Polypropylene film, laminated metal film using same, and film capacitor
By optimizing the strength and shrinkage of the polypropylene film, adding cyclic olefin resin, and combining biaxial stretching and heat treatment processes, the problems of insulation breakdown voltage and dimensional stability of the polypropylene film in high-temperature environments have been solved, achieving Improve the performance of film capacitors under high temperature and high voltage.
Patent Information
- Application Number
- CN202280092874.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2022-12-19
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult for existing polypropylene films to maintain stable insulation breakdown voltage and dimensional stability in high-temperature environments, resulting in insufficient reliability and processability of film capacitors, especially under high-temperature and high-voltage conditions.
By setting the strength in the main orientation direction as F(A23) and the strength in the orthogonal direction of the main orientation as F(B23) in the polypropylene film, ensure that F(A23)+F(B23) reaches above 120MPa and below 1000MPa, and The shrinkage rate at 150°C is -2.0% or more and 3.0% or less. It also contains cyclic olefin-based resin and adopts biaxial stretching and heat treatment processes to improve mechanical properties and thermal dimensional stability.
It achieves excellent withstand voltage characteristics and reliability in high-temperature environments, is suitable for long-term use of polypropylene films in film capacitors, and improves the performance and processability of film capacitors under high temperatures and high voltages.
Smart Images

Figure CN118786167A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to polypropylene films which are particularly suitable for use in film capacitor applications. Background Art
[0002] In recent years, most of the various electrical equipment have been converted to inverters, and with this, the demand for miniaturization and high capacity of film capacitors has become stronger. In particular, for vehicles such as automobiles (including electric vehicles and hybrid vehicles), solar power generation, and wind power generation, in addition to improving voltage resistance, maintaining productivity and processing adaptability in capacitor element production, the film used for film capacitors is also required to be thinner and heat resistant.
[0003] Polypropylene film is considered to be excellent in heat resistance and dielectric breakdown voltage as a dielectric for film capacitors. On the other hand, when applied to the above fields, it is important for the film to have excellent dimensional stability at the ambient temperature of use and stable electrical properties (voltage resistance, etc.) in a region 10 to 20°C higher than the ambient temperature of use. From the perspective of heat resistance, in the future, when considering the use of power semiconductors using silicon carbide (SiC), it is believed that the ambient temperature of use will become higher.
[0004] Under such background, film capacitors are required to have further improved heat resistance and voltage resistance, and films for film capacitors are required to have improved dielectric breakdown voltage in a high temperature environment exceeding 110° C. However, as described in Non-Patent Document 1, the upper limit of the operating temperature of polypropylene films is considered to be about 110° C., and it is extremely difficult for polypropylene films to stably maintain dielectric breakdown voltage in such a temperature environment.
[0005] In order to miniaturize the film capacitor and improve the heat resistance, it is considered to use a thin film with a high relative dielectric constant, or a film composed of a resin component having a glass transition temperature exceeding the ambient temperature range of the film capacitor, or a film containing such a resin component. For example, the following laminate is proposed, which has a laminate structure in which two layers with different relative dielectric constants are alternately overlapped, one layer uses a cyclic olefin resin layer whose glass transition temperature exceeds 130°C, and the other uses a polypropylene layer, so that it can maintain a large electrostatic capacitance while having heat resistance and voltage resistance (for example, Patent Document 1).
[0006] In addition, films with improved processability by coextrusion and costretching when forming a laminate of a cyclic olefin resin and polypropylene have been proposed (for example, Patent Documents 2 and 3). Furthermore, films with improved thermal dimensional stability in a high temperature environment by blending a cyclic olefin resin and a polypropylene resin and performing film formation and biaxial stretching have been proposed (for example, Patent Document 4).
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2015-012076
[0010] Patent Document 2: WO2017 / 022706 Pamphlet
[0011] Patent Document 3: Japanese Patent Application Publication No. 2018-034510
[0012] Patent Document 4: Japanese Patent Application Publication No. 2020-521867
[0013] Non-patent literature
[0014] Non-patent document 1: Motobu Kawai, "Furuman's Leap Forward, Koruman's Leap" , Nikkei Torokusu, Nikkei BP, September 17, 2012, p.57~62 Summary of the invention
[0015] Problems to be solved by the invention
[0016] However, since the film of Patent Document 1 is not a co-extruded laminate but a laminate in which a cyclic olefin resin layer is formed on a polypropylene film by a coating method, the cyclic olefin resin layer is easy to peel off, and it is difficult to say that the performance and reliability of the film capacitor are sufficient.
[0017] The film of Patent Document 2 also has difficulty in increasing the area stretching ratio because the base layer of the laminated structure is a single cyclic olefin resin, and the voltage resistance in a high temperature environment is insufficient. Therefore, it is difficult to say that the performance and reliability of the film capacitor are sufficient.
[0018] The film of Patent Document 3 also has a laminated structure in which the base layer is a cyclic olefin resin. Although it contains an elastomer to increase the area stretching ratio, its voltage resistance in a high temperature environment is unsatisfactory, and it is difficult to say that its performance and reliability when made into a film capacitor are sufficient.
[0019] Since the film of Patent Document 4 is a film obtained by blending a cyclic olefin resin with a high glass transition temperature with a polypropylene resin, when the film is made thinner by increasing the area stretching ratio, the film may break during the manufacturing process and processing process, and voids may be formed, resulting in insufficient voltage resistance in a high temperature environment. As a result, it is difficult to say that the performance and reliability of the film capacitor are sufficient. Furthermore, if the film is stretched at a high area stretching ratio, the long-term dimensional stability is insufficient, and the risk of shape deformation when used as a film capacitor increases.
[0020] Therefore, an object of the present invention is to provide a polypropylene film having excellent voltage resistance characteristics, dimensional stability, reliability and processability when used in a film capacitor under high temperature environment, and suitable for film capacitor applications that can be used for a long time under high temperature / high voltage.
[0021] Means for solving problems
[0022] The present inventors have repeatedly conducted intensive studies to solve the above-mentioned problems and have invented the following polypropylene film, wherein when the strength in the main orientation direction measured at 23°C is set to F(A23), and the strength in the direction orthogonal to the main orientation measured at 23°C is set to F(B23), F(A23)+F(B23) is greater than 120 MPa and less than 1000 MPa, and the shrinkage in the main orientation direction measured at 150°C is greater than -2.0% and less than 3.0%, and the film contains a cyclic olefin resin.
[0023] Effects of the Invention
[0024] According to the present invention, it is possible to provide a polypropylene film which has excellent withstand voltage characteristics and reliability in a high temperature environment and is suitable for film capacitor applications that can be used for a long period of time under high temperature and high voltage. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a schematic diagram showing a rectangle of 1 μm×2 μm defined so that a pair of short sides are parallel to the thickness direction in the cross section X of the polypropylene film of the present invention, and a domain of the cyclic olefin-based resin passing through the pair of short sides of the rectangle.
[0026] Figure 2 This is an enlarged photograph (magnification 2,000 times) of a cross section X of a polypropylene film according to one embodiment (the embodiment of Example 5) of the present invention. DETAILED DESCRIPTION
[0027] The present inventors have repeatedly conducted intensive studies to solve the above problems and have come to the following conclusions as to why the films described in Patent Documents 1 to 4 are insufficient in terms of dielectric breakdown voltage under high temperature environments, voltage withstand characteristics under high temperature environments when the films are made into film capacitors, reliability, and processability.
[0028] It can be considered that the film of patent document 1 has the following problems: since it is an unstretched film laminated by a coating method, interlayer peeling occurs under high temperature environment, mechanical properties, especially elongation at break, are insufficient and easy to break during capacitor element processing, and the withstand voltage under high temperature environment is reduced. It can be considered that the films of patent documents 2 and 3 have the following problems: regarding the expected withstand voltage under high temperature environment, the ratio of longitudinal stretching in the film making is not necessarily sufficient, and there are a large number of movable amorphous components in the film, so the insulation breakdown voltage under high temperature becomes low. Regarding the film of patent document 4, regarding the assumed withstand voltage under high temperature environment, the mixing state of cyclic olefin resin and polypropylene resin is also insufficient, so it can be considered that if the ratio of area stretching in film making is to be fully increased, gaps will be formed at the interface, and the insulation breakdown voltage under high temperature becomes a problem. In addition, it can be considered that there are also the following problems: due to the formation of coarsened domains, the sliding property and tensile strength are reduced, especially when the film is thinned, it is easy to break in the processing steps such as evaporation, cutting, element winding, and pressing.
[0029] According to the above considerations, the present inventors have further repeatedly studied and found that the above-mentioned problems can be solved by the following polypropylene film, wherein when the strength in the main orientation direction measured at 23°C is set to F(A23), and the strength in the direction orthogonal to the main orientation measured at 23°C is set to F(B23), F(A23)+F(B23) is 120 MPa or more and 1000 MPa or less, and the shrinkage rate in the main orientation direction measured at 150°C is -2.0% or more and 3.0% or less, and the polypropylene film contains a cyclic olefin resin.
[0030] Hereinafter, the polypropylene film of the present invention will be specifically described. In addition, when the upper limit and the lower limit are described below about the preferred range, the combination thereof may be arbitrary.
[0031] In addition, in this specification, the polypropylene film is sometimes referred to as a film. In addition, the polypropylene film of the present invention is not a microporous film, so it does not have many pores. That is, the so-called polypropylene film of the present invention refers to a polypropylene film other than a microporous film. The so-called microporous film here is defined as a film having a pore structure that penetrates both surfaces of the film and has the following air permeability, wherein the air permeability is a permeability of less than 5,000 seconds / 100 ml at 23°C and a relative humidity of 65% using a B-type Gurley tester of JIS P 8117 (1998) with a permeation time of 100 ml of air.
[0032] From the viewpoint of withstand voltage under high temperature environment, when the strength in the main orientation direction measured at 23°C is F(A23) and the strength in the direction orthogonal to the main orientation measured at 23°C is F(B23), F(A23)+F(B23) is 120 MPa or more and 1000 MPa or less. From the above viewpoints, F(A23)+F(B23) is preferably 250 MPa or more, more preferably 350 MPa or more, and further preferably 420 MPa or more. The polypropylene film of the present invention can reduce the movable amorphous component by making F(A23)+F(B23) 120 MPa or more, so that high withstand voltage is exhibited even at high temperature. Regarding F(A23)+F(B23), from the viewpoint of withstand voltage, the higher the better, but from the viewpoint of feasibility, it is 1000 MPa or less.
[0033] The strength of the polypropylene film of the present invention at 23°C can be measured by the following steps. First, a tensile test is performed on a rectangular polypropylene film of 10 mm × 150 mm (measurement direction) under the conditions of an initial chuck distance of 20 mm, a temperature of 23°C, and a tensile speed of 300 mm / min. Then, the load at the time of the polypropylene film breaking is divided by the cross-sectional area of the sample before the test (film thickness × width (10 mm)) to calculate the strength. In addition, the tensile test can be performed by a known tensile testing machine, and for example, "Tensilon" (registered trademark) UCT-100 manufactured by Orientec can be used appropriately.
[0034] The method for improving F(A23)+F(B23) is not particularly limited, and for example, a method in which biaxial stretching is performed when manufacturing a polypropylene film to increase the stretching ratio in the length direction and the width direction can be cited. Stretching can be performed by simultaneous biaxial stretching or by successive biaxial stretching, but it is preferably performed by successive biaxial stretching from the viewpoint of productivity. The so-called length direction here refers to the direction in which the polypropylene film moves in the manufacturing process (in the film roll, the winding direction is equivalent to this direction), and the so-called width direction refers to the direction orthogonal to the length direction in the film surface. In addition, F(A23)+F(B23) can also be improved by using a polypropylene resin with high stereoregularity as a raw material. For example, it is easy to improve F(A23)+F(B23) by using a polypropylene with a high rate of meso-pentad components.
[0035] Here, the so-called polypropylene film refers to a sheet-shaped molded body with polypropylene resin as the main component, and the so-called main component refers to a component contained in more than 50% by mass and less than 100% by mass when all the components constituting the film are set to 100% by mass. In addition, when a plurality of components equivalent to polypropylene resin are included in the film, even if each component is less than 50% by mass, as long as the total of these components exceeds 50% by mass, it is regarded as a film with polypropylene resin as the main component.
[0036] The polypropylene resin refers to a resin containing more than 50 mol % and 100 mol % or less of propylene units when all structural units constituting the resin are 100 mol %, and does not correspond to a cyclic olefin resin (described later).
[0037] The main orientation direction in the polypropylene film of the present invention is described below. The so-called main orientation direction refers to the direction in which the polypropylene molecular chain is oriented the most. When biaxial stretching is performed in the manufacture of the polypropylene film, it is usually stretched in the length direction and the width direction, and generally speaking, the direction with the larger stretching ratio becomes the main orientation axis direction. When the stretching direction (length direction and width direction) can be specified but the ratio is unclear, the maximum load until breaking can be measured in the tensile test at 23°C described later, and the direction with the larger measured value is set as the main orientation axis direction.
