Ag / EP composite materials, among which, Fig.14 The overall performance diagram of the electromagnetic shielding materials prepared in Examples 1 to 4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5; Fig.15 The reflection efficiency diagram of the electromagnetic shielding materials prepared in Examples 1 to 4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5; Fig.16 Absorption efficiency diagram of the electromagnetic shielding materials prepared in Examples 1-4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5; Fig.17 The reflection coefficient diagram of the electromagnetic shielding materials prepared in Examples 1-4 of the present invention and the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure prepared in Example 5; for the composite material with a uniform structure, SE T , SE R , SE A , R increase with the increase of the conductivity of the composite material. When the frequency is 8 GHz, SE of Example 1 T is only 8.64 dB, R is 0.48, while the SE of Example 4 is T It reached 24.92 dB, and R reached 0.87. Although simply increasing the amount of Ni powder added does not significantly improve the conductivity, resulting in poor electromagnetic shielding performance, the increase in Ni powder content is beneficial to improving the composite material's magnetic loss capacity against electromagnetic waves. Fig.18The electromagnetic shielding mechanism of the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure obtained in Example 5. Example 5 prepared by printing with inks with different filler contents has a layered gradient structure. The conductivity of different filler layers is different. There will be a certain impedance mismatch between the layers, which will cause interlayer electromagnetic wave reflection. In order to make the surface layer impedance match as good as possible, avoid excessive surface layer reflection, and allow more electromagnetic waves to enter the interior of the composite material, the surface layer of the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure of the present invention selects Example 1 with lower conductivity and higher magnetic permeability. The conductivity of the following three layers gradually increases, and the magnetic permeability gradually decreases. The bottom layer selects Example 4 with the highest conductivity, which can weaken the penetration of electromagnetic waves into the composite material, reflect the electromagnetic waves and enter the absorption layer again, and convert the electromagnetic waves into internal energy in the form of dielectric loss and magnetic loss. After the electromagnetic waves enter the composite material, they are reflected and absorbed multiple times between the layers to form an "absorption-reflection-reabsorption" shielding effect, so that SE A It has been improved to 14.43 dB, SE T The SE of Example 3 with a higher conductivity is 17.74 dB, which is higher than that of Example 3 with a higher conductivity. A and SE T ; The present invention has a layered gradient structure of epoxy resin-based electromagnetic shielding composite material SE R , R are 3.31 dB and 0.53 respectively, both lower than SE of Example 2 with smaller conductivity R and R, indicating that this layered gradient structure is beneficial to improving the absorption loss of electromagnetic waves by the composite material, by increasing SE A To improve SE T At the same time, it weakens the reflection of electromagnetic waves by composite materials, which is beneficial to reduce the secondary pollution caused by electromagnetic waves re-entering the air. By controlling the distribution of metal fillers and carbon fillers through direct writing printing technology to control the conductivity and magnetic conductivity gradient, it can avoid the high reflectivity caused by high conductivity to a certain extent, and also avoid the high transmittance and poor electromagnetic shielding performance caused by low conductivity.
[0079]
[0080] Among them, SE T is the total electromagnetic shielding effectiveness, SE A is the electromagnetic shielding absorption efficiency, SE R is the electromagnetic shielding reflection efficiency, A is the absorption loss coefficient, R is the reflection loss coefficient, SE M It is the internal multiple reflection efficiency. When the electromagnetic wave propagates inside the shielding material, the required thickness when the energy loss reaches 1 / e of the initial energy is less than the thickness of the shielding material. SE M Can be omitted, because most of the multi-reflected electromagnetic waves will be absorbed and lost by the shielding material at this time, so SEM Included in SE A Inside.
[0081] The S parameters (scattering parameters) are obtained as follows Fig.19 As shown, the shielding material is equivalent to a two-port network, and the scattering parameters are directly measured using a vector network analyzer (VNA).
[0082] In summary, the layered gradient structure electromagnetic shielding composite material prepared by the method proposed in the present invention can improve the absorption loss capacity of electromagnetic waves to a certain extent, and weaken the secondary pollution caused by the strong reflection of electromagnetic waves on the surface of the material due to impedance mismatch. This method has certain application prospects in the preparation of new electromagnetic shielding materials.
[0083] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. An epoxy resin-based electromagnetic shielding composite material with a layered gradient structure, It is characterized in that The invention comprises a first shielding layer, a second shielding layer, a third shielding layer and a fourth shielding layer which are arranged in sequence from top to bottom. The first shielding layer, the second shielding layer, the third shielding layer and the fourth shielding layer are all made by 3D printing. The raw materials of the 3D printing ink used in each shielding layer consist of the following components: epoxy resin, methyl hexahydrophthalic anhydride, N, N-dimethylbenzylamine, polyether polyol, acetylene carbon black and functional filler; wherein the functional filler of the fourth shielding layer is flaky silver powder, and the mass percentage of the flaky silver powder in the raw material is 19-21%; the functional filler of the third shielding layer is multi-walled carbon nanotubes and nickel powder, and the mass percentage of the multi-walled carbon nanotubes and the nickel powder in the raw material is 0.5-1.5% and 5-7% respectively; the functional filler of the second shielding layer is multi-walled carbon nanotubes and nickel powder, and the mass percentage of the multi-walled carbon nanotubes and the nickel powder in the raw material is 0.4-0.6% and 9-11% respectively; the functional filler of the first shielding layer is nickel powder, and the mass percentage of the nickel powder in the raw material is 13-15%.
