Method for preparing separator (M) containing sulfonated polyarylene sulfone polymer (sP)

Through the preparation method of sulfonated polyarylene sulfone polymer separators used in fuel cells, electrolysis cells and electrodialysis cells, the high cost and performance deficiencies of existing PFSA separators are solved, and high-efficiency, low-swelling separators are achieved preparation, improving the performance of the separator.

CN118786169APending Publication Date: 2024-10-15BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023912.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-28
Filing Date
2023-02-23
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing sulfonic acid side chain fluorinated polymer (PFSA) separators have high cost, toxicity and persistence problems in production and use, and their performance in fuel cells, electrolytic cells and electrodialysis cells such as proton conductivity, swelling There is still room for improvement in mechanical stability.

Method used

A separator containing a sulfonated polyarylene sulfone polymer is prepared by a method comprising combining an aromatic dihalosulfone, an aromatic dihydroxy compound, a carbonate compound and an aprotic polar solvent in specific proportions and conditions. A polycondensation reaction is carried out to form a sulfonated polyarylene sulfone polymer, and through the removal of inorganic halides and the separation of solvents, a separator with good proton conductivity, low swelling and high tensile elongation is obtained.

Benefits of technology

It significantly reduces the preparation time of the sulfonated polyarylene sulfone polymer separator, avoids the use of a large amount of solvent and subsequent separation processes, and improves the performance of the separator, including proton conductivity, swelling and mechanical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012505840000151
    Figure BDA0005012505840000151
  • Figure BDA0005012505840000181
    Figure BDA0005012505840000181
  • Figure BDA0005012505840000191
    Figure BDA0005012505840000191
Patent Text Reader

Abstract

The invention relates to a method for preparing a separator (M) containing a sulfonated polyarylene sulfone polymer (sP), to the separator (M) obtained by the method according to the invention, to a fuel cell, to an electrodialysis cell and to an electrolytic cell comprising the separator (M), to the use of the separator (M) in an electrolytic cell, to an electrodialysis cell or to a fuel cell, and to a method for preparing electrical energy and / or hydrogen.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for preparing a membrane (M) containing a sulfonated polyarylene sulfone polymer (sP), the membrane (M) obtained by the method of the present invention, a fuel cell, an electrodialysis cell and an electrolysis cell comprising the membrane (M), the use of the membrane (M) in an electrolysis cell, an electrodialysis cell or a fuel cell, and a method for preparing electrical energy and / or hydrogen.

[0002] Politics, society and industry aim to reduce CO2 emissions by decarbonizing industry and transport. In this context, green hydrogen plays a strategic role as it can replace hydrocarbons for fuel cell propulsion in chemical and industrial processes, energy conversion and mobility applications. Renewable electricity can be used to operate electrolysis cells to produce green, sustainable hydrogen.

[0003] Key components in electrolysis cells, electrodialysis cells and fuel cells are so-called polymer electrolyte membranes (PEMs), which have to meet several requirements. They need to be ion-conducting and at the same time they have to separate hydrogen and oxygen. Furthermore, the membranes have to be robust and stable for long-term operation and lifetime with constant performance.

[0004] State-of-the-art membranes are mainly based on fluorinated polymers with sulfonic acid side chains (PFSA), which are marketed under the trade name Due to the complexity of PFSA production, these polymers are still quite expensive. In addition, the toxicity and persistence of fluorinated chemicals pose several challenges to the production, use and recycling of these materials. Therefore, science and industry try to develop more sustainable solutions to replace PFSA membranes.

[0005] One class of promising materials for these applications is polyarylene sulfone polymers. They belong to the group of high-performance polymers that have high thermal resistance, chemical resistance, excellent mechanical properties and durability (EM Koch, H.-M. Walter, Kunststoffe 80 (1990) 1146; E. Kunststoffe 80, (1990)1149, N.Inchaurondo-Nehm, Kunststoffe 98, (2008)190).

[0006] In addition to being used as engineering plastics, polyarylene sulfone polymers are also used as membrane materials for water treatment.

[0007] The polyarylene sulfone polymers can be formed, but are not limited to, by the hydroxide process, wherein a salt is first formed from a dihydroxy component and a hydroxide, or by the carbonate process.

[0008] General information on the formation of polyarylene sulfone polymers by the hydroxide process is found, inter alia, in RN Johnson et al., J. Polym. Sci. A-1 5 (1967) 2375, while the carbonate process is described in JEMcGrath et al., Polymer 25 (1984) 1827.

[0009] Processes for forming polyarylene sulfone polymers from aromatic dihalides and aromatic bisphenols or their salts in an aprotic solvent in the presence of one or more alkali metal or ammonium carbonates or bicarbonates are known to those skilled in the art and are described, for example, in EP-A 297 363 and EP-A 135 130.

[0010] High performance thermoplastics such as polyarylene sulfone polymers are formed by polycondensation reactions, which are typically carried out at high reaction temperatures in polar aprotic solvents such as DMF (dimethylformamide), DMAc (dimethylacetamide), sulfolane, DMSO (dimethylsulfoxide), and NMP (N-methylpyrrolidone).

[0011] In order to be used as a separator material in water electrolysis cells, electrodialysis cells or fuel cells, the polymer must exhibit ion conductivity, which can be achieved by functionalizing the polyarylene sulfone polymer with sulfonic acid groups.

[0012] Sulfonated polyarylene sulfone polymers have been known for decades. While direct sulfonation of polyarylene sulfone polymers leads to side reactions and allows only limited control over the degree of sulfonation, the use of disulfonated aromatic dihalosulfones such as sulfonated dichlorodiphenyl sulfone (sDCDPS) as comonomers allows the synthesis of well-defined sulfonated polyarylene sulfone polymers.

[0013] Although sulfonated polyarylene sulfone polymers show several interesting properties for use as ion-conducting membranes in fuel cells or electrolysis cells, there is still room for improvement of the sulfonated polyarylene sulfone membranes described in the prior art from the viewpoint of proton conductivity, swelling and mechanical stability.

[0014] It is therefore an object of the present invention to provide a process for preparing a membrane (M) containing a sulfonated polyarylene sulfone polymer (sP) which does not retain the disadvantages of the prior art or only retains them in a weakened form. The process should be easy to implement. The membrane (M) containing the sulfonated polyarylene sulfone polymer (sP) should be suitable for electrolysis cells and fuel cells. In addition, the membrane (M) should be suitable for separating hydrogen from a hydrogen-containing gas mixture.

[0015] This object is achieved by a method for preparing a membrane (M) containing a sulfonated polyarylene sulfone polymer (sP), the method comprising the following steps

[0016] i) Conversion reaction mixture (R G ), the reaction mixture comprising

[0017] An aromatic dihalogenated sulfone component (component (A)), the aromatic dihalogenated sulfone component comprising

[0018] at least one sulfonated aromatic dihalosulfone (component (A1)) and at least one non-sulfonated aromatic dihalosulfone (component (A2)),

[0019] at least one aromatic dihydroxy compound (component (B)),

[0020] at least one carbonate compound (component (C)), and

[0021] at least one aprotic polar solvent (component (D)),

[0022] To obtain a product mixture (P) comprising the sulfonated polyarylene sulfone polymer (sP), the at least one aprotic polar solvent and the at least one inorganic halide compound G ),

[0023] ii) from the product mixture (P G ) to obtain a solution (S) comprising the sulfonated polyarylene sulfone polymer (sP) and the at least one aprotic polar solvent

[0024] iii) separating the at least one aprotic polar solvent from the solution (S) to obtain a membrane (M) containing the sulfonated polyarylene sulfone polymer (sP).