[0038] As mentioned above, if the stretching direction and the stretching ratio are known, the main orientation axis direction can be easily specified, but in the case of films where they are unclear, the main orientation axis direction can be specified by the following method. Specifically, prepare a film, with an arbitrary direction facing up, cut into a rectangle of 50 mm in length and 10 mm in width as sample <1>, and define the direction of the long side of sample <1> as 0°. Next, take a sample <2> of the same size in such a way that the long side direction becomes a direction rotated 15° to the right from the 0° direction. Similarly, the long side direction of the rectangular sample is rotated 15° each, and samples <3> to <12> are taken in the same way. Next, each rectangular sample is placed in a tensile testing machine with an initial distance of 20 mm between the chucks in such a way that the long side direction becomes the stretching direction, and a tensile test is performed at room temperature with the stretching speed set to 300 mm / minute. At this time, read the maximum load until the sample breaks, and calculate the value divided by the cross-sectional area (film thickness × width) of the sample before the test as the stress of the maximum point strength. The longitudinal direction of the sample having the largest value was defined as the main orientation axis of the polypropylene film, and the direction perpendicular thereto was defined as the direction perpendicular to the main orientation axis of the polypropylene film.
[0039] In the case where the width of the sample is less than 50 mm and the above-mentioned tensile test cannot be performed, the crystal orientation of the α crystal (110) plane using wide-angle X-rays is measured as follows, and the film length and width directions are set based on the following judgment criteria. That is, X-rays (CuKα rays) may be incident on the film surface in a vertical direction, and the crystal peak at 2θ=about 14° (α crystal (110) plane) may be scanned in the circumferential direction, and the direction with the highest diffraction intensity of the obtained diffraction intensity distribution may be set as the film width direction and the main orientation direction, and the direction orthogonal thereto may be set as the length direction and the direction orthogonal to the main orientation direction.
[0040] From the viewpoint of improving the reliability when used for film capacitors, the shrinkage of the polypropylene film of the present invention in the main orientation direction measured at 150°C is -2.0% or more and 3.0% or less. From the above viewpoint, the above shrinkage is preferably 1.5% or less, more preferably 1.0% or less, further preferably 0.5% or less, and particularly preferably 0.0% or less. When the above shrinkage is below 0.0%, the smaller the absolute value, the better. From the viewpoint of feasibility, the above shrinkage is preferably -1.5% or more, more preferably -1.0% or more. In addition, a negative shrinkage means that the polypropylene film expands by heating.
[0041] When the shrinkage rate of the polypropylene film exceeds 3.0%, the polypropylene film tends to shrink in a high temperature environment (eg, 135° C.), and thus when used in a film capacitor, the reliability thereof may be reduced.
[0042] In the polypropylene film of the present invention, the shrinkage at 150°C can be measured by the following method. First, a sample with a width of 10 mm and a length of 200 mm (measurement direction) is cut out, and marks are made at positions 25 mm from both ends to obtain a test length of 150 mm (l 0 ) test piece. Next, the test piece was sandwiched between paper and heated in an oven kept at 150°C for 15 minutes without applying any load. The test piece was then removed from the oven, cooled at room temperature, and the dimensions (l 1 ), and the shrinkage rate was calculated using the following formula.
[0043] Shrinkage rate = {(l 0 -l 1 ) / l 0}×100(%).
[0044] As a method for making the above-mentioned shrinkage ratio be greater than -2.0% and less than 3.0%, for example, it is effective to use a polypropylene resin with high stereoregularity and melting point (for example, a polypropylene resin having a high meso pentad fraction and a high melting point, etc.), to set the preheating temperature immediately before stretching in the width direction after uniaxial stretching in the longitudinal direction to 175°C or more, and to carry out a relaxation treatment at a relaxation rate of more than 5% in the heat treatment step after biaxial stretching.
[0045] The polypropylene film of the present invention contains a cyclic olefin resin. The so-called cyclic olefin resin refers to a resin containing 10 mol% or more and 100 mol% or less of cyclic olefin units when all structural units constituting the resin are set to 100 mol%. In addition, a resin containing multiple structural units equivalent to cyclic olefin units is equivalent to a cyclic olefin resin even if the individual cyclic olefin units are less than 10 mol%, as long as the total of these structural units exceeds 10 mol%.
[0046] By including the cyclic olefin resin, the polypropylene film has high adhesion to the polypropylene resin due to the high heat resistance of the cyclic olefin resin, thereby improving the withstand voltage in a high temperature environment. Therefore, the film capacitor using the polypropylene film of the present invention can maintain the withstand voltage even when used for a long time at high temperature, and exhibits excellent reliability.
[0047] For the polypropylene film of the present invention, from the viewpoint of making the dispersion state of the cyclic olefin resin and the polypropylene resin good, it is preferred to mix the cyclic olefin resin with the polypropylene resin (further with an antioxidant as needed) in advance and perform pre-mixing (hereinafter sometimes referred to as compounding). A single-screw extruder, a twin-screw extruder, etc. can be used for compounding, but from the viewpoint of a good dispersion state and high transparency, a twin-screw extruder is particularly preferred. By homogenizing the dispersion state of the cyclic olefin resin and the polypropylene resin, the reduction in local withstand voltage caused by the local high concentration of the cyclic olefin resin can be suppressed. Therefore, when the polypropylene film is used for film capacitor purposes, the reliability of the film capacitor can be made high, and the shape change of the capacitor element when used for a long time at 135°C can be reduced.
[0048] In the polypropylene film of the present invention, when the total components constituting the film are set to 100% by mass, the lower limit of the content of the cyclic olefin resin is preferably 1% by mass, more preferably 4% by mass, and further preferably 7% by mass. On the other hand, when the total components constituting the film are set to 100% by mass, the upper limit is preferably 39% by mass, more preferably 32% by mass, more preferably 25% by mass, more preferably 19% by mass, further preferably 14% by mass, particularly preferably 9.5% by mass, and most preferably 9.0% by mass. If the proportion of cyclic olefin resin in the polypropylene film is too much, then sometimes the area stretch ratio is not improved when stretched, and the voltage resistance under high temperature environment is reduced. In addition, cyclic olefin resin is generally more expensive than polypropylene, and it is also preferred to make the content less from the viewpoint of economy. On the other hand, if the proportion of cyclic olefin resin in the polypropylene film is insufficient, then sometimes the structural stabilization effect brought by cyclic olefin resin becomes insufficient, and the voltage resistance under high temperature environment and the reliability when the film capacitor is made are reduced.
[0049] From the viewpoint of processability, the polypropylene film of the present invention preferably has a developed area ratio Sdr of at least one surface of 0.002% to 0.050%. Sdr is a parameter that increases as the protrusions on the surface become denser, and the higher the Sdr, the higher the slip properties of the polypropylene film surface.
[0050] That is, by making the Sdr of at least one surface 0.002% or more, the slip property of the polypropylene film surface is improved, so the processability of the polypropylene film in the process of processing it as a dielectric for a film capacitor, such as vapor deposition, slitting, element winding, pressing, etc., becomes good. From the above viewpoint, the Sdr of at least one surface is more preferably 0.005% or more, and further preferably 0.010% or more.
[0051] On the other hand, by setting the Sdr of at least one surface to 0.050% or less, the slip property of the polypropylene film surface is appropriately low, and winding displacement when a wound body is formed can be easily suppressed. From the above viewpoint, the Sdr of at least one surface is more preferably 0.035% or less.
[0052] In addition, from the viewpoint of both processability and quality when made into a wound body, it is more preferable that Sdr is 0.002% or more and 0.050% or less, or the above preferred range, on both sides. In addition, Sdr can be measured and calculated according to ISO25178 (2012), which is described in detail below.
[0053] The polypropylene film of the present invention comprises polypropylene resin and cyclic olefin resin, thereby can form a dense surface derived from phase separation. The adjustment of Sdr can be adjusted by adjusting the raw material, stacking ratio, surface thickness, and stretching conditions. More specifically, by using a composite resin raw material in which cyclic olefin resin and polypropylene resin are pre-mixed by a twin-shaft mixer and increasing their ratio, the dispersion diameter of the cyclic olefin resin can be made small, and as a result, Sdr is high. On the other hand, by making the stretching ratio in the length direction and the width direction high, Sdr can be made small.
[0054] Hereinafter, in the polypropylene film of the present invention, a method for determining a rectangle of 1 μm×2 μm in size in a cross section X in which a pair of short sides are parallel to the thickness direction, and a method for determining the number of domains of the cyclic olefin resin passing through a pair of short sides of the rectangle will be described with reference to the accompanying drawings. Figure 1 This is a schematic diagram showing a rectangle of 1 μm×2 μm defined so that a pair of short sides are parallel to the thickness direction in the cross section X of the polypropylene film of the present invention, and a domain of the cyclic olefin-based resin passing through the pair of short sides of the rectangle. Figure 1 Symbols 1 to 5 in the figure respectively represent a part of the cross section X, a sea part, an island part (domain), a rectangle of 1 μm×2 μm in size determined in the cross section X so that a pair of short sides are parallel to the thickness direction, and a pair of short sides parallel to the thickness direction. Figure 1 The left figure is a part of the cross section X, and the right figure is an enlarged view of a rectangle of 1 μm×2 μm in cross section X, which is determined in such a way that a pair of short sides are parallel to the thickness direction ( Figure 1 (Enlarged view of the dotted line portion in the left figure). In the polypropylene film of the present invention, the sea portion is made of polypropylene resin, and the island portion is made of cyclic olefin resin.
[0055] When a rectangle of 1 μm×2 μm is determined in the cross section X so that a pair of short sides are parallel to the thickness direction, the bottom side of the rectangle is set as the sea part, and when a domain is located on the side opposite to the bottom side, it is regarded as not existing and is not counted as the number (in Figure 1 In the example above, no such domain exists. ).
[0056] Here, the "domain of the cyclic olefin resin passing through a pair of short sides parallel to the thickness direction" refers to the domain of the cyclic olefin resin passing through both of the pair of short sides parallel to the thickness direction. Figure 1 In the example (right figure), the 1st, 4th to 6th domains from the top correspond to the above domains, and the 2nd and 3rd domains from the top do not correspond to the above domains. Therefore, the number of "domains of cyclic olefin-based resins passing through a pair of short sides parallel to the thickness direction" in this example is 4.
[0057] The polypropylene film of the present invention preferably has a cross section X in which the A layer is cut along a plane parallel to the main orientation axis direction and the thickness direction, and in the cross section X, Figure 1 As shown in FIG. 1 , in a rectangle of 1 μm×2 μm in size determined in such a manner that a pair of short sides are parallel to the thickness direction, there are two or more domains of the cyclic olefin resin passing through the pair of short sides. In the polypropylene film of the present invention, the number of domains of the cyclic olefin resin passing through the pair of short sides parallel to the thickness direction is preferably 4 or more, more preferably 6 or more. The upper limit is not particularly limited, but is 100, preferably 20.
[0058] By making the number of domains of the cyclic olefin resin passing through a pair of short sides parallel to the thickness direction two or more, the cyclic olefin resin is microdispersed in a flatter shape in the plane, and the high thermal stability of the cyclic olefin resin and the high withstand voltage of the polypropylene resin can be reflected in the polypropylene film, and the insulation breakdown voltage of the polypropylene film in a high temperature environment can be increased. Furthermore, if such a film is used for a film capacitor, it is difficult to cause short circuit breakdown even if it is used for a long time in a high temperature environment, and the withstand voltage of the film capacitor is maintained, and high reliability can be obtained.
[0059] The method for bringing the number of the above domains into an appropriate range is not particularly limited, but it is effective to set the filter temperature lower than the extrusion temperature in an extruder for extruding a resin containing a cyclic olefin resin and to perform biaxial stretching in a manner such that the area stretching ratio is 45 times or more.
[0060] From the viewpoint of moldability, the polypropylene film of the present invention more preferably contains a linear polypropylene resin (hereinafter, sometimes referred to as a polypropylene resin (A)) as a main component.
[0061] The lower limit of the number average molecular weight (Mn) of the polypropylene resin (A) is preferably 30,000, more preferably 40,000, and further preferably 50,000. On the other hand, the upper limit of Mn is preferably 90,000, more preferably 80,000. By making the molecular weight of the polypropylene resin (A) within the above range, the deterioration of film stability, film strength, dimensional stability, and heat resistance can be alleviated. In addition, the number average molecular weight (Mn) can be measured by gel permeation chromatography (GPC).
[0062] From the viewpoint of heat resistance when a polypropylene film is made, the meso pentad component rate of the polypropylene resin (A) is preferably 0.960 or more. From the above viewpoint, it is more preferably 0.965 or more, further preferably 0.970 or more, particularly preferably 0.975 or more, and most preferably 0.980 or more. The meso pentad component rate is an index representing the stereoregularity of the crystalline phase of polypropylene measured by nuclear magnetic resonance (NMR method). The higher the numerical value of the polypropylene resin, the higher the crystallinity and melting point, and the more suitable it is for use at high temperatures, so it is preferred. There is no particular provision for the upper limit of the meso pentad component rate, but it is considered to be 1.000 from the viewpoint of feasibility.
[0063] In order to obtain such a resin with high stereoregularity, for example, it is preferable to adopt a method of washing the obtained resin powder with a solvent such as n-heptane, a method of appropriately selecting a catalyst and / or a co-catalyst, and a method of selecting a composition.