2. The epoxy resin-based electromagnetic shielding composite material with a layered gradient structure as claimed in claim 1, It is characterized in that In each shielding layer, the mass ratio of the epoxy resin to the polyether polyol is 100:(2-3), the mass ratio of the methyl hexahydrophthalic anhydride to the epoxy resin is (80-90):185, the mass ratio of the N,N-dimethylbenzylamine to the epoxy resin is (0.5-1.5):100, and the mass ratio of the acetylene black to the epoxy resin is (11-13):
100.
3. A method for preparing the epoxy resin-based electromagnetic shielding composite material with a layered gradient structure as claimed in claim 1 or 2, It is characterized in that The preparation method specifically comprises the following steps: S1, preparing printing ink for the first shielding layer; S2, preparing printing ink for the second shielding layer; S3, preparing printing ink for the third shielding layer; S4, preparing printing ink for the fourth shielding layer; S5. Use 3D software to draw a 3D model, import it into a direct writing 3D printer and set the printer parameters. Place the prepared printing ink in the printing syringes respectively, and then use the direct writing 3D printer to print layer by layer in the order of the fourth shielding layer, the third shielding layer, the second shielding layer and the first shielding layer. After printing, place it in a drying oven to heat and cure.
4. The method for preparing the epoxy resin-based electromagnetic shielding composite material having a layered gradient structure according to claim 3, It is characterized in that In the step S1, the preparation method of the printing ink of the first shielding layer includes the following steps: placing epoxy resin in a container, adding polyether polyol according to the mass ratio, and then placing it in a drying oven to preheat to 75-78°C to fully dissolve it, and then adding methyl hexahydrophthalic anhydride and N, N-dimethylbenzylamine in sequence, and then adding acetylene carbon black, after mechanically stirring for 50-60 minutes, adding nickel powder and stirring for 30-35 minutes, after stirring, filtering with a filter cloth with a pore size of 80-82 μm and vacuuming for 10-12 minutes to obtain the printing ink of the first shielding layer.
5. The method for preparing the epoxy resin-based electromagnetic shielding composite material having a layered gradient structure according to claim 3, It is characterized in that In the step S2, the preparation method of the printing ink of the second shielding layer includes the following steps: placing epoxy resin in a container, adding polyether polyol according to the mass ratio, and then placing it in a drying oven to preheat to 75-78°C to fully dissolve it, adding multi-walled carbon nanotubes and ultrasonic dispersion for 10-12 min, and then adding methyl hexahydrophthalic anhydride and N, N-dimethylbenzylamine in sequence, and then adding acetylene carbon black, after mechanical stirring for 50-60 min, adding nickel powder and stirring for 30-35 min, after stirring, filtering with a filter cloth with a pore size of 80-82 μm and vacuuming for 10-12 min to obtain the printing ink of the second shielding layer.
6. The method for preparing the epoxy resin-based electromagnetic shielding composite material having a layered gradient structure according to claim 3, It is characterized in that In the step S3, the preparation method of the printing ink of the third shielding layer includes the following steps: placing epoxy resin in a container, adding polyether polyol according to the mass ratio, and then placing it in a drying oven to preheat to 75-78°C to fully dissolve it, adding multi-walled carbon nanotubes and ultrasonic dispersion for 10-12 min, and then adding methyl hexahydrophthalic anhydride and N, N-dimethylbenzylamine in sequence, and then adding acetylene carbon black, after mechanical stirring for 50-60 min, adding nickel powder and stirring for 30-35 min, after stirring, filtering with a filter cloth with a pore size of 80-82 μm and vacuuming for 10-12 min to obtain the printing ink of the third shielding layer.
7. The method for preparing the epoxy resin-based electromagnetic shielding composite material having a layered gradient structure according to claim 3, It is characterized in that In the step S4, the preparation method of the printing ink of the fourth shielding layer comprises the following steps: placing epoxy resin in a container, adding polyether polyol according to the mass ratio, and then placing it in a drying oven to preheat to 75-78° C. to fully dissolve it, and then sequentially adding methyl hexahydrophthalic anhydride and N, N-dimethylbenzylamine, and then adding acetylene carbon black, after mechanically stirring for 50-60 min, adding flaky silver powder and stirring for 30-35 min, after stirring, filtering with a filter cloth with a pore size of 80-82 μm and vacuuming for 10-12 min to obtain the printing ink of the fourth shielding layer.
8. The method for preparing the epoxy resin-based electromagnetic shielding composite material having a layered gradient structure according to claim 3, It is characterized in that In step S5, the parameters of printing with a direct writing 3D printer are as follows: the printing needle diameter is 0.41-0.42 mm, the layer height is set to 0.4-0.41 mm, each ink is printed one layer in sequence, the printing speed is 10-11 mm / s, the printing spacing is 0.4-0.5 mm, the printing air pressure is 0.1-0.2 MPa, the broken wire height is 2 mm, and the early wire is 200-202 ms.
9. The method for preparing the epoxy resin-based electromagnetic shielding composite material having a layered gradient structure according to claim 3, It is characterized in that In step S5, the specific steps of heating and curing are: heating at 90-92°C for 30-32 min, heating to 118-120°C for 1-1.2 h, then heating to 140-145°C for 30-32 min, and finally heating to 150-160°C for 2-2.5 h.
Citation Information
Patent Citations
Multi-band-frequency electromagnetic wave shield composite film layer and preparation and application thereof
CN111304653A
Novel electromagnetic shielding material and preparation method thereof
CN112261859A