[0025] Surprisingly, it has been found that by the process of the invention, a membrane (M) is obtained which exhibits good proton conductivity, low swelling and high tensile elongation. By the process of the invention, the preparation time of a membrane (M) containing a sulfonated polyarylene sulfone polymer (sP) can be significantly reduced. The condensation according to step i) produces a polymer suspension containing a sulfonated polyarylene sulfone polymer (sP) and an inorganic halide salt. After separation of the salt, in the prior art, precipitation is usually carried out in isopropanol to separate the sulfonated polyarylene sulfone polymer (sP), which results in large amounts of solvent mixture having to be reprocessed or disposed of.

[0026] Furthermore, a portion of the product is not completely precipitated and can lead to clogging of the filter during the subsequent separation. Furthermore, the sulfonated copolymer must be dissolved again in order to produce the membrane (M). The process according to the invention prevents the production of large amounts of solvent mixtures and avoids separation prior to membrane preparation.

[0027] The present invention will be described in more detail below.

[0028] method

[0029] The process according to the invention for preparing a membrane (M) comprising a sulfonated polyarylene sulfone polymer (sP) comprises steps i), ii) and iii).

[0030] Step i)

[0031] In step i) according to the present invention, a reaction mixture (R) comprising an aromatic dihalosulfone component, at least one aromatic dihydroxy compound, at least one carbonate compound and at least one aprotic polar solvent is converted. G ) to obtain a product mixture (P) comprising a sulfonated polyarylene sulfone polymer (sP), the at least one aprotic polar solvent and at least one inorganic halide G ).

[0032] The aromatic dihalogenated sulfone component is also referred to as component (A). The terms aromatic dihalogenated sulfone component and component (A) in the present invention are used synonymously and thus have the same meaning.

[0033] The at least one aromatic dihydroxy compound is also referred to as component (B). The terms at least one aromatic dihydroxy compound and component (B) in the present invention are used synonymously and thus have the same meaning.

[0034] The at least one carbonate compound is also referred to as component (C). The terms at least one carbonate compound and component (C) in the present invention are used synonymously and therefore have the same meaning.

[0035] The at least one aprotic polar solvent is also referred to as component (D). The terms at least one aprotic polar solvent and component (D) in the present invention are used synonymously and therefore have the same meaning.

[0036] Reaction mixture (R G ) is provided in step i) for forming a product mixture (P G ) in a mixture of sulfonated polyarylene sulfone polymer (sP). G ) refers to the mixture present before the conversion, ie the polycondensation, according to step i).

[0037] By polycondensation of components (A) and (B), polycondensation occurs to convert the reaction mixture (R G ) into a production mixture (P) comprising a sulfonated polyarylene sulfone polymer (sP) G ).

[0038] In step i), components (A) and (B) enter into a polycondensation reaction. Component (C) acts as a base to deprotonate the hydroxyl groups of component (B). Component (D) serves as a solvent.

[0039] The product mixture (P) obtained after the polycondensation according to step i) G ) comprises a sulfonated polyarylene sulfone polymer (sP). The product mixture (P G ) further comprises the at least one inorganic halide compound and the at least one aprotic polar solvent (component (D)). G ). During the conversion, component (C) reacts with component (B) to deprotonate component (B). The deprotonated component (B) then reacts with component (A) to form at least one inorganic halide compound. This method is known to those skilled in the art.

[0040] Reaction mixture (R G ) are preferably reacted simultaneously. The components can be mixed in an upstream step and then reacted. It is also possible to feed the components into a reactor, where they are mixed and then reacted.

[0041] In step i) of the process according to the invention, the reaction mixture (R G ) are preferably reacted simultaneously. The reaction is preferably carried out in one stage. This means that the deprotonation of component (B) and the condensation reaction between components (A) and (B) are preferably carried out in a single reaction stage without isolating intermediate products, such as the deprotonated material of component (B).

[0042] Furthermore, it is preferred that the reaction mixture (R) provided in step i) G ) does not include toluene or monochlorobenzene. In particular, it is preferred that the reaction mixture (R G ) does not include any substance that forms an azeotrope with water. The same applies to the product mixture (P G ).

[0043] The ratio of component (A) and component (B) in step i) results in principle from the stoichiometry of the polycondensation reaction which is carried out theoretically with elimination of hydrogen halide, preferably hydrogen chloride, and is established in a known manner by the person skilled in the art.

[0044] Preferably, in step i), the ratio of halogen end groups derived from component (A) to phenolic end groups derived from component (B) is adjusted by controlled establishment of an excess of component (A) relative to component (B) as starting compound.

[0045] More preferably, in step i), the molar ratio of component (A) to component (B) is from 0.95 to 1.08, especially from 0.98 to 1.06, most preferably from 0.985 to 1.05.

[0046] Preferably, the conversion in the polycondensation reaction in step i) is at least 0.9.

[0047] The polycondensation reaction in step i) is usually carried out at a temperature in the range of 80° C. to 250° C., preferably in the range of 100° C. to 220° C. The upper limit of the temperature is preferably determined by the boiling point of the at least one aprotic polar solvent (component (D)) at standard pressure (1013.25 mbar). The reaction is usually carried out at standard pressure. The reaction is preferably carried out within a time interval in the range of 0.5 hour to 14 hours, in particular 1 hour to 12 hours.

[0048] In a preferred embodiment, in step i), the reaction mixture (R G ), the reaction mixture comprising

[0049] Based on the reaction mixture (R G ) in the total molar amount of the aromatic dihalosulfone component (component A),

[0050] X mol of an aromatic dihalogenated sulfone component (component A)),

[0051] X 1 mol.-% of at least one sulfonated aromatic dihalosulfone (component (A1)), and

[0052] X 2 mol.-% of at least one non-sulfonated aromatic dihalosulfone (component (A2)), wherein

[0053] X 1 In the range of 20 to 70, and

[0054] X 2 In the range of 30 to 80,

[0055] Y mol of at least one aromatic dihydroxy compound (component (B))

[0056] Z mol of at least one carbonate compound (component (C)),

[0057] in

[0058] The ratio of X to Y is in the range of 0.95 to 1.08,

[0059] And among them

[0060] Z is in the range of P to Q,

[0061] Where P is calculated according to the following formula:

[0062] P=Y*(1.05+X 1 / 100*1.05),

[0063] And where Q is calculated according to the following formula:

[0064] Q=Y*(1.05+X 1 / 100*1.4).

[0065] In a preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) obtained in step i) is not removed from the product mixture (P G ) are separated.

[0066] In one embodiment, between step i) and step ii), no further process steps are carried out. In another embodiment, before or during step ii), at least one additional component (FC) may be added to the product mixture (P G In another preferred embodiment, before carrying out step ii), the product mixture (P G ) in which the sulfonated polyarylene sulfone polymer (sP) remains in dissolved form.

[0067] Step ii)

[0068] In step ii), the inorganic halide compound formed during the condensation reaction in step i) is removed from the product mixture (P G ) is removed. A solution (S) comprising the sulfonated polyarylene sulfone polymer (sP) and component (D) is obtained.

[0069] The inorganic halide compounds can be removed by means known in the art, such as filtration, centrifugation, decantation, and the like.

[0070] Therefore, the present invention also provides a method, wherein the method comprises the following steps

[0071] ii) filtering, centrifuging and / or decanting the product mixture (P) obtained in step i) G ) to obtain a solution (S).