[0064] The melting point of the polypropylene resin (A) is preferably 160° C. or higher, more preferably 161° C. or higher, further preferably 162° C. or higher, particularly preferably 164° C. or higher, and most preferably 167° C. or higher. When the melting point of the polypropylene resin (A) is 160° C. or higher, the decrease in voltage resistance in a high temperature environment when the film is produced is reduced.
[0065] The melting point of the resin is defined as the melting peak temperature obtained when the resin is heated from 30°C to 260°C at 20°C / min using a differential scanning calorimeter DSC, then cooled to 30°C at 20°C / min, and then heated again from 30°C to 260°C. In some cases, two or more melting peak temperatures are observed in the above temperature range, or a multi-step peak called a shoulder is observed. In such cases, the temperature of the peak with the largest absolute value of the heat flow (unit: mW) on the vertical axis of the DSC chart is defined as the melting point of the resin.
[0066] The polypropylene resin (A) is preferably mainly composed of a homopolymer of propylene, in other words, preferably homopolypropylene, but a copolymer of propylene containing other unsaturated hydrocarbons as copolymer components can be used within the scope of not impairing the purpose of the present invention, and homopolypropylene can also be mixed with the above copolymer for use. As the copolymer components contained in the copolymer of propylene, for example, ethylene, 1-butene, 1-pentene, 3-methylpentene-1, 3-methylbutene-1, 1-hexene, 4-methylpentene-1, 5-ethylhexene-1, 1-octene, 1-decene, 1-dodecene, vinylcyclohexene, styrene, allylbenzene, cyclopentene, norbornene, 5-methyl-2-norbornene, etc. In addition, the so-called homopolypropylene here refers to a resin containing propylene units of 99.5mol% or more and 100mol% or less when all the structural units constituting the resin are set to 100mol%.
[0067] When the polypropylene resin (A) contains copolymer components other than propylene, the copolymerization amount is preferably less than 1 mol% from the viewpoint of dielectric breakdown voltage and heat resistance. Here, the copolymerization amount of components other than propylene is less than 1 mol%, which means that when all the structural units of the resin constituting the polypropylene resin (A) are 100 mol%, the structural units other than propylene units are less than 1 mol%. That is, when the polypropylene resin (A) is composed of a polypropylene polymer having a copolymerization amount of less than 1 mol%, or when a polypropylene polymer having a copolymerization amount of 1 mol% or more and a homopolypropylene (or a polypropylene polymer having a copolymerization amount of less than 1 mol%) are mixed so that the structural units other than propylene occupy less than 1 mol% in the whole, the copolymerization amount of the components other than propylene is also set to be less than 1 mol%.
[0068] The polypropylene film of the present invention preferably has an insulation breakdown voltage of more than 325V / μm and less than 900V / μm measured at 135°C. The lower limit of the above insulation breakdown voltage is more preferably 345V / μm, further preferably 390V / μm, and particularly preferably 420V / μm. The higher the above insulation breakdown voltage, the more preferred it is, but from the perspective of feasibility, it is less than 900V / μm, preferably less than 550V / μm. When the film insulation breakdown voltage at 135°C is more than 325V / μm, when a film capacitor is made, especially in a high temperature environment, it is difficult to cause short-circuit breakdown even if used for a long time, and the voltage resistance is maintained, and high reliability can be obtained.
[0069] In order to control the film insulation breakdown voltage at 135°C to a range exceeding 325V / μm, it is effective to use homopolypropylene with a high meso pentad fraction as the polypropylene resin, dilute or directly melt-extrude a composite resin raw material obtained by pre-mixing a cyclic olefin resin and a polypropylene resin using a twin-screw extruder to form sheets, and perform successive biaxial stretching so that the stretching ratio in the longitudinal direction is 4.0 times or more, the stretching ratio in the width direction is 8.5 times or more, and the area stretching ratio (stretching ratio in the longitudinal direction × stretching ratio in the width direction) is 42 times or more.
[0070] From the viewpoint of being particularly suitable for heat-resistant film capacitors of thin films required for automotive applications (including hybrid vehicle applications) used in high temperature environments, the polypropylene film of the present invention preferably has a thickness of 0.50 μm or more and 5.5 μm or less. For the above-mentioned heat-resistant film capacitor application, the upper limit is preferably 4.0 μm or less, and more preferably 3.2 μm or less, from the balance between the characteristics and the size of the film capacitor caused by the thin film. In addition, the film thickness can be measured with a known micrometer, which is described in detail below.
[0071] There is no particular limitation on the method for adjusting the film thickness. For example, the film thickness can be reduced by reducing the slit width of the die, reducing the amount of molten resin composition discharged from the die, increasing the casting pulling speed, and increasing the stretching ratio. These methods can be appropriately combined.
[0072] The polypropylene film of the present invention preferably has a thickness unevenness in the longitudinal direction of 0.001% or more and 15% or less. Compared with a film not containing the cyclic olefin resin, a film containing the cyclic olefin resin needs to be stretched at a higher temperature during the manufacturing process. As a result, in the film containing the cyclic olefin resin, a position that is locally thinned compared to the center thickness is easily generated. If a film having a position that is locally thinned is used as a dielectric of a film capacitor, the position sometimes becomes the starting point of insulation breakdown and the withstand voltage is reduced.
[0073] By making the thickness unevenness of the polypropylene film less than 15%, the decrease in withstand voltage caused by the above mechanism can be reduced, and the withstand voltage when the film capacitor is made can be improved. From the above viewpoint, the thickness unevenness of the polypropylene film is more preferably less than 12%, further preferably less than 10%, and particularly preferably less than 6%. From the above viewpoint, the smaller the thickness unevenness of the polypropylene film, the better, but from the viewpoint of feasibility, it is preferably more than 0.001%. There is no particular limitation on the method for making the thickness unevenness of the polypropylene film within the above range. For example, a method of making the longitudinal stretching ratio of the film high within the suitable range described later and a method of making the content of cyclic olefin resin low within the suitable range described later are effective. In addition, these methods can be appropriately combined, but for films containing cyclic olefin resins, it is particularly effective to set the longitudinal stretching ratio high.
[0074] From the viewpoint of suitability for film capacitor applications, the polypropylene film of the present invention preferably has a shrinkage in a direction perpendicular to the main orientation of the film measured at 150° C. of not less than -2.0% and not more than 4.0%. From the above viewpoint, the shrinkage is more preferably not more than 2.5%, further preferably not more than 2.0%, particularly preferably not more than 1.0%, and most preferably not more than 0.0%.
[0075] By setting the shrinkage in the direction perpendicular to the main orientation of the film measured at 150° C. to 4.0% or less, the risk of failure can be reduced when a capacitor using the polypropylene film of the present invention as a film capacitor film is used for a long time at 135° C. When the above shrinkage is 0.0% or less, the smaller the absolute value, the better. From the perspective of feasibility, it is -2.0% or more, preferably -1.5% or more, and more preferably -1.0% or more.
[0076] As a method for making the above-mentioned shrinkage rate greater than -2.0% and less than 4.0%, for example, it is effective to use homopolypropylene with a high meso pentad fraction as the polypropylene resin, to increase the stretching ratio in the longitudinal direction (for example, greater than 4.5 times) during biaxial stretching, to increase the heat treatment temperature after transverse stretching, etc.
[0077] The layer structure of the polypropylene film of the present invention can be a single-layer structure or a laminated structure. However, from the perspective of the stretchability of the performance film, the excellent reliability in a high temperature environment, and the processability, it is preferred to have the following A layer and B layer, wherein the layer containing a cyclic olefin resin as the main component of the polypropylene resin is set as the A layer, and the layer containing a polypropylene resin as the main component and a lesser content of the cyclic olefin resin than the A layer is set as the B layer, and has. In particular, by adopting such a laminated structure, it becomes easy to improve the film-making properties while making the area stretching ratio 45 times or more. Here, the so-called "layer containing a lesser content of the cyclic olefin resin than the A layer" refers to a layer with a lower content of the cyclic olefin resin than the amount (mass %) of the cyclic olefin resin in the A layer when all the components constituting the A layer are set to 100% by mass.
[0078] As specific examples of such a scheme, there can be cited a structure in which a B layer is provided on one side of the A layer (a two-layer structure of an A layer / B layer), a structure in which a B layer is provided on both sides of the A layer (a three-layer structure of a B layer / A layer / B layer), a structure in which a B layer is provided on one side of the A layer and a C layer having a resin composition different from that of both the A layer and the B layer is provided on the side without the B layer (a three-layer structure of a C layer / A layer / B layer), a structure in which the B layer is the outermost layer of both surfaces of the film, and the like. From the above viewpoints, a three-layer structure in which the B layer is provided on one side of the A layer, a structure in which the B layer is the outermost layer of both surfaces of the film, and a three-layer structure in which the B layer is provided on one side of the A layer, and a structure in which the B layer is the outermost layer of both surfaces of the film, and a three-layer structure in which the B layer is provided on one side of the A layer, are more preferably used. In addition, in the case of having a plurality of B layers, the composition of the B layer may be the same or different as long as it contains a large amount of polypropylene resin compared to the A layer and has a small content of cyclic olefin resin (hereinafter, with respect to the polypropylene film of the laminated structure, "A layer" and "B layer" are used based on this definition).
[0079] From the viewpoint of voltage resistance at high temperatures, the polypropylene film of the present invention preferably has a cooling crystallization temperature (Tmc) measured by differential scanning calorimetry of 110°C or more. From the above viewpoints, the Tmc of the polypropylene film is more preferably 112°C or more, and further preferably 114°C or more. By making the Tmc of the polypropylene film 110°C or more, especially when the polypropylene film of the present invention is manufactured by biaxial stretching, the film before stretching becomes a structure having a fine crystal structure. Therefore, a polypropylene film with dense protrusions formed can be obtained by biaxial stretching. As a result, the polypropylene film has excellent voltage resistance at high temperatures and excellent productivity. The upper limit of the Tmc of the polypropylene film is preferably 150°C from the viewpoint of feasibility.
[0080] There is no particular limitation on the method for making the Tmc of the polypropylene film above 110°C, and examples include a method in which the polypropylene film of the present invention contains a crystallization nucleating agent that promotes the crystallization of polypropylene. As the crystallization nucleating agent that can be used in the polypropylene film of the present invention, sorbitol-based nucleating agents, nonol-based nucleating agents, amide-based nucleating agents, aromatic carboxylic acid metal salts, phosphate metal salts, polypropylene resins with a cross-linked structure, and branched polypropylene resins can be cited, but from the perspective of suppressing film breakage during production caused by foreign matter, branched polypropylene resins are preferably used. In addition, the so-called branched polypropylene here refers to a polypropylene having one or more side chains with a carbon number of 6 or more in the molecular chain.
[0081] Branched polypropylene has a nucleating agent function that accelerates crystallization when the polypropylene resin is melt-solidified. By including branched polypropylene in the film, uniform crystallization is promoted, film breakage and void formation during stretching are suppressed, and film formation accompanied by stretching at a high ratio becomes easy, and in particular, film forming properties can be improved when stretching at a high area stretching ratio of 45 times or more.
[0082] From the viewpoint of including Tmc in the above range, when the mass of the film is set to 100 mass %, the content of branched polypropylene is preferably 0.01 mass % or more, more preferably 0.1 mass % or more, further preferably 1.0 mass % or more, and particularly preferably 5.0 mass % or more. On the other hand, when the mass of the entire film is set to 100 mass %, the content of branched polypropylene is preferably 50 mass % or less, more preferably 30 mass % or less, and further preferably 10 mass % or less. By suppressing the content of branched polypropylene to less than 50 mass %, it is possible to reduce the film breakage during extrusion accompanied by the rise of melt tension.
[0083] As the lamination method that can be used in the manufacture of the polypropylene film of the present invention, for example, a feed block method using coextrusion, a multi-manifold method, a coating method, etc. can be cited, but from the viewpoint of production efficiency and production cost, a lamination method using coextrusion (such as melt coextrusion) is preferred.
[0084] In the case where the polypropylene film is a laminated structure, from the perspective of controlling film-forming properties and surface shape, the upper limit of the ratio of the thickness of the A layer to the total thickness of the polypropylene film is preferably 99%, more preferably 95%, further preferably 90%, and most preferably 85%. In addition, the lower limit is preferably 10%, more preferably 15%, and further preferably 20%. For example, in the case where the polypropylene film is a three-layer structure of B layer / A layer / B layer in which the B layer is directly laminated on the two surface layers of the A layer, the ratio of the thickness of the A layer can be obtained by dividing the thickness of the A layer excluding the thickness of the B layer on both surfaces by the thickness of the polypropylene film and expressing it as a percentage. By making the ratio of the A layer less than 99%, the area stretching ratio in stretching can be fully increased, and the reduction in voltage resistance under high temperature environment can be reduced. On the other hand, by making the ratio of the A layer more than 10%, the reduction in thermal dimensional stability under high temperature environment is reduced.
[0085] From the viewpoint of obtaining high withstand voltage and excellent stretchability, when all constituent components of layer B are set to 100% by mass, the content of the polypropylene resin in layer B in the polypropylene film of the present invention is preferably 95% by mass or more, more preferably 96% by mass or more, and further preferably 97% by mass or more. The upper limit is not particularly limited, but is set to 100% by mass.