[0072] In a preferred embodiment, the solution (S) obtained in step ii) does not contain solid inorganic halide compounds. In another preferred embodiment, the solution (S) obtained in step ii) contains less than 3 wt%, more preferably less than 1.5 wt%, and particularly preferably less than 0.5 wt% of inorganic halide components based on the total weight of the solution (S) obtained in step ii).

[0073] In a more preferred embodiment, the solution (S) obtained in step ii) comprises no solid inorganic compounds.

[0074] In another preferred embodiment, the solution (S) obtained in step ii) contains less than 0.4 wt%, more preferably less than 0.3 wt%, and particularly preferably less than 0.2 wt% of inorganic components, based on the total weight of the solution (S) obtained in step ii).

[0075] In a preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) in step ii) is not isolated from the solution (S).

[0076] In one embodiment, between step ii) and step iii), no further process steps are carried out. In a preferred embodiment, at least one further component (FC) is added to the solution (S) before step iii).

[0077] In another preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) in the solution (S) in step ii) remains in dissolved form before being subjected to step iii).

[0078] In a particularly preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) in the process according to the invention remains dissolved until step iii) is carried out.

[0079] In another particularly preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) is not isolated before carrying out step iii). In other words, the process according to the invention preferably comprises only one isolation step (step iii)) of the sulfonated polyarylene sulfone polymer (sP), in which the membrane (M) is formed.

[0080] Step iii)

[0081] In step iii), the at least one aprotic polar solvent is separated from the solution (S) to obtain the membrane (M). In a preferred embodiment, the solution (S) is degassed before performing step iii).

[0082] The separation of the at least one aprotic polar solvent from the solution (S) in step iii) can be carried out by any method known to the skilled person which is suitable for separating solvents from polymers.

[0083] Preferably, separation of the at least one aprotic polar solvent from the solution (S) in step iii) is performed via a phase inversion method.

[0084] In the context of the present invention, a phase inversion process is understood to mean a process in which a dissolved sulfonated polyarylene sulfone polymer (sP) is converted into a solid phase. Thus, a phase inversion process can also be indicated as a precipitation process. According to step iii), the conversion is carried out by separating the at least one aprotic polar solvent from the sulfonated polyarylene sulfone polymer (sP). Suitable phase inversion processes are known to the person skilled in the art.

[0085] The phase inversion method can be carried out, for example, by cooling the solution (S). During this cooling, the sulfonated polyarylene sulfone polymer (sP) contained in the solution (S) precipitates. Another possibility for carrying out the phase inversion method is to contact the solution (S) with a protic polar liquid, which is a non-solvent for the sulfonated polyarylene sulfone polymer (sP). The sulfonated polyarylene sulfone polymer (sP) will then also precipitate. Suitable protic polar solvents as non-solvents for the sulfonated polyarylene sulfone polymer (sP) are, for example, the protic polar solvents in liquid form described below. Another phase inversion method that is preferred in the context of the present invention is a phase inversion carried out by immersing the solution (S) in at least one protic polar solvent.

[0086] Thus, in one embodiment, in step iii), the at least one aprotic polar solvent comprised in the solution (S) is separated from the sulfonated polyarylene sulfone polymer (sP) comprised in the solution (S) by immersing the solution (S) in at least one protic polar solvent.

[0087] This means that the membrane (M) in step iii) is formed by immersing the solution (S) in at least one protic polar solvent.

[0088] Suitable at least one protic polar solvent is known to the skilled person. Preferred at least one protic polar solvent is water, methanol, ethanol, n-propanol, isopropanol, glycerol, ethylene glycol and mixtures thereof.

[0089] Therefore, in a preferred embodiment, step iii) comprises the following steps:

[0090] iii-1) casting the solution (S) provided in step ii) to obtain a film of the solution (S),

[0091] iii-2) separating the at least one aprotic polar solvent from the membrane of the solution (S) obtained in step iii-1) to obtain a membrane (M) in the form of a membrane.

[0092] The separation in step iii-2) can be carried out as described above. Preferably, the separation in step iiii-2) is carried out by evaporating the at least one aprotic polar solvent from a membrane of solution (S).

[0093] Therefore, in a particularly preferred embodiment, step iii) comprises the following steps:

[0094] iii-1) casting the solution (S) provided in step ii) to obtain a film of the solution (S),

[0095] iii-2) evaporating the at least one aprotic polar solvent from the film of the solution (S) obtained in step iii-1) to obtain the separator (M) in the form of a membrane.

[0096] This means that the membrane (M) is formed by evaporating the at least one aprotic polar solvent from a film of the solution (S).

[0097] In step iii-1), the solution (S) can be cast by any method known to the skilled person. Typically, the solution (S) is cast with a casting knife, a comet bar, a Meyer bar, a slot die or a reverse roll preferably heated to a temperature in the range of 20°C-150°C, preferably in the range of 40°C-100°C, more preferably between 60°C and 85°C.

[0098] In step iii-1), the solution (S) is generally cast on a substrate (support material) which does not react with the sulfonated polyarylene sulfone polymer (sP) and / or the at least one solvent comprised in the solution (S).

[0099] Suitable substrates (carrier materials) are, for example, steel belts, drying cylinders or polymer films. The substrate (carrier material) is usually not part of the finished membrane (M), but is only used for processing purposes.

[0100] The solution (S) may also be cast on a porous support layer which becomes part of the membrane (M).

[0101] After step iii), the membrane can be further processed. The membrane can, for example, be coated with a stabilizer or a catalyst.

[0102] Suitable stabilizers are, for example, cerium dioxide, cerium-containing complexes or titanium dioxide.

[0103] Suitable catalysts are selected, for example, from the group consisting of platinum, iridium, ruthenium or palladium in elemental form or in the form of their oxides, mixtures or alloys, as powder or deposited on a catalyst support such as SnO2, carbon or TiO2.

[0104] To prepare a catalyst coated membrane (CCM), the catalyst can be dispersed in a medium containing water, alcohol and other solvents along with a binder. The binder can be a proton conducting polymer such as Nafion, sulfonated polyarylether, sulfonated polystyrene copolymer. The dispersion is then coated on the membrane by common coating techniques (slot die coating, doctor blade coating, spray coating).

[0105] Component (A)

[0106] Component (A), also referred to as the aromatic dihalosulfone component, comprises at least one sulfonated aromatic dihalosulfone and at least one non-sulfonated aromatic dihalosulfone.

[0107] The at least one sulfonated aromatic dihalosulfone is also referred to as component (A1). The terms at least one sulfonated aromatic dihalosulfone and component (A1) are used synonymously in the present invention and therefore have the same meaning.

[0108] The at least one non-sulfonated aromatic dihalosulfone is also referred to as component (A2). The terms at least one non-sulfonated aromatic dihalosulfone and component (A2) in the present invention are used synonymously and therefore have the same meaning.

[0109] "At least one sulfonated aromatic dihalosulfone" as meant herein is precisely one sulfonated aromatic dihalosulfone, as well as a mixture of two or more sulfonated aromatic dihalosulfones. Preferably, precisely one sulfonated aromatic dihalosulfone is used.

[0110] "At least one non-sulfonated aromatic dihalosulfone" as meant herein is exactly one non-sulfonated aromatic dihalosulfone, as well as a mixture of two or more non-sulfonated aromatic dihalosulfones. Preferably exactly one non-sulfonated aromatic dihalosulfone is used.

[0111] In the above preferred embodiments, "X" preferably represents the reaction mixture (R G ) in the reaction mixture (R G ) in the total molar amount of the aromatic dihalosulfone component (component (A)). In other words, "X" preferably represents the total molar amount of the aromatic dihalosulfone component (component (A)) contained in the component (A) (preferably contained in the reaction mixture (R G The sum of the molar amounts of component (A1) and component (A2) in the reaction mixture (R G ) in the total molar amount of component (A), "X 1 " means in this context the molar amount in mol.-% of component (A1), and "X 2 " means here the molar amount in mol.-% of component (A2).

[0112] X 1 The amount of the solvent may be in the range of 20 mol.-% to 70 mol.-%, preferably in the range of 27.5 mol.-% to 65 mol.-%, more preferably in the range of 30 mol.-% to 60 mol.-%, and most preferably in the range of 32.5 mol.-% to 57.5 mol.-%, in each case based on the reaction mixture (R G) is the total molar amount of the aromatic dihalosulfone component (component (A)).

[0113] X 2 The content of the esters may be in the range of 30 mol.-% to 80 mol.-%, preferably in the range of 35 mol.-% to 72.5 mol.-%, more preferably in the range of 40 mol.-% to 70 mol.-%, and most preferably in the range of 42.5 mol.-% to 67.5 mol.-%, in each case based on the reaction mixture (R G ) is the total molar amount of the aromatic dihalosulfone component (component (A)).

[0114] X 1 and X 2 The amounts generally add up to 100 mol.-%.

[0115] Component (A1)

[0116] Component (A1), also known as sulfonated aromatic dihalosulfone, preferably comprises at least one -SO3X 3 Group.

[0117] Component (A1) preferably contains at least one -SO3X 3 Group. As used herein, "at least one -SO3X 3 The component (A1) may contain exactly one -SO3X 3 group and two or more -SO3X 3 More preferably, component (A1) contains two -SO3X 3 Group.

[0118] General formula - SO3X 3 Contains sulfonic acid functional groups and derivatives of sulfonic acid functional groups such as sulfonates. 3 In the group, X 3 This may be hydrogen and / or a cation equivalent.

[0119] In the context of the present invention, "a cation equivalent" refers to a cation of a single positive charge or a charge equivalent of a cation having two or more positive charges, such as Li, Na, K, Mg, Ca, NH4, preferably Na, K. Particularly preferred are Na or K.

[0120] Component (A1) is preferably selected from the group consisting of 4,4'-dichlorodiphenylsulfone-3,3'-disulfonic acid and 4,4'-difluorodiphenylsulfone-3,3'-disulfonic acid and derivatives thereof.

[0121] In the context of the present invention, the terms "sulfonic acid" and "-SO3X 3The term "sulfonic acid" in 4,4'-dichlorodiphenylsulfone-3,3'-disulfonic acid and 4,4'-difluorodiphenylsulfone-3,3'-disulfonic acid means "-SO3X 3 Group", where X 3 is the hydrogen or cation equivalent.

[0122] In one embodiment, component (A1) preferably comprises -SO3X having a cationic equivalent 3 Particularly preferably, component (A1) is selected from the group consisting of 4,4′-dichlorodiphenyl sulfone-3,3′-disulfonic acid, 4,4′-dichlorodiphenyl sulfone-3,3′-disulfonic acid disodium salt, 4,4′-dichlorodiphenyl sulfone-3,3′-disulfonic acid dipotassium salt, 4,4′-difluorodiphenyl sulfone-3,3′-disulfonic acid, 4,4′-difluorodiphenyl sulfone-3,3′-disulfonic acid disodium salt and 4,4′-difluorodiphenyl sulfone-3,3′-disulfonic acid dipotassium salt.

[0123] Another object of the present invention is therefore a process, wherein component (A1) comprises at least one compound selected from the group consisting of 4,4′-dichlorodiphenyl sulfone-3,3′-disulfonic acid, 4,4′-dichloro-diphenyl sulfone-3,3′-disulfonic acid disodium salt, 4,4′-dichlorodiphenyl sulfone-3,3′-disulfonic acid dipotassium salt, 4,4′-difluorodiphenyl sulfone-3,3′-disulfonic acid, 4,4′-difluoro-diphenyl sulfone-3,3′-disulfonic acid disodium salt and 4,4′-difluorodiphenyl sulfone-3,3′-disulfonic acid dipotassium salt.

[0124] In one embodiment, component (A1) comprises a mixture based on the reaction mixture (R G ) in the total weight of component (A1), not less than 70wt%, preferably not less than 90wt%, and more preferably not less than 98wt% of at least one aromatic dihalogenated sulfone component, the aromatic dihalogenated sulfone component comprising at least one -SO3X selected from the group consisting of 3 Groups: 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid disodium salt and 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt.

[0125] In another particularly preferred embodiment, component (A1) consists of at least one aromatic dihalosulfone comprising at least one -SO3X selected from the group consisting of 3Groups: 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid, 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid disodium salt and 4,4'-difluorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt.

[0126] In these embodiments, 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt and 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid disodium salt are particularly preferably used as component (A1).

[0127] In another particularly preferred embodiment, component (A1) consists of 4,4'-dichlorodiphenyl sulfone-3,3'-disulfonic acid dipotassium salt or 4,4'-dichloro-diphenyl sulfone-3,3'-disulfonic acid disodium salt.

[0128] Component (A2)

[0129] Component (A2), also referred to as the non-sulfonated aromatic dihalosulfone component, preferably does not contain -SO3X 3 Group.

[0130] Preferably, component (A2) comprises a mixture based on the reaction mixture (R G ) in the total weight of component (A2), not less than 80 wt%, preferably not less than 90 wt% and more preferably not less than 98 wt% of at least one aromatic dihalosulfone selected from the group consisting of 4,4′-dichlorodiphenyl sulfone and 4,4′-difluorodiphenyl sulfone. The weight percentages for component (A2) here also relate to the sum of the used 4,4′-dichlorodiphenyl sulfone and the used 4,4′-difluorodiphenyl sulfone.

[0131] Therefore, another object of the present invention is a process in which component (A2) comprises a mixture based on the reaction mixture (R G ) in the total weight of component (A2), not less than 80 wt% of at least one aromatic dihalogenated sulfone selected from the group consisting of 4,4'-dichlorodiphenyl sulfone and 4,4'-difluoro-diphenyl sulfone.

[0132] In another particularly preferred embodiment, component (A2) consists of at least one aromatic dihalosulfone selected from the group consisting of 4,4'-dichlorodiphenyl-sulfone and 4,4'-difluorodiphenyl sulfone.

[0133] In these embodiments, 4,4'-dichlorodiphenyl sulfone is particularly preferably used as component (A2).

[0134] In a further particularly preferred embodiment, component (A2) consists of 4,4'-dichlorodiphenyl sulfone.

[0135] Preferably, component (A2) is selected from the group consisting of 4,4'-dichlorodiphenyl sulfone and 4,4'-difluorodiphenyl sulfone.

[0136] Component (B)

[0137] Component (B), also referred to as aromatic dihydroxy compounds, generally comprises two hydroxyl groups.

[0138] The "at least one aromatic dihydroxy compound" referred to herein is specifically one aromatic dihydroxy compound, as well as a mixture of two or more aromatic dihydroxy compounds. Preferably, specifically one aromatic dihydroxy compound is used.

[0139] In the above preferred embodiments, "Y" preferably means the reaction mixture (R G ) in the reaction mixture (R G ) is the total molar amount of the aromatic dihydroxy compound (component (B)).