[0086] When the B layer in the polypropylene film of the present invention contains a cyclic olefin resin, from the viewpoint of obtaining high voltage resistance and excellent stretchability, when all the constituent components of the B layer are set to 100% by mass, the content is preferably 5% by mass or less, more preferably 4% by mass or less, further preferably 3% by mass or less, and particularly preferably 1% by mass or less. In addition, it is optional that the B layer contains a cyclic olefin resin, and the lower limit is set to 0.0% by mass (that is, a solution that does not contain a cyclic olefin resin).
[0087] From the viewpoint of improving thermal dimensional stability at high temperatures and reliability when used as a capacitor, the content of the cyclic olefin resin in the A layer in the polypropylene film of the present invention is preferably 0.5% by mass or more, more preferably 1% by mass or more, further preferably 4% by mass or more, and particularly preferably 7% by mass or more, when all the constituent components of the A layer are set to 100% by mass. On the other hand, from the viewpoint of preventing film breakage when the area stretching ratio is increased during stretching, the content of the cyclic olefin resin in the A layer is preferably 38% by mass or less, more preferably 34% by mass or less, further preferably 25% by mass or less, particularly preferably 19% by mass or less, particularly preferably 9.5% by mass or less, and most preferably 9.0% by mass or less, when all the constituent components of the A layer are set to 100% by mass.
[0088] Next, resins that can be suitably used for the polypropylene film of the present invention will be described.
[0089] The cyclic olefin resin used in the polypropylene film of the present invention is described below. Examples of the cyclic olefin monomer that can be used to produce the cyclic olefin resin used in the polypropylene film of the present invention include monocyclic olefins such as cyclobutene, cyclopentene, cycloheptene, cyclooctene, cyclopentadiene, and 1,3-cyclohexadiene, bicyclo〔2,2,1〕hept-2-ene, 5-methyl-bicyclo〔2,2,1〕hept-2-ene, 5,5-dimethyl-bicyclo〔2,2,1〕hept-2-ene, 5-ethyl-bicyclo〔2,2,1〕hept-2-ene, 5-butyl-bicyclo〔2,2,1〕hept-2-ene, 5-ethyl-bicyclo〔2,2,1〕hept-2-ene, 5-hexyl-bicyclo〔2,2,1〕hept-2-ene, 5-octyl-bicyclo〔2,2,1〕hept-2-ene, 5-octadecyl- Bicyclic olefins such as bicyclo[2,2,1]hept-2-ene, 5-methylene-bicyclo[2,2,1]hept-2-ene, 5-vinyl-bicyclo[2,2,1]hept-2-ene, 5-propenyl-bicyclo[2,2,1]hept-2-ene, tricyclo[4,3,0,12.5]dec-3,7-diene, tricyclo[4,3,0,12.5]dec-3-ene, tricyclo[4,3,0,12.5]undec-3,7-diene, tricyclo[4,3,0,12.5]undec-3,8-diene, tricyclo[4,3,0,12.5]undec-3-ene, 5-cyclopentyl-bicyclo[2,2,1]hept-2-ene, 5-cyclohexyl-bicyclo[2,2,1]hept-2-ene , tricyclic olefins such as 5-cyclohexenylbicyclo〔2,2,1〕hept-2-ene, 5-phenyl-bicyclo〔2,2,1〕hept-2-ene, tetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-methyltetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-ethyltetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-methylenetetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-ethyltetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-vinyltetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8 -propenyl-tetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, and tetracyclic olefins such as 8-cyclopentyl-tetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-cyclohexyl-tetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-cyclohexenyl-tetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, 8-phenyl-cyclopentyl-tetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene, tetracyclo〔7,4,13.6,01.9,02.7〕tetradec-4,9,11,13-tetraene, tetracyclo〔8,4,14.7,01.10,03.8〕pentadeca-5,10,12,14-tetraene, pentacyclo〔6,6,13.6,02.7,09.14〕-4-hexadecene, pentacyclo〔6,5,1,13.6,02.7,09.13〕-4-pentadecaene, pentacyclo〔7,4,0,02.7,13.6,110.13〕-4-pentadecaene, heptacyclo〔8,7,0,12.9,14.7,111.17,03.8,012.16〕-5-eicosene, heptacyclo〔8,7,0,12.9,03.8,14.7,012.17,113.16〕-14-eicosene, cyclopentadiene and other polycyclic olefins such as tetramers. These cyclic olefin monomers can be used alone or in combination of two or more. .
[0090] As the cyclic olefin monomer, among the above, from the viewpoint of productivity and surface properties, it is preferable to use a tricyclic olefin having 10 carbon atoms such as bicyclo〔2,2,1〕hept-2-ene (hereinafter referred to as norbornene), a tricyclic olefin having 10 carbon atoms such as tricyclo〔4,3,0,12.5〕dec-3-ene (hereinafter referred to as tricyclodecene), a tetracyclic olefin having 12 carbon atoms such as tetracyclo〔4,4,0,12.5,17.10〕dodec-3-ene (hereinafter referred to as tetracyclododecene), cyclopentadiene, or 1,3-cyclohexadiene.
[0091] The cyclic olefin resin may be any of a resin obtained by polymerizing only the cyclic olefin monomer (hereinafter sometimes referred to as COP) and a resin obtained by copolymerizing the cyclic olefin monomer and a chain olefin monomer (hereinafter sometimes referred to as COC) as long as it satisfies the above definition.
[0092] As a method for producing COP, known methods such as addition polymerization or ring-opening polymerization of cyclic olefin monomers can be cited, for example, a method of subjecting norbornene, tricyclodecene, tetracyclodecene and derivatives thereof to ring-opening metathesis polymerization and then hydrogenating them, a method of subjecting norbornene and derivatives thereof to addition polymerization, a method of subjecting cyclopentadiene and cyclohexadiene to 1,2- and 1,4-addition polymerization and then hydrogenating them, etc. Among them, a method of subjecting norbornene, tricyclodecene, tetracyclodecene and derivatives thereof to ring-opening metathesis polymerization and then hydrogenating them is more preferred from the viewpoint of productivity and moldability.
[0093] In the case of COC, preferred chain olefin monomers include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene.
[0094] Among them, from the viewpoints of productivity, cost, and compatibility with polypropylene resin, ethylene or propylene can be particularly preferably used, and they can be used together. In addition, as a method for manufacturing a resin in which a cyclic olefin monomer and a chain olefin monomer are copolymerized, known methods such as the addition polymerization of a cyclic olefin monomer and a chain olefin monomer can be cited. In particular, from the viewpoints of productivity and moldability, a method of using a binary polymerization or a ternary polymerization consisting of norbornene or tetracyclododecene and their derivatives, and ethylene and / or propylene can be used as a preferred method. That is, for example, a binary polymerization of a tetracyclododecene derivative and ethylene, and a ternary polymerization of norbornene, ethylene, and propylene can be used as a preferred method.
[0095] The cyclic olefin resin used in the polypropylene film of the present invention is preferably amorphous. The glass transition temperature of the amorphous cyclic olefin resin is preferably 125°C or more and 175°C or less. By setting the glass transition temperature to 125°C or more and 175°C or less, the followability to the polypropylene resin can be improved during the molding process, and it becomes easy to suppress the uneven thickness of the film. Therefore, the reliability and withstand voltage at high temperatures of the film capacitor using the polypropylene film of the present invention can be improved. From the above viewpoints, the glass transition temperature is more preferably 130°C or more, and more preferably 135°C or more. On the other hand, from the viewpoint of molding processability, the glass transition temperature is more preferably 160°C or less, more preferably 150°C or less, and particularly preferably 142°C or less.
[0096] In particular, when stretching and subsequent relaxation treatment are performed during the molding process, if the glass transition temperature is designed to be 25°C or more lower than the heat treatment temperature, the polypropylene film with excellent long-term thermal stability and high reliability can be easily manufactured when used as a film capacitor. In addition, the cyclic olefin resin in the polypropylene film of the present invention is amorphous, which is defined as the fact that the melting peak temperature (Tm) obtained when the cyclic olefin resin is heated from 30°C to 260°C by a differential scanning calorimeter DSC at 20°C / min is not observed.
[0097] In the polypropylene film of the present invention, the glass transition temperature of the cyclic olefin resin can be measured as follows according to JIS K7121-1987. Using a differential scanning calorimeter, 3 mg of the film or resin is heated from 30 ° C to 260 ° C at 20 ° C / minute in a nitrogen atmosphere, then, after being kept at 260 ° C for 5 minutes, the temperature is lowered to 30 ° C at 20 ° C / minute. Further, after being kept at 20 ° C for 5 minutes, the temperature is raised from 30 ° C to 260 ° C at 20 ° C / minute as a re-heating. From the DSC curve obtained during the re-heating process, the glass transition temperature (Tg) is calculated by the following formula. In addition, the differential scanning calorimeter is not particularly limited as long as it can be measured, and a known one can be used, for example, EXSTAR DSC6220 made by Seiko Instruments can be used.
[0098] Glass transition temperature = (extrapolated glass transition start temperature + extrapolated glass transition end temperature) / 2.
[0099] From the viewpoint of eliminating defects and voids and improving withstand voltage, the polypropylene film of the present invention preferably has a total light transmittance of 85% or more and 99.9% or less. Here, the so-called total light transmittance is the total light transmittance when light is incident perpendicularly to the film surface, in other words, the total light transmittance in the film thickness direction. In addition, from the above viewpoint, the total light transmittance is more preferably 88% or more, further preferably 91% or more, and particularly preferably 94% or more. From the viewpoint of feasibility, the upper limit is 99.9%. In addition, the total light transmittance can be measured with a known haze meter, which is described in detail below.
[0100] There are no particular limitations on the method for bringing the total light transmittance into a suitable range, and when the polypropylene film contains a cyclic olefin resin, examples include a method of pre-mixing the cyclic olefin resin with the polypropylene resin, adding a branched polypropylene to the surface layer, and forming a laminated structure in which a layer A is sandwiched between layers B (for example, B / A / B). In order to increase the total light transmittance, it is also effective to reduce the amount of the cyclic olefin resin in the entire polypropylene film after forming the laminated structure as described above.
[0101] The polypropylene film of the present invention may contain various additives, such as organic particles, inorganic particles, crystal nucleating agents, antioxidants, heat stabilizers, chlorine scavengers, slip agents, antistatic agents, antiblocking agents, fillers, viscosity modifiers, and anti-coloring agents, within a range not impairing the purpose of the present invention.
[0102] When an antioxidant is contained among them, the type and amount of the antioxidant are important from the viewpoint of long-term heat resistance. That is, as such an antioxidant, a sterically hindered phenolic antioxidant is used, and at least one of them is preferably a high molecular weight antioxidant with a molecular weight of 500 or more. As specific examples thereof, various substances can be cited, for example, preferably 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (for example, BASF "Irganox" (registered trademark) 1330: molecular weight 775.2) or tetrakis[methylene-3(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane (for example, BASF "Irganox" (registered trademark) 1010: molecular weight 1,177.7) and the like are used together with 2,6-di-tert-butyl-p-cresol (BHT: molecular weight 220.4).
[0103] The total content of high molecular weight antioxidants with a molecular weight of 500 or more is preferably in the range of 0.1 to 1.0 parts by mass relative to the total amount of resin. If the antioxidant is too little, the long-term heat resistance is sometimes poor. If the antioxidant is too much, the capacitor element is sometimes adversely affected due to the adhesion at high temperatures caused by the seepage of these antioxidants. A more preferred total content is 0.2 to 0.7 parts by mass of the total mass of the resin, and 0.3 to 0.5 parts by mass is particularly preferred. In the case of a laminated structure of more than two layers, the high molecular weight antioxidant with a molecular weight of 500 or more in each layer is 0.3 to 0.5 parts by mass, which is preferred from the viewpoint of suppressing defects such as fish eyes and obtaining high quality and withstand voltage performance.
[0104] The polypropylene film of the present invention may include resins other than polypropylene resin (A) and cyclic olefin resins in the range that does not damage the purpose of the present invention. As specific resins, vinyl polymer resins, polyester resins, polyamide resins, polyphenylene sulfide resins, polyimide resins, polycarbonate resins, etc., including various polyolefin resins can be cited, and polymethylpentene, syndiotactic polystyrene, etc. are particularly preferably exemplified. When the resin component constituting the polypropylene film is set to 100% by mass as a whole, the content of these resins is preferably less than 3% by mass, more preferably less than 2% by mass, and further preferably less than 1% by mass. If the content of the resin other than the polypropylene resin is more than 3% by mass, the influence of the domain interface becomes large, so sometimes the insulation breakdown voltage under high temperature environment is reduced.
[0105] The polypropylene film of the present invention is preferably used as a dielectric film for a film capacitor, but the type of film capacitor is not limited. Specifically, from the viewpoint of electrode composition, it can be any of a wound film capacitor of a metal foil and a film, a metal vapor-deposited film capacitor, and is also preferably used in an oil-immersed film capacitor impregnated with insulating oil, or a dry capacitor that does not use insulating oil at all. However, according to the characteristics of the polypropylene film of the present invention, it is preferably used as a metal vapor-deposited film capacitor. From the viewpoint of shape, it can be a wound type or a laminated type.