[0140] Preferably, component (B) is selected from the group consisting of 4,4′-dihydroxybiphenyl, 4,4′-dihydroxydiphenyl sulfone, bisphenol A (2,2-bis(4-hydroxyphenyl)propane), 4,4′-dihydroxybenzophenone and hydroquinone. Among the above aromatic dihydroxy components, 4,4′-dihydroxybiphenyl, 4,4′-dihydroxydiphenyl sulfone and bisphenol A are preferred, and 4,4′-dihydroxybiphenyl is particularly preferred.

[0141] Therefore, the present invention also provides a process, wherein component (B) is selected from the group consisting of 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl sulfone, bisphenol A, 4,4'-dihydroxybenzophenone and hydroquinone.

[0142] Preferably, component (B) comprises a mixture based on the reaction mixture (R G ) in an amount of not less than 80 wt%, preferably not less than 90 wt%, and more preferably not less than 98 wt% of 4,4′-dihydroxybiphenyl.

[0143] Therefore, another object of the present invention is a process in which component (B) comprises a mixture based on the reaction mixture (R G ) in the total weight of component (B), is not less than 80wt% of 4,4′-dihydroxybiphenyl.

[0144] The percentages by weight for component (B) here further relate to the sum of the 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl sulfone, bisphenol A (2,2-bis-(4-hydroxyphenyl)propane), 4,4'-dihydroxybenzophenone and hydroquinone used.

[0145] In another particularly preferred embodiment, component (B) consists of at least one aromatic dihydroxy component selected from the group consisting of 4,4′-dihydroxybiphenyl, 4,4′-dihydroxydiphenyl sulfone, bisphenol A (2,2-bis(4-hydroxy-phenyl)propane), 4,4′-dihydroxybenzophenone and hydroquinone.

[0146] In these embodiments, 4,4'-dihydroxybiphenyl, bisphenol A, and 4,4'-dihydroxydiphenyl sulfone are particularly preferably used as component (B), with 4,4'-dihydroxybiphenyl being most preferred.

[0147] Component (C)

[0148] Reaction mixture (R G ) comprises at least one carbonate compound as component (C). In this case, the term "at least one carbonate compound" is understood to mean exactly one carbonate compound, and also a mixture of two or more carbonate compounds. The at least one carbonate compound is preferably at least one metal carbonate. The metal carbonate is preferably anhydrous. In this case, the terms "at least one carbonate compound" and "component (C)" are used synonymously and therefore have the same meaning.

[0149] Alkali metal carbonates and / or alkaline earth metal carbonates are preferred as metal carbonates. At least one metal carbonate selected from the group consisting of sodium carbonate, potassium carbonate and calcium carbonate is particularly preferred as metal carbonate. Potassium carbonate is most preferred.

[0150] For example, component (C) comprises a mixture based on the reaction mixture (R G ) in an amount of not less than 50 wt %, more preferably not less than 70 wt %, and most preferably not less than 90 wt % of potassium carbonate.

[0151] Therefore, another object of the present invention is a process in which component (C) comprises a mixture based on the reaction mixture (R G ) in the total weight of component (C), not less than 50wt% of potassium carbonate.

[0152] In a preferred embodiment, component (C) consists of potassium carbonate. Potassium carbonate with a volume weighted average particle size of less than 200 μm is preferred, more preferably less than 100 μm, even more preferably less than 70 μm, and most preferably less than 50 μm. The volume weighted average particle size of potassium carbonate is determined using a particle size analyzer in a suspension of potassium carbonate in a mixture of chlorobenzene / sulfolane (60 / 40 by weight).

[0153] In the above preferred embodiments, "Z" preferably means the reaction mixture (R G ) in the reaction mixture (R G ) in the total molar amount of at least one carbonate component (component (C)).

[0154] Z is in the range of P to Q.

[0155] "P" is calculated according to the following formula:

[0156] P=Y*(1.05+X 1 / 100*1.05)

[0157] "Q" is calculated according to the following formula:

[0158] Q=Y*(1.05+X 1 / 100*1.4)

[0159] In this formula, Y is the reaction mixture (R G ) in the molar amount of component (B), and X 1 Also the reaction mixture (R G ) in mol.-% value of component (A1).

[0160] Component (D)

[0161] Reaction mixture (R G ) preferably comprises at least one aprotic polar solvent as component (D). According to the invention, "at least one aprotic polar solvent" is understood to mean exactly one aprotic polar solvent and also mixtures of two or more aprotic polar solvents. In this case, the terms "at least one aprotic polar solvent" and "component (D)" are used synonymously and therefore have the same meaning.

[0162] Suitable aprotic polar solvents are, for example, selected from the group consisting of anisole, dimethylformamide, dimethyl sulfoxide, sulfolane, N-methylpyrrolidone, N-ethylpyrrolidone and N-dimethylacetamide.

[0163] Preferably, component (D) is selected from the group consisting of N-methylpyrrolidone, N-dimethylacetamide, dimethyl sulfoxide and dimethylformamide. N-methylpyrrolidone is particularly preferred as component (D).

[0164] Preferably, component (D) comprises a mixture based on the reaction mixture (R G ) in the total weight of component (D), not less than 50 wt%, preferably not less than 70 wt% and more preferably not less than 90 wt% of at least one solvent selected from the group consisting of N-methylpyrrolidone, N-dimethylacetamide, dimethyl sulfoxide and dimethylformamide. N-methylpyrrolidone is particularly preferred as component (D).

[0165] Another object of the present invention is therefore a process in which component (D) comprises a mixture based on the reaction mixture (R G ) in the total weight of component (D), not less than 50wt% of at least one solvent selected from the group consisting of N-methylpyrrolidone, N-dimethylacetamide, dimethyl sulfoxide and dimethyl-formamide.

[0166] In a preferred embodiment, component (D) consists of N-methylpyrrolidone, which is also known as NMP or N-methyl-2-pyrrolidone.

[0167] Additional components (FC)

[0168] In a preferred embodiment, the membrane (M) comprises at least one further component as component (FC). According to the invention, "at least one further component" is understood to mean exactly one further component and also mixtures of two or more further components. In this case, the terms "at least one further component" and "component (FC)" are used synonymously and therefore have the same meaning.

[0169] In a preferred embodiment, component (FC) is added in the process according to the invention before or during step iii), preferably before carrying out step iii). In another preferred embodiment, component (FC) is added to the solution (S) obtained in step ii) before carrying out step iii).

[0170] Component (FC) is preferably at least one component selected from the group consisting of a stabilizer and a hydrophilic polymer.

[0171] Preferred as component (FC) are components which are soluble in component (D), the at least one aprotic organic solvent.

[0172] Suitable stabilizers are, for example, heat stabilizers, antioxidant stabilizers or organic free-radical scavengers.

[0173] As suitable stabilizers, sterically hindered phenols, phosphites or quinones may be used. A suitable free radical scavenger is, for example, (4-hydroxy-2,2,6,6-tetramethylpiperidin-1-yl)oxy (TEMPO).

[0174] More details on suitable additives can be found in: P. Gijsman, “Polymer Stabilisation” in Handbook of Environmental Degradation of materials, 3rd edition, William Andrew, 2018.

[0175] Suitable hydrophilic polymers are, for example, polyvinylpyrrolidone (PVP), polyethylene oxide, polyethylene oxide-polypropylene oxide copolymers.

[0176] Membrane (M) containing sulfonated polyarylene sulfone polymer (sP)

[0177] Another object of the present invention is a membrane (M) comprising the sulfonated polyarylene sulfone polymer (sP) obtainable by the process of the present invention.

[0178] The sulfonated polyarylene sulfone polymer (sP) obtained in step i) of the process according to the invention for preparing a membrane (M) preferably comprises repeating units of the general formula I:

[0179]

[0180] in

[0181] t and q: each independently 0, 1, 2 or 3,

[0182] Q 1 , T and Y 1 : Each independently is a chemical bond or is selected from -O-, -S-, -SO2-, -S(=O)-, -C(=O)-, -N=N- and -CR a R b , where R a and R b are independently a hydrogen atom or a C1-C 12 -alkyl, C1-C 12 -alkoxy or C6-C 18 -aryl group, and wherein at least one of Q, T and Y is -SO2-,

[0183] Ar and Ar 1 : Each independently is C6-C 18 Aryl, wherein the C6-C 18 Aryl is unsubstituted or selected from C1-C 12 Alkyl, C1-C12 Alkoxy, C6-C 18 is substituted with at least one substituent selected from aryl, halogen and -SO3X,

[0184] p, m, n and k: each independently 0, 1, 2, 3 or 4, provided that the sum of p, m, n and k is not less than 1, and

[0185] X 3 : is hydrogen or a cation equivalent.

[0186] Therefore, another object of the present invention is a membrane (M) comprising a sulfonated polyarylene sulfone polymer (sP), wherein the sulfonated polyarylene sulfone polymer (sP) comprises recurring units of the general formula (I) as defined above.

[0187] In a preferred embodiment, the sulfonated polyarylene sulfone polymer (sP) comprised in the membrane (M) comprises at least 80 mol.-% of repeating units of the general formula (I), based on the total molar amount of the sulfonated polyarylene sulfone polymer (sP) comprised in the membrane (M).

[0188] If Q with the above prerequisites 1 , T or Y 1 is a chemical bond, which means that the adjacent groups on the left-hand side and the adjacent groups on the right-hand side are directly connected to each other by a chemical bond.

[0189] R a and R b are independently hydrogen or C1-C 12 alkyl.

[0190] Preferred C1-C 12 Alkyl groups include straight and branched saturated alkyl groups of 1 to 12 carbon atoms. The following parts are particularly suitable: C1-C6-alkyl, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, 2- or 3-methylpentyl, or relatively long chain parts, such as unbranched heptyl, octyl, nonyl, decyl, undecyl, lauryl and their branched analogs.

[0191] C1-C used 12 The alkyl moiety in the alkoxy group includes the alkyl groups of 1 to 12 carbon atoms as defined above. The cycloalkyl moieties preferably used include in particular C3-C 12 Cycloalkyl moieties such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclopropylmethyl, cyclopropylethyl, cyclopropylpropyl, cyclobutylmethyl, cyclobutylethyl, cyclopentylethyl, -propyl, -butyl, -pentyl, -hexyl, -cyclohexylmethyl, -dimethyl, -trimethyl.

[0192] Ar and Ar1 Each independently is C6-C 18 Aryl. Ar is preferably derived from an electron-rich aromatic substance that is very susceptible to electrophilic attack, preferably selected from the group consisting of sulfonated or unsulfonated hydroquinone, resorcinol, dihydroxynaphthalene (especially 2,7-dihydroxynaphthalene). Preferably, Ar 1 is unsubstituted C6 or C 12 Arylene group.

[0193] In a preferred embodiment of formula (I), Ar and Ar 1 Each is preferably independently selected from the group consisting of sulfonated or unsulfonated 1,4-phenylene, 1,3-phenylene, naphthylene, in particular 2,7-dihydroxynaphthalene and 4,4'-biphenylene.

[0194] Preferred are membranes (M) containing sulfonated polyarylene sulfone polymers (sP) having one or more of the following structural units (Ia) to (Io):

[0195]

[0196]

[0197] in

[0198] 1, k, m, n, o, p are each independently 0, 1, 2, 3 or 4, provided that the sum of l, k, m, n, o and p is ≥ 1, and

[0199] X 3 is hydrogen or a cation equivalent.

[0200] In the context of the present invention, "one cation equivalent" refers to a charge equivalent of a single positively charged cation or a cation with two or more positive charges, such as Li, Na, K, Mg, Ca, NH4, preferably Na, K.

[0201] Besides the preferred building blocks (Ia) to (Io), preference is also given to those structural units in which one or more sulfonated or unsulfonated 1,4-dihydroxyphenyl units are replaced by resorcinol or dihydroxynaphthalene.

[0202] Copolymers constructed from various combinations of structural units or sulfonated and non-sulfonated structural units may also be used.

[0203] Particular preference is given to using the structural units (Ia), (Ib), (Ig) and (Ik) or copolymers thereof as repeating units of the general formula (I).

[0204] In a particularly preferred embodiment, Ar is 1,4-phenylene, t is 1, T is a chemical bond, and Y1 is -SO2-, q is 0, p is 0, m is 0, n is 1 and k is 1. Sulfonated polyphenylene sulfone constructed from this enumerated structural repeating unit is represented as sPPSU.

[0205] In a particularly preferred embodiment, Ar is 1,4-phenylene, t is 0, Y is -SO2-, q is 0, n is 0 and k is 0. Polyarylene sulfones constructed from this enumerated structural repeat unit are known as sulfonated polyetherethersulfones (sPEES).

[0206] In an advantageous embodiment, the membrane (M) contains a sulfonated polyarylene sulfone polymer (sP) comprising

[0207] The non-sulfonated repeating unit of formula (1)

[0208]

[0209] and the sulfonated repeating unit of formula (2)

[0210]

[0211] In particular, the sulfonated polyarylene sulfone polymer (sP) contained in the membrane (M) consists only of non-sulfonated repeating units of formula (1) and sulfonated repeating units of formula (2).

[0212] In a very advantageous embodiment, the sulfonated polyarylene sulfone polymer (sP) contained in the membrane comprises

[0213] The non-sulfonated repeating unit of formula (1a)

[0214]

[0215] and the sulfonated repeating unit of formula (2a)

[0216]

[0217] In particular, the sulfonated polyarylene sulfone polymer (sP) contained in the membrane (M) consists only of non-sulfonated repeating units of formula (1a) and sulfonated repeating units of formula (2a).

[0218] The sulfonated polyarylene sulfone polymer (sP) contained in the membrane (M) according to the invention preferably has a viscosity number of 20 ml / g to 250 ml / g, preferably 50 ml / g to 200 ml / g. The viscosity number is quantified in accordance with DIN EN ISO 1628-1 at 25° C. in a 1% solution in N-methylpyrrolidone (NMP). The measurement can also be carried out at a lower polymer concentration (e.g. 0.5%).

[0219] The weight average molecular weight (M) of the sulfonated polyarylene sulfone polymer (sP) contained in the membrane (M) is W ) is generally in the range of 10000 g / mol to 250000 g / mol, preferably in the range of 15000 g / mol to 200000 g / mol, and more preferably in the range of 18000 g / mol to 150000 g / mol. The weight average molecular weight (M W ) is measured using gel permeation chromatography (GPC). Dimethylacetamide (DMAc) is used as a solvent, and narrow distribution polymethyl methacrylate is used as a standard in the measurement.

[0220] In a preferred embodiment, the separator (M) obtained by the process of the present invention has a good balance of low swelling and high conductivity.

[0221] Equipment including diaphragm (M)

[0222] Another object of the present invention is a device comprising the membrane (M) obtained by the process of the present invention. The device is preferably a fuel cell or an electrolysis cell.