[0106] Polypropylene film generally has low surface energy and is difficult to stably perform metal deposition. Therefore, in order to improve the adhesion to the metal film, it is preferably subjected to surface treatment before deposition. Specifically, the surface treatment includes corona discharge treatment, plasma treatment, glow treatment, flame treatment, and the like.
[0107] The polypropylene film of the present invention can be obtained by using a raw material that can obtain the above-mentioned properties, and performing biaxial stretching, heat treatment and relaxation treatment. As a biaxial stretching method, it can be obtained by a blowing simultaneous biaxial stretching method, a tenter simultaneous biaxial stretching method, and a tenter sequential biaxial stretching method. Among them, the tenter sequential biaxial stretching method and the tenter simultaneous biaxial stretching method are preferably used in terms of improving the film forming stability, crystalline / amorphous structure, surface characteristics, and especially the stretching ratio of the present invention while controlling the mechanical characteristics and thermal dimensional stability.
[0108] Next, a material using polypropylene resin (A) as the polypropylene resin (material whose main component is polypropylene resin (A)) is cited as an example to illustrate the method for manufacturing the polypropylene film of the present invention. First, the resin raw material is diluted or directly melt-extruded on a support to form an unstretched film. As the resin raw material, it is preferred to use a composite resin in which a cyclic olefin resin and a polypropylene resin (A) are pre-mixed. The unstretched film is stretched in the length direction and then stretched in the width direction to perform biaxial stretching in succession. Then, a heat treatment and a relaxation treatment are performed to manufacture a biaxially oriented polypropylene film. The following is described in more detail, but the present invention is not necessarily limited to this and is interpreted.
[0109] First, for the polypropylene film of the present invention, from the viewpoint of making the dispersion state of the cyclic olefin resin and the polypropylene resin (A) good, especially improving the insulation breakdown voltage of the film at high temperature, it is preferred to pre-mix the cyclic olefin resin with the polypropylene resin and the antioxidant for compounding to form a composite resin. Single-screw extruders, twin-screw extruders, etc. can be used in the compounding, but from the viewpoint of good dispersion state and high transparency, it is particularly preferred to use a twin-screw extruder. The resin temperature during compounding is preferably included in the following temperature range. First, it is preferably below 300°C, more preferably below 280°C. On the other hand, it is preferably above 200°C, more preferably above 230°C.
[0110] When the composite resin component as a whole is set to 100% by mass, the content of the cyclic olefin resin in the composite resin is preferably 0.5% by mass or more, more preferably 1% by mass or more, further preferably 4% by mass or more, particularly preferably 10% by mass or more, and from an economic point of view, more preferably 15% by mass or more, further preferably 25% by mass or more. On the other hand, from the viewpoint of improving the dispersion state of the cyclic olefin resin, the content of the cyclic olefin resin in the composite resin is preferably 49% by mass or less, preferably 40% by mass or less, and preferably 36% by mass or less.
[0111] The amount of the antioxidant is preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, and further preferably 0.4 parts by mass or more relative to 100 parts by mass of the composite resin component. The upper limit is set to 1.0 parts by mass. In addition, by making the meso pentad fraction of the polypropylene resin (A) 0.960 or more, the melting point becomes high, which is suitable for use at high temperatures, and is therefore preferred.
[0112] Next, the polypropylene resin (A) and the composite resin are supplied to a single screw extruder, and extruded from a slit die after passing through a filter for filtration. The molten sheet extruded from the slit die is solidified on a temperature-controlled casting drum (cooling drum) to obtain an unstretched polypropylene film. The temperature of the cooling drum is preferably 10° C. or higher, and on the other hand, preferably 110° C. or lower.
[0113] From the viewpoint of increasing the area stretch ratio, a laminated structure is preferred. In this case, the composite resin for layer A is mixed with the polypropylene resin (A) and supplied to the single screw extruder for the inner layer (layer A), and the polypropylene resin (A) is supplied to the single screw extruder for the surface layer (layer B). Then, the resin having a three-layer structure of layer B / layer A / layer B is laminated in a feed block manner by melt co-extrusion and extruded from a slit-shaped die as a molten sheet, and solidified on a temperature-controlled cooling drum to obtain an unstretched polypropylene film. The temperature of the cooling drum is preferably above 10°C. On the other hand, the temperature of the cooling drum is preferably below 110°C, and more preferably below 95°C.
[0114] As a method for bonding the molten sheet to the casting drum, any of the following methods can be used: an electrostatic application method, a bonding method using the surface tension of water, an air knife method, a pressure roll method, an underwater casting method, an air chamber method, etc., but the air knife method is preferred because it has good planarity and can control surface roughness. In addition, in order to prevent vibration of the film, it is preferred to appropriately adjust the position of the air knife so that the air flows to the downstream side of the film forming process.
[0115] Next, the unstretched polypropylene film is biaxially stretched and biaxially oriented. During stretching, the unstretched polypropylene film is brought into contact with a roller set to a predetermined longitudinal stretching temperature and stretched in the longitudinal direction at a predetermined ratio. The longitudinal stretching temperature is preferably above 100°C, more preferably above 120°C, and further preferably above 148°C. On the other hand, the longitudinal stretching temperature is preferably below 170°C, more preferably below 165°C, and further preferably below 160°C. The stretching ratio in the longitudinal direction is preferably above 4.0 times, more preferably above 4.5 times, and further preferably above 5.0 times. On the other hand, it is preferably below 10 times. After stretching in the longitudinal direction, it is cooled to room temperature.
[0116] Next, the polypropylene film that has been uniaxially stretched in the length direction is guided to a tenter while being held by clamps at both ends in the width direction. In the present invention, it is preferred that the tenter atmosphere temperature (preheating temperature in the width direction) in the preheating process immediately before stretching in the width direction is preferably above the stretching temperature in the width direction + 5°C. On the other hand, the temperature in the preheating process is preferably below the stretching temperature in the width direction + 15°C, more preferably below + 12°C, and further preferably below + 10°C. By bringing the temperature of the preheating process within the above range, the fibril structure that has been highly oriented in the length direction by uniaxial stretching can be further strengthened, and the dielectric breakdown voltage of the polypropylene film can be improved. In addition, after uniaxial stretching, it is preferred to stabilize the insufficiently oriented molecular chains by high-temperature preheating from the viewpoint that thermal dimensional stability can be improved.
[0117] Next, from the viewpoint of uniformly stretching the cyclic olefin resin with a high glass transition temperature and improving the reliability of the film capacitor, the tentering machine atmosphere temperature (stretching temperature in the width direction) for stretching the film in the width direction while the ends of the film are held by a clamp is preferably 150° C. or more, more preferably 155° C. or more, and further preferably 170° C. or more. On the other hand, from the above viewpoint, the stretching temperature in the width direction is preferably 190° C. or less, and more preferably 185° C. or less.
[0118] From the viewpoint of improving the dielectric breakdown voltage of the film, the stretching ratio in the width direction is preferably 7.4 times or more, more preferably 8.5 times or more, further preferably 9.3 times or more, and particularly preferably 10.0 times or more. On the other hand, from the viewpoint of stably making a film, the stretching ratio in the width direction is preferably 20.0 times or less, more preferably 17.0 times or less, and further preferably 15.0 times or less. If the stretching ratio in the width direction is less than 7.4 times, the orientation contribution of the fibril structure highly oriented along the length direction by uniaxial stretching remains largely, so sometimes when the dielectric breakdown voltage is evaluated at high temperature, the molecular chains in the film are easy to move and become a film with a dielectric breakdown voltage difference. Compared with the length direction, the stretching ratio in the width direction is increased, and since the orientation in the width direction is given under the state of maintaining the high orientation state in the length direction, the molecular chains in the plane are tightened and increased, so as to obtain the effect of improving the dielectric breakdown voltage, especially at high temperature, and therefore it is preferred.
[0119] Here, the area stretch ratio is preferably 40.0 times or more. By making the area stretch ratio 40.0 times or more, the molecular chain tension in the film surface is increased and F(A23)+F(B23) can be easily increased. As a result, the resulting film has a high dielectric breakdown voltage, especially at high temperatures. In the present invention, the so-called area stretch ratio is a value obtained by multiplying the stretch ratio in the length direction by the stretch ratio in the width direction. The area stretch ratio is more preferably 40.0 times or more, further preferably 42.0 times or more, and particularly preferably 49.0 times or more. The upper limit of the area stretch ratio is not particularly limited, but from the viewpoint of feasibility, it is 90.0 times in the case of successive biaxial stretching and 150 times in the case of simultaneous biaxial stretching.
[0120] The important point in the present invention is to achieve a high area stretch ratio while keeping the shrinkage in the main orientation direction low. That is, in the present invention, by increasing the dispersibility of the cyclic olefin resin domains dispersed in the polypropylene resin and carrying out the heat setting temperature after biaxial stretching at a high temperature, a structure in which the domains are enlarged is formed in the plane without generating micro-voids in the domain interface of the cyclic olefin resin, and at the same time, the tension state of the polypropylene that causes shrinkage is relaxed, so that the shrinkage in the main orientation direction can be kept low while achieving a high area stretch ratio.
[0121] In the manufacture of the polypropylene film of the present invention, for the subsequent heat treatment and relaxation treatment process, a relaxation of 2 to 20% is given in the width direction while the width direction is held tightly by a clamp, and the heat treatment is performed at a temperature of 165°C or more and 190°C or less and at a temperature of the glass transition temperature of the cyclic olefin resin + 30°C or more at the tenter atmosphere temperature. From the viewpoint of improving the reliability of the film capacitor when it is made, it is preferred, and more preferably 172°C or more. In addition, by performing the heat treatment at a temperature above the melting point of the polypropylene resin used and 30°C or more higher than the glass transition temperature of the cyclic olefin resin used, the reliability of the film capacitor can be effectively improved. From the above viewpoints, the relaxation treatment rate is preferably 5% or more, more preferably 7% or more, and further preferably 9% or more. On the other hand, from the viewpoint of improving the insulation breakdown voltage of the polypropylene film, the relaxation treatment is more preferably 18% or less, and further preferably 15% or less.
[0122] After the heat treatment and relaxation treatment, the film is guided to the outside of the tenter, the clamps at the film ends are released at room temperature, and the film edges are cut in the winding process to wind up a film product roll with a thickness of 0.50 μm or more and less than 5.0 μm. In order to improve the adhesion of the vapor-deposited metal, it is preferred to perform a corona discharge treatment on the vapor-deposited surface in air, nitrogen, carbon dioxide or a mixed gas thereof before winding the polypropylene film.
[0123] In addition, in order to obtain the polypropylene film of the present invention, if an attempt is made to specifically cite the production conditions of interest, the following is an example. In addition, it is preferred that all of these production conditions are satisfied, but not necessarily all of them are available, and appropriate combinations can be made. For example, instead of "the preheating temperature before stretching in the width direction in the sequential biaxial stretching is the stretching temperature in the width direction + 5°C or more and + 15°C or less.", simultaneous biaxial stretching can be used.
[0124] The meso pentad fraction of the polypropylene resin as the main component is 0.960 or more.
[0125] The present invention comprises the above-mentioned layer A and layer B, wherein the layer B contains branched polypropylene.
[0126] · Pre-mix the cyclic olefin resin and the polypropylene resin.
[0127] The content of the cyclic olefin-based resin is set to 1% by mass or more and 39% by mass or less.
[0128] The area stretching ratio of the biaxial stretching is 40.0 times or more.
[0129] The stretching ratio in the width direction is higher than that in the length direction.
[0130] In the sequential biaxial stretching, the preheating temperature before stretching in the width direction is the stretching temperature in the width direction + 5 to + 15°C.
[0131] After biaxial stretching, heat treatment and relaxation treatment are performed.
[0132] The heat treatment temperature after biaxial stretching is 165° C. or higher and the glass transition temperature of the cyclic olefin resin + 30° C. or higher.
[0133] Next, a metal film laminated film formed using the polypropylene film of the present invention, a film capacitor formed using the metal film laminated film, and methods for producing the same will be described.
[0134] The metal film laminated film of the present invention has a metal film on at least one side of the polypropylene film of the present invention. The metal film laminated film can be obtained by providing a metal film on at least one side of the polypropylene film of the present invention.
[0135] In the present invention, the method of applying the metal film is not particularly limited, and preferably, for example, a method of evaporating aluminum or an alloy of aluminum and zinc on at least one side of a polypropylene film to form a metal film such as an evaporation film that becomes an internal electrode of a film capacitor is used. In this case, other metal components such as nickel, copper, gold, silver, chromium, etc. may also be evaporated simultaneously or successively with the aluminum. In addition, a protective layer may be provided on the evaporation film using oil or the like. In the case where the surface roughness of the polypropylene film is different on the front and back sides, it is preferred to provide a metal film on the surface side with a smooth roughness to form a metal film laminate film from the viewpoint of improving the withstand voltage.
[0136] In the present invention, after forming the metal film, the metal film laminate can be annealed or heat treated at a specific temperature as needed. In addition, for insulation or other purposes, at least one side of the metal film laminate can be coated with a resin such as polyphenylene ether.