[0223] Another object of the present invention is a fuel cell comprising the membrane (M) obtained by the process of the present invention. Furthermore, another object of the present invention is an electrolysis cell comprising the membrane (M) obtained by the process of the present invention. Furthermore, another object of the present invention is the use of the membrane (M) obtained by the process of the present invention in an electrolysis cell or a fuel cell.

[0224] In order to use the diaphragm (M) obtained by the method of the present invention, in a preferred embodiment, the diaphragm (M) is activated. The activation can be carried out by contacting the diaphragm (M) with an acidic aqueous solution such as an aqueous mineral acid. Preferably, an aqueous sulfuric acid (H2SO4) solution is used for activation. The concentration of the acidic aqueous solution is preferably in the range of 0.1M to 4.0M. After the diaphragm (M) is contacted with an acidic aqueous solution such as an aqueous sulfuric acid solution, the diaphragm can be contacted with water, preferably deionized water. After activation, the diaphragm (M) is usually in the form of H2SO4. + Obtained in form.

[0225] In other words, after activation, the sulfonated polyarylene sulfone polymer (sP) contained in the membrane (M) contains -SO3X 3 The total molar amount of the groups is at least 70 mol.-%, more preferably at least 80 mol.-%, and particularly preferably at least 90 mol.-% -SO3H groups.

[0226] The invention is more particularly illustrated by the following examples without being restricted thereto.

[0227] Components used:

[0228] DCDPS 4,4'-dichlorodiphenyl sulfone,

[0229] sDCDPS 4,4'-dichlorodiphenylsulfone-3,3'-disulfonic acid disodium salt

[0230] BP 4,4'-dihydroxybiphenyl,

[0231] K2CO3: Potassium carbonate, anhydrous, average particle size 32.6 μm

[0232] NMP: N-Methylpyrrolidone, anhydrous

[0233] The viscosity number VN of the sulfonated polyarylene sulfone polymers (sP) is measured in accordance with DIN ISO 1628-1 in a 0.5% by weight solution in NMP.

[0234] The doping ratio (doping rate) of sDCDPS is determined by 1 In addition, the polymer content of the polymer solution after filtration was also determined by CDCl3 1 H-NMR was used for quantification.

[0235] Unless otherwise specified, the separation of the sulfonated polyarylene sulfone polymer (sP) was carried out by dropping a solution of the sulfonated polyarylene sulfone polymer (sP) in NMP into isopropanol at room temperature. The drop height was 0.5 m. The throughput was about 2.5 1 / h. The beads obtained were then extracted with water at 85°C (water throughput 160 1 / h) for twenty hours. The beads were then heated below the glass transition temperature T g The beads are washed at least once with isopropanol and then dried at a temperature below Tg, preferably in vacuum to a residual isopropanol content of less than 1 wt%. In some cases, the powder is obtained by precipitation, then filtered off and washed at least once with isopropanol. The powder can then be extracted with water or isopropanol and finally dried at a temperature below the Tg of the product, preferably in vacuum to a residual water content or isopropanol content of less than 1 wt%.

[0236] Filtration of the product mixture was performed in a heated metal pressure filter using a filter with a pore size of 5 μm and a N2 pressure of 3 bar. The filter was heated to 60°C to reduce the viscosity of the reaction mixture.

[0237] The yield of polymer after precipitation was determined gravimetrically.

[0238] Synthesis Example 1 :

[0239] In a 4-liter glass reactor equipped with a thermometer, a gas inlet tube and a Dean-Stark separator, 288.599 g (1.005 mol) of DCDPS, 257.906 g (0.525 mol) of sDCDPS, 279.315 g (1.50 mol) of BP and 308.209 g (2.23 mol) of potassium carbonate having a volume average particle size of 32.6 μm were suspended in 938 ml of NMP in a nitrogen atmosphere.

[0240] The mixture was heated to 190° C. within one hour. In the following, the reaction time is understood to be the time during which the reaction mixture was kept at 190° C. The water formed in the reaction was removed continuously by distillation, making up for the losses in NMP.

[0241] After a reaction time of 9 hours, the reaction was stopped by adding 1750 ml of NMP and cooling to room temperature (within one hour). The potassium chloride formed in the reaction was removed by filtration. The polymer solution obtained was then divided into two equal parts. One portion was precipitated in isopropanol, the resulting polymer beads were separated and then extracted with hot water (85° C.) for 20 h. The beads were then dried at 120° C. for 24 h under reduced pressure (<100 mbar). Another portion of the solution was used for diaphragm preparation. The polymer content of the solution was 18.1 wt.%.

[0242] Synthesis Example 2:

[0243] In a 4-liter glass reactor equipped with a thermometer, a gas inlet tube and a Dean-Stark separator, 267.059 g (0.93 mol) of DCDPS, 294.750 g (0.60 mol) of sDCDPS, 279.315 g (1.50 mol) of BP and 317.883 g (2.30 mol) of potassium carbonate having a volume average particle size of 32.6 μm were suspended in 938 ml of NMP in a nitrogen atmosphere.

[0244] The mixture was heated to 190° C. within one hour. In the following, the reaction time is understood to be the time during which the reaction mixture was kept at 190° C. The water formed in the reaction was removed continuously by distillation, making up for the losses in NMP.

[0245] After a reaction time of 9 hours, the reaction was stopped by adding 2312 ml of NMP and cooling to room temperature (within one hour). The potassium chloride formed in the reaction was removed by filtration. The polymer solution obtained was divided into equal weight portions. A portion was then precipitated in isopropanol, the resulting polymer beads were separated and then extracted with hot water (85° C.) for 20 h. The beads were then dried at 120° C. for 24 h under reduced pressure (<100 mbar). Another portion of the solution was used for diaphragm preparation. The polymer content of the solution was 18.1 wt.%.

[0246] Table 1 :

[0247] Example 1 2 Condensation time [h] 9 9 VN[ml / g] 70.1 71.9 sDCDPS-control unit [mol %] 32.9 38.1 Yield [wt. %] 88 81

[0248] To prepare the membranes, solutions of the precipitated sulfonated polyarylene sulfone polymers (sP) from Examples 1 and 2 in NMP were prepared using a polymer content of 17.5 wt.%. The solutions made from the precipitated sulfonated polyarylene sulfone polymers (sP) obtained in Examples 1 and 2 are designated 1P and 2P hereinafter.

[0249] The unprecipitated solutions obtained in Examples 1 and 2 were diluted with NMP to obtain a polymer content of 17.5 wt. %, and these solutions are hereinafter designated as 1S and 2S.

[0250] Diaphragm preparation method 1

[0251] Diaphragms were prepared from solutions 1P, 2P, 1S and 2S by casting these solutions onto a glass plate with a doctor blade at a speed of 5 mm / s at a temperature of 60°C. The glass plate was transferred to a vacuum furnace, and the temperature was gradually increased to 100°C and kept there for 12 hours. After cooling to room temperature, the plate was placed in a water bath, which caused the diaphragm to detach from the glass plate. The wet diaphragm was then fixed and vacuum dried at 120°C for 12 hours. The diaphragm obtained from solution 1P is hereinafter referred to as 1PM1. The diaphragm obtained from solution 2P is hereinafter referred to as 2PM1. The diaphragm obtained from solution 1S is hereinafter referred to as 1SM1. The diaphragm obtained from solution 2S is hereinafter referred to as 2SM1.