[0137] The film capacitor of the present invention is formed by using the metal film laminated film of the present invention. That is, the film capacitor of the present invention has the metal film laminated film of the present invention. For example, the film capacitor of the present invention can be obtained by laminating or winding the metal film laminated film of the present invention by various methods. If a preferred manufacturing method of a wound film capacitor is exemplified, it is as follows.
[0138] Aluminum is deposited on one side of a polypropylene film under reduced pressure. At this time, the deposition is in the form of stripes with blank portions running in the length direction. Next, a knife is inserted in the center of each deposition portion and each blank portion on the surface to make a strip-shaped winding reel with a blank portion on one side of the surface. For the strip-shaped winding reel with a blank portion on the left or right, two sheets of the left blank and the right blank are overlapped and wound in such a way that the deposition portion exceeds the blank portion in the width direction to obtain a winding body.
[0139] When vapor deposition is performed on both sides, one side is vapor deposited in a stripe shape with blank portions running in the length direction, and the other side is vapor deposited in a stripe shape in a manner that the blank portion in the length direction is located in the center of the vapor deposition portion on the back side. Next, a knife is inserted into the center of the blank portions on the front and back sides to cut, and a strip-shaped winding reel is made with blanks on one side of each side (for example, if there is a blank on the right side of the front side, there is a blank on the left side of the back side). The obtained reel and one undeposited counterfilm are overlapped and wound in such a way that the metallized film exceeds the counterfilm in the width direction to obtain a wound body.
[0140] As a method for obtaining the film capacitor of the present invention from the metal layer laminated film of the present invention, for example, a core material is pulled out from the wound body produced by the above operation and pressed, metal is sprayed on both end faces to form external electrodes, and leads are welded on the metal spraying to form a wound film capacitor. The uses of film capacitors are spread over many aspects such as electric vehicles, hybrid vehicles, fuel cell vehicles and other electric vehicles, power control units of electric aircraft such as remote-controlled unmanned aircraft, railway vehicle uses, solar power generation / wind power generation uses and general household appliances, and the film capacitor of the present invention can also be suitable for these uses. In addition, the polypropylene film of the present invention can also be used in various uses such as packaging films, demoulding films, process films, sanitary products, agricultural products, construction products, medical products, etc., and can be particularly preferably used for uses including heating processes in film processing.
[0141] The preferred capacitance density of the film capacitor of the present invention is 1.1 μF / cm 3 Above and 18μF / cm 3 The higher the capacitance density of a film capacitor, the smaller the volume of a capacitor element with the same capacitance, and the more compact it can be. Therefore, 1.5 μF / cm is more preferable. 3 From the viewpoint of miniaturization of the film capacitor, the higher the capacitance density of the film capacitor, the better. However, from the viewpoint of feasibility, 18 μF / cm is preferred. 3 Below, preferably 5.0 μF / cm 3 the following.
[0142] By using a film having a thickness of 4.5 μm or less as the polypropylene film of the present invention, the capacitance density of the film capacitor can be 1.1 μF / cm 3 The above is made easy by using a film with a thickness of 3.5 μm or less, so that the capacitance density of the film capacitor can be 1.5 μF / cm 3 The above becomes easy.
[0143] In addition, the capacitance density of the film capacitor in the present invention can be calculated by dividing the element capacitance (μF) by the element volume (cm 3) and calculated. The component capacity can be measured at a frequency of 1 kHz and an ambient temperature of 23°C in accordance with JIS C 4908:2007. In addition, the so-called component volume is the volume of the portion around which the vapor-deposited film is wound, excluding the external packaging material, metal spraying, and the reel, and can be measured by a known 3D scanner type three-dimensional measuring machine. The method for measuring the capacitance density of a film capacitor is described in detail below.
[0144] The film capacitor of the present invention preferably has a withstand voltage of 0.60 kV or more at 135° C. The withstand voltage is more preferably 0.75 kV or more, and further preferably 1.0 kV or more. The polypropylene film of the present invention has a high withstand voltage at high temperatures due to the above characteristics, so by using the polypropylene film of the present invention as a dielectric of a film capacitor, it becomes easy to make the withstand voltage at 135° C. 0.60 kV or more or the above preferred range.
[0145] The power control unit, electric vehicle, and electric aircraft of the present invention are described below. The power control unit of the present invention has the film capacitor of the present invention. The power control unit is a system for managing power in an electric vehicle, electric aircraft, etc. having a mechanism driven by electricity. By installing the film capacitor of the present invention in the power control unit, the power control unit itself can be miniaturized, heat-resistant, and efficient, and as a result, the energy consumption rate is improved.
[0146] The electric vehicle of the present invention has the power control unit of the present invention. The so-called electric vehicle here refers to a car having a mechanism driven by electricity, such as an electric car, a hybrid car, and a fuel cell car. As described above, the power control unit of the present invention is not only miniaturized, but also has excellent heat resistance and efficiency. Therefore, the electric vehicle is equipped with the power control unit of the present invention, thereby improving the energy consumption rate.
[0147] The electric aircraft of the present invention has the power control unit of the present invention. Here, the so-called electric aircraft refers to an aircraft having a mechanism driven by electricity, such as a manned electric aircraft and a remote-controlled unmanned aircraft. As described above, the power control unit of the present invention is not only miniaturized, but also has excellent heat resistance and efficiency. Therefore, the electric aircraft is equipped with the power control unit of the present invention, thereby improving the energy consumption rate.
[0148] The packaging material of the present invention is characterized by having the polypropylene film of the present invention. The packaging material of the present invention has excellent structural stability against heat during vapor deposition, and particularly has good water vapor barrier properties and oxygen barrier properties when a transparent vapor-deposited layer is laminated, so it can be suitably used for packaging materials that are easily degraded by water vapor and oxygen.
[0149] Example
[0150] The polypropylene film of the present invention is described in more detail below by way of examples. However, the polypropylene film of the present invention is not limited to these examples. In addition, the method for measuring the characteristic values and the method for evaluating the effects in the present invention are as follows.
[0151] [Measurement and evaluation methods]
[0152] (1) Film thickness
[0153] The thickness of the polypropylene film was measured at 10 random locations using a contact-type electronic micrometer (K-312A model) manufactured by Anritsu Co., Ltd. in an atmosphere of 23° C. and 65% RH. The arithmetic mean of the thickness at the 10 locations was defined as the film thickness of the polypropylene film (unit: μm).
[0154] (2) The main orientation direction and the orthogonal direction of the film
[0155] In the present invention, the main orientation direction of the film is determined by the above method. The main orientation direction of the film described in the examples is determined more specifically as follows. In addition, the main orientation orthogonal direction is defined as a direction orthogonal to the main orientation direction in the film plane.
[0156] Examples 1 to 7 and Comparative Examples 1, 3, and 4: Since the films were produced by sequential biaxial stretching in a manner such that the transverse stretching ratio was higher than the longitudinal stretching ratio, the transverse stretching direction was set as the main orientation direction.
[0157] Comparative Example 2: Since the film was produced by simultaneous biaxial stretching so that the transverse stretching ratio was higher than the longitudinal stretching ratio, the transverse stretching direction was set as the main orientation direction.
[0158] Comparative Example 5: Since the film was not stretched, the main orientation direction was determined by using the above-mentioned stretching test method.
[0159] (3) Melting peak temperature (Tm) of resin and film
[0160] Using a differential scanning calorimeter (EXSTAR DSC6220 manufactured by Seiko Instruments), 3 mg of the film was heated from 30°C to 260°C at 20°C / min in a nitrogen atmosphere, then kept at 260°C for 5 minutes and then cooled to 30°C at 20°C / min. The endothermic peak temperature obtained during the heating process was set as the melting peak temperature of the film. In this embodiment, (Tm) was calculated from the average value of n=3 measurements. There are cases where two or more peak temperatures are observed in the range of more than 170°C and less than 200°C, and where observable peak temperatures appear in a multi-stage DSC graph called a shoulder (observed in the case of a graph where two or more peaks overlap). In this embodiment, the temperature of the peak with the largest absolute value of the heat flow (unit: mW) on the vertical axis of the DSC graph is set as (Tm)(°C). In addition, the (Tm) of the resin was also measured in the same manner.
[0161] (4) Glass transition temperature (Tg) of cyclic olefin resin
[0162] The temperature was measured according to JIS K7121-1987. Using a differential scanning calorimeter (EXSTAR DSC6220 manufactured by Seiko Instruments), 3 mg of the film or resin was heated from 30°C to 260°C at 20°C / min in a nitrogen atmosphere, then kept at 260°C for 5 minutes and then cooled to 30°C at 20°C / min. Further, after being kept at 20°C for 5 minutes, the temperature was raised from 30°C to 260°C at 20°C / min as a re-heating. The glass transition temperature (Tg) was calculated from the DSC curve obtained during the re-heating process by the following formula.
[0163] Glass transition temperature = (extrapolated glass transition start temperature + extrapolated glass transition end temperature) / 2.
[0164] (5) F(A23) and F(B23)
[0165] A rectangular polypropylene film (width (short side) 10 mm × length (long side) 150 mm) cut out with the film test length direction (main orientation direction or main orientation orthogonal direction) as the long side direction was used as the measurement sample. Next, the sample was placed in a tensile testing machine (Orientec "Tensilon" (registered trademark) UCT-100) with an initial chuck distance of 20 mm, and the tensile test of the film was performed in a room at 23°C with the tensile speed set to 300 mm / min. At this time, the position of the sample in the length direction was adjusted so that the center of the sample was located near the center of the chucks. The load applied to the film when the sample broke was read, and the value obtained by dividing the cross-sectional area of the sample before the test (film thickness × width (10 mm)) was calculated as the strength (unit: MPa). The samples for measurement in the length direction and width direction were measured 5 times each, and the strength in the test length direction was calculated as the arithmetic mean. The strength when the test length direction is the main orientation direction is F(A23), and the strength when the test length direction is the main orientation orthogonal direction is F(B23). The film thickness used to calculate the strength is the value measured in (1) above.
[0166] (6) Shrinkage measured at 150°C
[0167] With respect to the main orientation direction and the main orientation orthogonal direction of the film, five samples with a width of 10 mm and a length of 200 mm (measurement direction) were cut out, and marks were made at 25 mm from both ends to set the test length to 150 mm (l 0 Next, the test piece was sandwiched between paper and placed in an oven kept at 150°C with zero load. After heating for 15 minutes, it was taken out and cooled to room temperature. The size (l 1 ), and was determined using the following formula: For each direction, the arithmetic mean of the heat shrinkage rates of five samples was defined as the heat shrinkage rate measured at 150° C. in that direction.
[0168] Thermal shrinkage = {(l 0 -l 1 ) / l 0}×100(%).
[0169] (7) Development area ratio Sdr
[0170] The developed area ratio was measured and calculated in accordance with ISO25178 (2012). The measurement was performed using a scanning white interference microscope "VS1540" (manufactured by Hitachi High-Tech Science & Technology Co., Ltd., the measurement conditions and device configuration are described below). In addition, the captured image was supplemented (completely supplemented) by the attached analysis software, and after surface correction was performed using a fourth-order polynomial approximation, it was processed using a median filter (3×3 pixels), and the result was set as the measured electromagnetic surface. In addition, the S-Filter Nesting Index of the S-filter was set to 0.445. Both sides of the film cut into a square shape of 5 cm×5 cm were measured. The intersection of the diagonal lines was set as the first measurement point (point 1), and the positions 1 cm away from the opening point toward each of the four corners were set clockwise as points 2, 3, 4, and 5, respectively, the midpoint of the line segment connecting point 2 and point 3 was set as point 6, the midpoint of the line segment connecting point 3 and point 4 was set as point 7, the midpoint of the line segment connecting point 4 and point 5 was set as point 8, and the midpoint of the line segment connecting point 5 and point 2 was set as point 9. A total of 9 measurement points from point 1 to point 9 were determined, and measurements were performed at each measurement point. From the measurement results, the Sdr of each measurement position was calculated according to the above steps, and the average value of the five values other than the first and second largest values and the eighth and ninth largest values among the 9 values obtained for each surface was used as the Sdr of the film on the surface. In Tables 1-2 and 2-2, for convenience, one surface of the film was set as surface 1, and the back surface was set as surface 2 to determine the surface, and the Sdr of each surface was recorded.
[0171] <Measurement conditions and device configuration>
[0172] Objective lens: 10x
[0173] Tube: 1x
[0174] Variable focal length lens: 1x
[0175] Wavelength filter: 530nm white
[0176] Measurement mode: Wavelength
[0177] Measurement software: VS-Measure 10.0.4.0
[0178] Analysis software: VS-Viewer10.0.3.0
[0179] Measurement area: 561.1μm×561.5μm
[0180] Number of pixels: 1,024 × 1,024.
[0181] (8) Total light transmittance
[0182] The haze meter (HGM-2DP) manufactured by Suga Testing Instrument Co., Ltd. was used for measurement under the following device configuration and optical conditions. The polyolefin film was cut into 6.0 cm × 3.0 cm pieces, and light was incident perpendicularly to the surface of the polyolefin film for measurement. The total light transmittance in the film thickness direction was obtained from the measured value at that time. In addition, the measurement was performed 5 times, and the average value was set as the total light transmittance.
[0183] Light source: Halogen lamp 12V, 50W
[0184] Light receiving characteristics: 395~745nm
[0185] Optical conditions: in accordance with JIS-K7105-1981.