[0252] Diaphragm preparation method 2

[0253] Separators were also prepared from solutions 1P, 2P, 1S and 2S, wherein casting was also carried out according to the following procedure: To produce a monolayer film, an automatic film applicator and a universal applicator from Zehntner were used. The coating solutions 1P, 2P, 1S and 2S were applied to a PET substrate ( Mitsubishi polyester film). The gap width of the doctor blade was chosen so that the layer had a thickness of 60 μm after drying at 70° C. The film was subsequently detached from the PET support for further processing. The diaphragm obtained from solution 1P is referred to as 1PM2 in the following. The diaphragm obtained from solution 2P is referred to as 2PM2 in the following. The diaphragm obtained from solution 1S is referred to as 1SM2 in the following. The diaphragm obtained from solution 2S is referred to as 2SM2 in the following.

[0254] The membranes prepared as described were cut to the required size (5×5 cm). For activation, the membranes were immersed in 0.5 M H2SO4 at 80°C for 2 h. Subsequently, the membranes were immersed in deionized water (MiliQ 18.2 MOhm) at 80°C for another 2 h and finally stored in a new batch of deionized water at room temperature. The swelling of the membrane in the xy direction was determined by measuring the corresponding lengths before and after activation. The swelling in the z direction was determined by measuring the thickness of the membrane before and after activation using a micrometer. To determine the conductivity, the membranes were sandwiched between a diaphragm equipped with two rectangular gold electrodes (0.25 cm 2 ) in a special Teflon cell. Constant pressure is achieved by adjusting the torque of the 4 screws to 4Nm.

[0255] Table 2 :

[0256]

[0257] The membranes obtained from direct use of sulfonated poly(arylene sulfone) polymer (sP) solutions showed less swelling and at the same time improved conductivity.

[0258] Preparation of Catalyst Coated Membrane (CCM)

[0259] To prepare the catalyst-coated membrane CCM, the activated membrane 1SM1 (in H + The PE sheets (SP Bel-Art Fritware porous polyethylene sheets medium porosity, 0.125 inch thick) were dried at room temperature and sandwiched between two porous PE sheets to prevent curling.

[0260] The catalyst coating of the membrane 1SM1 was carried out by spraying the catalyst ink (91.6 wt% H2O, 3.4 wt% Nafion, 0.8 wt% catalyst, 4,2 wt% dispersant) onto both sides of the membrane 1SM1, which was placed on a hot plate at 60°C. After coating on both sides (the anode side was coated with 2 mg Ir black cm -2 , and 1 mg Pt black cm-2 on the cathode side), the catalyst coated separator 1SM1 was calendered at 130° C. The final CCM 1SM1 was then assembled into a single cell PEM test rig and subjected to polarization curves at 80° C.

[0261] Another catalyst-coated membrane was prepared using the activated membrane 1PM1, wherein the preparation was carried out as described above.

[0262] As a comparative example, prior art Nafion 117 coated with the same amount of catalyst was measured.

[0263] In the case of CCM 1SM1, comparable performance to Nafion 117 was achieved ( Figure 1 ), while CMC 1PM1 shows a much higher resistance.

Claims

1. A method for preparing a membrane (M) containing a sulfonated polyarylene sulfone polymer (sP), the method comprising the following steps i) Conversion reaction mixture (R G ), the reaction mixture comprising An aromatic dihalogenated sulfone component (component (A)), the aromatic dihalogenated sulfone component comprising at least one sulfonated aromatic dihalosulfone (component (A1)) and at least one non-sulfonated aromatic dihalosulfone (component (A2)), at least one aromatic dihydroxy compound (component (B)), at least one carbonate compound (component (C)), and at least one aprotic polar solvent (component (D)), To obtain a product mixture (P) comprising the sulfonated polyarylene sulfone polymer (sP), the at least one aprotic polar solvent and the at least one inorganic halide compound G ), ii) from the product mixture (P G ) to obtain a solution (S) comprising the sulfonated polyarylene sulfone polymer (sP) and the at least one aprotic polar solvent iii) separating said at least one aprotic polar solvent from said solution (S) to obtain said membrane (M) containing said sulfonated polyarylene sulfone polymer (sP).

2. The method according to claim 1, wherein component (A1) comprises at least one compound selected from the group consisting of 4,4′-dichlorodiphenyl sulfone-3,3′-disulfonic acid, 4,4′-dichlorodiphenyl sulfone-3,3′-disulfonic acid disodium salt, 4,4′-dichlorodiphenyl sulfone-3,3′-disulfonic acid dipotassium salt, 4,4′-difluorodiphenyl sulfone-3,3′-disulfonic acid, 4,4′-difluorodiphenyl sulfone-3,3′-disulfonic acid disodium salt and 4,4′-difluorodiphenyl sulfone-3,3′-disulfonic acid dipotassium salt.

3. The method according to claim 1 or 2, wherein based on the reaction mixture (R G ) in the total weight of component (A2), component (A2) comprising not less than 80 wt% of at least one aromatic dihalosulfone selected from the group consisting of 4,4'-dichlorodiphenyl sulfone and 4,4'-difluorodiphenyl sulfone.

4. The method according to any one of claims 1 to 3, wherein based on the reaction mixture (R G ) in the total weight of component (B), component (B) contains not less than 80 wt% of 4,4'-dihydroxybiphenyl.

5. The method according to any one of claims 1 to 4, wherein based on the reaction mixture (R G ) in the total weight of component (C), component (C) containing not less than 50wt% of potassium carbonate.

6. The method according to any one of claims 1 to 5, wherein based on the reaction mixture (R G ) in the total weight of component (D), component (D) containing not less than 50wt% of at least one solvent selected from the group consisting of N-methylpyrrolidone, N-dimethylacetamide, dimethyl sulfoxide and dimethyl-formamide.

7. The method according to any one of claims 1 to 6, wherein based on the reaction mixture (R G ) in an amount of 20 to 70 mol.-% of component (A1) and 30 to 80 mol.-% of component (A2).

8. The method according to any one of claims 1 to 7, wherein step iii) comprises the following steps iii-1) casting the solution (S) provided in step ii) to obtain a film of the solution (S), iii-2) evaporating said at least one aprotic polar solvent from said film of said solution (S) obtained in step iii-1) to obtain said membrane (M) in the form of a film.

9. The process according to any one of claims 1 to 8, wherein the separation of the at least one aprotic polar solvent from the solution (S) in step iii) is carried out by a phase inversion process.

10. A membrane (M) obtainable by the method according to any one of claims 1 to 9.

11. The membrane (M) according to claim 10, comprising at least one catalyst coating.

12. A catalyst-coated membrane, comprising a membrane (M) according to claim 10 or 11, wherein the catalyst layers for the anode and cathode are coated on both sides of the membrane (M) with a catalyst dispersion containing a binder, wherein the binder is selected from the group consisting of Nafion and Nafion-type polymers (PFSA), sulfonated polyarylene sulfone polymers (sP) and sulfonated styrene copolymers.

13. The catalyst-coated membrane according to claim 12, wherein the binder in the catalyst dispersion and the membrane (M) comprise the same sulfonated polyarylene sulfone polymer (sP) 14. A fuel cell comprising the membrane (M) according to claim 10 or 11.

15. An electrolysis cell or an electrodialysis cell comprising a membrane (M) according to claim 10 or 11.

16. Use of the membrane (M) according to claim 10 or 11 in an electrolysis cell, an electrodialysis cell or a fuel cell.

17. Method for producing electrical energy and / or hydrogen using a membrane (M) according to claim 10 or 11.