[0186] (9) Film insulation breakdown voltage (V / μm)
[0187] When measuring the dielectric breakdown voltage of the film at 135°C, the film was heated for 1 minute in an oven kept at 135°C, and then measured in the atmosphere according to JIS C2330 (2001) 7.4.11.2 B method (flat electrode method). As the lower electrode, a material of "Electrical Conductive Rubber E-100<65>" manufactured by Togawa Gomu Co., Ltd. of the same size as described in JIS C2330 (2001) 7.4.11.2 B method was used. The dielectric breakdown voltage test was performed 30 times, and the obtained value was divided by the thickness of the film (measured by (1) above) to convert it into V / μm. The average value of 20 points other than the 5 points in descending order from the maximum value and the 5 points in descending order from the minimum value among the total 30 measured values (calculated values) was set as the dielectric breakdown voltage at 135°C.
[0188] (10) Evaluation of film capacitor characteristics (withstand voltage at 135°C, reliability), film forming properties, and processability
[0189] On one side of the film (in addition, when the wetting tension is different between the front and back sides, the side with higher wetting tension) aluminum was vapor-deposited with a film resistance of 10Ω / sq and a so-called T-shaped blank (17mm spacing (period) in the longitudinal direction and 0.5mm fuse width by shielding oil) using a vacuum vapor deposition machine manufactured by Albuque Co., Ltd. After cutting, a vapor deposition reel with a film width of 50mm (end blank width of 2mm) was obtained. Next, the reel was used to wind the capacitor element using a component winding machine (KAW-4NHB) manufactured by Kaito Seisakusho Co., Ltd. After metal spraying, it was heat-treated at a temperature of 128°C for 12 hours under reduced pressure, and the lead wires were installed to complete the processing into a capacitor element. Using 10 capacitor elements obtained in this way, a voltage of 150 VDC was applied to the capacitor elements at a high temperature of 135°C. After 10 minutes at this voltage, the applied voltage was gradually increased stepwise at 50 VDC / 1 minute. This operation was repeated to perform a so-called step-up test.
[0190] <Withstand voltage evaluation>
[0191] In the step-up test, the change in electrostatic capacitance is measured and plotted on a graph, and the withstand voltage is calculated by dividing the voltage at which the capacitance becomes 75% of the initial value by the film thickness (the value measured in (1) above), and the average value of 10 capacitor elements is calculated and evaluated according to the following criteria: S, A, B, and C mean that they can be used, and D means that the performance is poor in practical use.
[0192] S: greater than 420V / μm.
[0193] A: greater than 390 V / μm and less than 420 V / μm.
[0194] B: greater than 325 V / μm and less than 390 V / μm.
[0195] C: greater than 300 V / μm and less than 325 V / μm.
[0196] D: 300V / μm or less.
[0197] <Reliability Evaluation>
[0198] After the voltage was increased until the electrostatic capacitance decreased to less than 18% relative to the initial value, the capacitor element with the highest withstand voltage increase among the 10 capacitor elements was disassembled, the state of damage was investigated, and the reliability was evaluated as follows. S means that it can be used, A, B, and C mean that it can be used according to conditions, and D means that the performance is poor in practical use.
[0199] S: Neither change in element shape nor through-breakage was observed.
[0200] A: There is no change in the device shape, and destruction penetrating from one to two layers of the film is observed.
[0201] B: There is no change in the device shape, but destruction penetrating from 3 to 5 layers of the film is observed.
[0202] C: There is no change in the device shape, but destruction penetrating 6 or more layers and 10 or less layers of the film is observed.
[0203] D: Changes in the device shape were observed, or penetration-like damage was observed in 11 or more layers.
[0204] <Film-forming property evaluation>
[0205] The film was continuously formed under the conditions described in the embodiments and comparative examples, and the operation of recording the length of the film that can be wound from the start of winding to the occurrence of film breakage was performed 3 times, and the average value of the 3 times was set as the film length that can be film-formed, and the film-formability was evaluated as follows. A means that the film can be stably formed, B and C mean that the film can be formed although the yield decreases, and D means that it is substantially difficult to form a film. In addition, when no film breakage was observed at the time of winding 15000m, the film length this time was set to 15000m and the next operation was performed.
[0206] A: The film length that can be produced is 10,000 m or more.
[0207] B: The film length that can be produced is 5000 m or more and less than 10000 m.
[0208] C: The film length that can be produced is 1000 m or more and less than 5000 m.
[0209] D: The film length that can be produced is less than 1000 m.
[0210] <Processability Evaluation>
[0211] When the polypropylene film was cut after the above-mentioned vapor deposition, the processability was evaluated according to the following evaluation criteria based on the frequency of the film breaking. In the evaluation criteria, "A" means that it can be used, "B" and "C" mean that it can be used under certain conditions, and "D" means that the performance is poor in practice and it is difficult to use.
[0212] A: The number of fractures per 20,000 m cut length is less than 1.
[0213] B: The number of fractures per 20,000 m of cut length is more than 1 and less than 3.
[0214] C: The number of fractures per 20,000 m of cut length is more than 3 times and less than 10 times.
[0215] D: The number of fractures per 20,000 m of cut length is more than 10 times.
[0216] (11) The number of cyclic olefin resin domains passing through a pair of sides parallel to the thickness direction in a 1 μm × 2 μm rectangle in layer A (domains / 2 μm) 2 )
[0217] The polypropylene film was cut in a plane parallel to the main orientation axis direction and the thickness direction using a slicing method to produce a polypropylene film sheet having a cut surface. 4 After dyeing, the dyed surface was cut to obtain an ultrathin section having a cross section (TD / ZD cross section). The cross section of the ultrathin section was observed using a transmission electron microscope (TEM) under the following conditions. In this case, the cyclic olefin resin was dyed blacker than the polypropylene resin.
[0218] · Equipment: Transmission electron microscope (TEM) HT7700 manufactured by Hitachi, Ltd.
[0219] Accelerating voltage: 100 kV
[0220] Observation magnification: 2,000 times
[0221] In the A layer portion of the cross-sectional TEM image taken, a rectangular 2 μm-diameter square with a pair of sides of 1 μm in the thickness direction and 2 μm in the direction perpendicular to the thickness direction was drawn. 2 The number of domains of the cyclic olefin resin passing through a pair of sides parallel to the thickness direction in the rectangle is counted. The same measurement is performed 10 times with the position of the rectangle in the image changed, and the average value of the obtained number of domains is calculated and set as the number of domains of the cyclic olefin resin passing through a pair of sides parallel to the thickness direction in the A layer (number / 2μm 2 ). In addition, when a rectangle with a pair of sides of 1 μm in the thickness direction and 2 μm in the direction perpendicular to the thickness direction is determined in the cross section X, the bottom side of the rectangle is set as the sea part, and when the domain is located on the side opposite to the bottom side, it is regarded as not existing and is not counted as the number. In addition, domains with constricted parts are also treated as connected domains.
[0222] (12) Cooling crystallization temperature (Tmc) of resin and film
[0223] The measurement was carried out in accordance with JIS7121-1987. First, a differential scanning calorimeter (EXSTAR DSC6220 manufactured by Seiko Instruments) was used to raise the temperature of 3 mg of the film from 30°C to 260°C at 20°C / min in a nitrogen atmosphere, and then, after being kept at 260°C for 5 minutes, the temperature was lowered to 30°C at 20°C / min. The peak temperature of the exothermic peak obtained during the cooling process was measured. In this embodiment, the average value of the peak temperature measured with n=3 was set as the cooling crystallization temperature (Tmc) of the film. When multiple exothermic peaks are observed in one measurement, the peak temperature of the exothermic peak with the highest peak temperature is set as the peak temperature of the measurement.
[0224] (13) Uneven thickness in the length direction
[0225] A sample was cut out from an arbitrary location of the polypropylene film so as to have a length of 200 mm and a width of 20 mm. The film thickness was measured using a contact-type film thickness meter (Litemac VL-50A, manufactured by Midoyo Co., Ltd.) The thickness was measured using a superhard spherical probe with a measuring load of 0.06 N. The thickness measurement position was set at 100 locations at 1 mm intervals in the center of the width direction of the sample with respect to the length direction. The thickness unevenness was calculated using the following formula from the maximum value, minimum value, and average value of 100 locations in the length and width directions.
[0226] Thickness variation (%) = ((maximum thickness - minimum thickness) / average thickness at 100) × 100
[0227] (14) Capacitance density of film capacitors
[0228] The capacitance of 10 capacitor elements was measured in accordance with JIS C 4908:2007 at a frequency of 1 kHz and an ambient temperature of 23°C using the E4980A Filter LCR meter manufactured by Keysight Technologies, and the average value of the 10 capacitor elements was set as the element capacitance. Next, the volume of each capacitor element was measured using a Keyence VL-500 3D scanner type three-dimensional measuring machine, which was set as the element volume. From the obtained values, the capacitance density was calculated for each element according to the following formula, and the average value of the 10 capacitor elements was used as the measured value. In addition, the so-called element volume here is the volume of the part of the vapor-deposited film that does not include the external packaging material, metal spraying, and reel.
[0229] Capacity density (μF / cm 3 ) = component capacitance (μF) / component volume (cm 3 ).
[0230] (15) Withstand voltage of film capacitors at 135°C
[0231] Using 10 capacitor elements, a voltage of 150VDC was applied to the capacitor elements at a high temperature of 135°C. After 10 minutes at this voltage, the applied voltage was slowly increased in steps at 50VDC / 1 minute. This operation was repeated to perform the so-called step-up test. In the step-up test, the change in electrostatic capacitance was measured and plotted on a graph, and the voltage at which the capacitance became 75% of the initial value was recorded as the withstand voltage of the film capacitor at 135°C.
[0232] (16) Film capacitor performance evaluation
[0233] <Lifespan Evaluation>
[0234] Ten capacitor elements were used, and a voltage of 750 VDC was applied to the capacitor elements at a high temperature of 135°C. The capacitor elements were taken out every 100 hours and the capacity was measured. The time when the capacity became less than 90% of the initial value was calculated, and the average value of the ten capacitor elements was calculated as the lifespan, and the evaluation was performed according to the following criteria. A means that it can be used, B means that the performance is poor in practical use, and C means that it is difficult to use.
[0235] A: The service life is more than 3000 hours.
[0236] B: Lifespan is less than 3000 hours and 2000 hours or more.
[0237] C: Lifespan is less than 2000 hours.
[0238] <Component size evaluation (indicator for miniaturization)>
[0239] The volume of 10 capacitor elements was measured using a Keyence VL-500 3D scanner type three-dimensional measuring machine, and the average value was set as the element volume, and the evaluation was performed based on the following criteria. A and B refer to being usable, and C refers to poor performance in practical use. In addition, the element volume referred to here is the same as that used in the measurement of "(14) Capacitance density of film capacitors".
[0240] A: The component volume is 80cm 3 the following.
[0241] B: Component volume is greater than 80cm 3 And 160cm 3 the following.
[0242] C: Component volume greater than 160cm 3 .
[0243] [Resin, etc.]
[0244] In the production of the polypropylene film in each of the Examples and Comparative Examples, the following resins and the like were used.
[0245] <Polypropylene resin>
[0246] Polypropylene resin 1:
[0247] Homopolypropylene having a meso pentad fraction of 0.984, a melting point of 168° C. and a melt flow rate (MFR) of 2.2 g / 10 minutes.
[0248] Polypropylene resin 2:
[0249] Homopolypropylene having a meso pentad fraction of 0.982, a melting point of 167° C. and a melt flow rate (MFR) of 2.2 g / 10 minutes.
[0250] Polypropylene resin 3
[0251] Homopolypropylene having a meso pentad fraction of 0.972, a melting point of 166° C. and a melt flow rate (MFR) of 2.2 g / 10 minutes.
[0252] Polypropylene resin 4:
[0253] Homopolypropylene ("Borclean" (registered trademark) HC300BF manufactured by Borealis AG) having a meso pentad fraction of 0.970, a melting point of 166°C and a melt flow rate (MFR) of 3.3 g / 10 min.
[0254] Branched polypropylene (B1): a branched polypropylene resin having a melt flow rate (MFR) of 2.4 g / 10 min ("Daploy" (registered trademark) WB135HMS manufactured by Borealis AG).
[0255] <Ingredients other than polypropylene resin>
[0256] Cyclic olefin resin (C1):
[0257] "TOPAS" (registered trademark) 6013F-04 manufactured by Polyplastics (resin obtained by copolymerizing ethylene and norbornene (COC), glass transition temperature of 138°C, amorphous)
[0258] Cyclic olefin resin (C2):
[0259] "TOPAS" (registered trademark) 6017S-04 manufactured by Polyplastics (resin obtained by copolymerizing ethylene and norbornene (COC), glass transition temperature of 178°C, amorphous)
[0260] Antioxidants:
[0261] "IRGANOX" (registered trademark) 1010 manufactured by H&S
[0262] <Cyclic olefin resin pre-mixed raw materials>
[0263] Raw materials (A1):
[0264] The components were mixed so that the polypropylene resin 1 was 69.5 parts by mass, the cyclic olefin resin (C1) was 30 parts by mass, and the antioxidant was 0.5 parts by mass, and kneaded and extruded using a twin-screw extruder set at 260° C. The strands were water-cooled and flakes were obtained to prepare a raw material (A1).
[0265] Raw materials (A2-1):
[0266] The components were mixed so that the polypropylene resin 2 was 69.5 parts by mass, the cyclic olefin resin (C1) was 30 parts by mass, and the antioxidant was 0.5 parts by mass, and kneaded and extruded using a twin-screw extruder set at 260° C. The strands were water-cooled and flaked to prepare a raw material (A2-1).
[0267] Raw materials (A2-2):
[0268] The components were mixed so that the polypropylene resin 2 was 54.5 parts by mass, the cyclic olefin resin (C1) was 45 parts by mass, and the antioxidant was 0.5 parts by mass, and kneaded and extruded using a twin-screw extruder set at 260° C. The strands were water-cooled and flakes were obtained as the raw material (A2-2).
[0269] Raw materials (A3)
[0270] The components were mixed so that the polypropylene resin 3 was 69.5 parts by mass, the cyclic olefin resin (C1) was 30 parts by mass, and the antioxidant was 0.5 parts by mass, and kneaded and extruded using a twin-screw extruder set at 260° C. The strands were water-cooled and flaked to prepare the raw material (A3).
[0271] Raw materials (A4):
[0272] The components were mixed so that the polypropylene resin 4 was 54.5 parts by mass, the cyclic olefin resin (C1) was 45 parts by mass, and the antioxidant was 0.5 parts by mass, and kneaded and extruded using a twin-screw extruder set at 260° C. The strands were water-cooled and flakes were obtained as raw material (A4).
[0273] Raw materials (A5):
[0274] The components were mixed so that the polypropylene resin 2 was 54.5 parts by mass, the cyclic olefin resin (C2) was 45 parts by mass, and the antioxidant was 0.5 parts by mass, and kneaded and extruded using a twin-screw extruder set at 260° C. The strands were water-cooled and flakes were obtained to prepare a raw material (A5).
[0275] <Branched polypropylene pre-mixed raw materials>
[0276] Raw materials (D1):
[0277] The components were mixed so that the polypropylene resin 1 was 89.5 parts by mass, the branched polypropylene (B1) was 10 parts by mass, and the antioxidant was 0.5 parts by mass, and kneaded and extruded using a twin-screw extruder set at 260° C. The strands were water-cooled and flaked to prepare a raw material (D1).
[0278] Raw materials (D2):
[0279] The components were mixed so that the polypropylene resin 2 was 89.5 parts by mass, the branched polypropylene (B1) was 10 parts by mass, and the antioxidant was 0.5 parts by mass, and kneaded and extruded using a twin-screw extruder set at 260° C. The strands were water-cooled and flaked to prepare a raw material (D2).
[0280] (Example 1)
[0281] The components were mixed in such a manner that the raw material (A2-1) was 35 parts by mass, the polypropylene resin 2 was 64.6 parts by mass, and the antioxidant was 0.4 parts by mass, and the mixture was supplied to a single screw melt extruder for the A layer. At the same time, the components were mixed in such a manner that the polypropylene resin 2 was 50 parts by mass and the raw material (D2) was 50 parts by mass, and the mixture was supplied to a single screw melt extruder for the B layer. They were melted at a temperature of 260°C, and after removing foreign matter with a sintered filter with a cutoff of 80 μm, the extrusion amount was adjusted using a feed block in such a manner that the 3-layer B / A / B stacking was 1 / 10 / 1 (the ratio of the inner layer A layer to the total thickness of the film was 83%), and the molten stacking polymer was discharged from a T-die. Then, the molten sheet was made to fit tightly on a casting drum maintained at 90°C by an air knife and cooled and solidified to obtain an unstretched polypropylene film. The unstretched polypropylene film was preheated in stages to 145°C using a plurality of roller groups, and then maintained at a temperature of 155°C and passed between rollers with a peripheral speed difference, and stretched to 5.4 times in the longitudinal direction. The film was then guided to a tenter, and preheated at a width direction (TD) preheating temperature of 188°C (6°C higher than the TD stretching temperature) while holding both ends of the film width with clamps, and then stretched 10.4 times in the width direction at a TD stretching temperature of 182°C. As a further heat treatment and relaxation treatment, a heat treatment was performed at 175°C while giving 10% relaxation in the width direction, and then guided to the outside of the tenter to release the clamps, and then the film surface (casting drum contact side) was heated at 25 W·min / m 2 The polypropylene film was obtained by corona discharge treatment in the atmosphere with a treatment intensity of . The evaluation results are shown in Table 1-2.
[0282] (Examples 2 to 5, 8, Comparative Examples 3, 4)
[0283] The polypropylene film was obtained in the same manner as in Example 1 except that the raw material prescription was the raw material prescription described in Table 1-1 and Table 2-1, and the film-forming conditions were the film-forming conditions described in Table 1-2 and Table 2-2. The evaluation results are shown in Table 1-2 and Table 2-2. In addition, the film thickness was adjusted by increasing or decreasing the discharge amount of the extruder (hereinafter, the same applies to other examples and comparative examples).
[0284] (Example 6)
[0285] The components were mixed so that the raw material (A3) was 10 parts by mass, the polypropylene resin 2 was 89.6 parts by mass, and the antioxidant was 0.4 parts by mass, and the mixture was supplied to a single screw melt extruder. The mixture was melted at a temperature of 260°C, and foreign matter was removed by a sintered filter with a cutoff of 80 μm. After the molten polymer was discharged from a T-die, the molten sheet was closely attached to a casting drum maintained at 90°C by an air knife and cooled and solidified. The other film-forming conditions were the film-forming conditions described in Table 1-2. The same operation as in Example 1 was performed to obtain a polypropylene film consisting only of the A layer. The evaluation results are shown in Table 1-2.
[0286] (Example 7, Comparative Examples 1, 5)
[0287] A polypropylene film was obtained in the same manner as in Example 6 except that the raw material prescriptions were the raw material prescriptions in Table 1-1 and Table 2-1, and the film forming conditions were the film forming conditions described in Table 1-2 and Table 2-2. The evaluation results are shown in Table 1-2 and Table 2-2. In addition, Comparative Example 5 is an unstretched film, and the steps from stretching to heat treatment were not performed.
[0288] (Comparative Example 2)
[0289] The components were mixed in such a manner that the polypropylene resin 4 became 79.6 parts by mass, the cyclic olefin resin (C1) became 20 parts by mass, and the antioxidant became 0.4 parts by mass, and were supplied to a single-axis extruder set at 260°C. After being melted at a temperature of 260°C, foreign matter was removed by a sintered filter with a cutoff of 80μm, and the molten monolayer polymer was discharged from the T-die. It was made to be closely fitted on a casting drum maintained at 90°C and cooled and solidified by an air knife to obtain an unstretched polypropylene film. The obtained unstretched polypropylene film was guided to a simultaneous biaxial stretching machine, and after preheating at 163°C while holding both ends of the film width with a clamp, it was simultaneously biaxially stretched at 3.6 times in the length direction and 8.2 times in the width direction. Next, it was guided to the outside of the simultaneous biaxial stretching machine without heat treatment and relaxation treatment, and the clamps at the ends of the film were released, and corona discharge treatment was performed in the same manner as in Example 1 to obtain a polypropylene film. The evaluation results are shown in Table 2-2.
[0290] (Comparative Examples 6 to 8)
[0291] Except that the raw material prescription was the raw material prescription of Table 2-1 and the film forming conditions were the film forming conditions described in Table 2-2, the same operation as in Example 1 was performed to obtain a 5.5 μm polypropylene film in Comparative Example 6, a 3.5 μm polypropylene film in Comparative Example 7, and a 4.5 μm polypropylene film in Comparative Example 8. However, the films could not be formed due to film breakage. Therefore, the film properties and capacitor properties could not be evaluated, and the column of this item in Table 2-2 is indicated by a diagonal line.
[0292] (Comparative Example 9)
[0293] A polypropylene film was obtained in the same manner as in Comparative Example 2 except that the raw material formulation was changed to that in Table 2-1 and the film forming conditions were changed to those described in Table 2-2. The evaluation results are shown in Table 2-2.
[0294] (Example C1)
[0295] The surface of the polypropylene film obtained in Example 2 that was subjected to corona discharge treatment was subjected to aluminum deposition with a film resistance of 20Ω / sq using a vacuum deposition machine manufactured by Albuque Co., Ltd. During the deposition, a deposition film C1A having a deposition pattern with a so-called T-shaped blank (a longitudinal pitch (period) of 17 mm and a fuse width of 0.5 mm) in which blank portions were provided in a direction perpendicular to the longitudinal direction by shielding oil, and a deposition film C1B having no deposition pattern with a T-shaped blank were produced. The above-mentioned deposition films C1A and C1B were cut separately to obtain deposition reels C1A and C1B with a film width of 50 mm (end blank width of 2 mm). Next, the capacitor element was processed using a component winding machine (KAW-4NHB) manufactured by Kaito Seisakusho Co., Ltd. in such a way that the vapor deposition reels C1A and C1B were alternately overlapped, and the capacitor element was wound in such a way that the component capacity after processing became 10μF. After metal spraying, a heat treatment was performed at a temperature of 128°C under reduced pressure for 12 hours, and the lead wire was installed to complete the processing as a capacitor element. The evaluation results of the obtained capacitor element are shown in Table 3. A capacitor element with a high rated voltage was obtained while keeping the element body particularly small.
[0296] (Example C2, Comparative Example C1, Comparative Example C2)
[0297] The film described in Table 3 was used, and otherwise, the capacitor element was obtained by the same operation as in Example C1. The capacitor element obtained in Example C2 is a capacitor element with a high rated voltage while keeping the element body in a small state. The capacitor element obtained in Comparative Example C1 has a high rated voltage but a large element body, which is a capacitor element with poor practical performance. The capacitor element obtained in Comparative Example C2 has a small element body but a low rated voltage, which is a capacitor element with poor practical performance.
[0298]
[0299]
[0300]
[0301]
[0302]
[0303] Industrial Availability
[0304] The polypropylene film of the present invention can be widely used in industrial applications such as film capacitors, packaging, demolding, and tapes. In particular, since the film has excellent voltage resistance and reliability in high temperature environments, it can be suitably used in film capacitors used under high temperature and high voltage.
[0305] Explanation of symbols
[0306] 1 Part of section X
[0307] 2 Sea part
[0308] 3. Island part (domain)
[0309] 4 A rectangle of 1 μm×2 μm in size determined so that a pair of short sides are parallel to the thickness direction in the cross section X; 5 A pair of short sides parallel to the thickness direction.
Claims
1. A polypropylene film, wherein when F(A23)+F(B23) is 120 MPa or more and 1000 MPa or less, the strength in the main orientation direction measured at 23°C is F(A23), and the strength in the direction orthogonal to the main orientation measured at 23°C is F(B23), and the shrinkage in the main orientation direction measured at 150°C is -2.0% or more and 3.0% or less, and the film comprises a cyclic olefin resin. 2 . The polypropylene film according to claim 1 , wherein a developed area ratio Sdr of at least one surface thereof is 0.002% or more and 0.050% or less.
3. The polypropylene film according to claim 1 or 2, comprising at least one layer (layer A) comprising the cyclic olefin resin and the polypropylene resin, When the cross section of the A layer cut along a plane parallel to the main orientation direction and the thickness direction is referred to as cross section X, in a rectangle of 1 μm×2 μm in size determined in the cross section X so that a pair of short sides are parallel to the thickness direction, there are two or more domains of the cyclic olefin-based resin passing through the pair of short sides. The polypropylene film according to any one of claims 1 to 3, wherein the dielectric breakdown voltage measured at 135°C exceeds 325 V / μm and is 900 V / μm or less. The polypropylene film according to any one of claims 1 to 4, which has a thickness of 0.50 μm to 5.5 μm. The polypropylene film according to any one of claims 1 to 5, wherein the shrinkage rate in a direction perpendicular to the main orientation of the film measured at 150°C is -2.0% to 4.0%. 7 . The polypropylene film according to claim 1 , comprising a cyclic olefin-based resin having a glass transition temperature of 125° C. or higher and 175° C. or lower. 8 . The polypropylene film according to claim 1 , which has a total light transmittance of 85% or more and 99.9% or less. 9 . The polypropylene film according to claim 1 , which has a temperature drop crystallization temperature Tmc measured by differential scanning calorimetry of 110° C. or higher. 10 . The polypropylene film according to claim 1 , wherein the thickness variation in the longitudinal direction is 0.001% or more and 15% or less. 11 . A metal film laminated film comprising a metal film on at least one surface of the polypropylene film according to claim 1 . 12 . A film capacitor using the metal film stacked film according to claim 11 .
13. The film capacitor according to claim 12, wherein the capacitance density is 1.1 μF / cm 3 Above and 18μF / cm 3 the following. 14 . The film capacitor according to claim 12 , wherein the withstand voltage at 135° C. is 0.60 kV or more. 15 . A power control unit comprising the film capacitor according to claim 12 .
16. An electric vehicle comprising the power control unit according to claim 15.
17. An electric aircraft comprising the power control unit according to claim 15.
18. A packaging material using the polypropylene film according to any one of claims 1 to 10.